A low-cost, high-purity, high-densification spherical magnesium oxide powder and a preparation method thereof
By using a combination of magnesium oxide ceramic powder, soluble magnesium ion salt, magnesium ion surfactant and reaction aid in the preparation of spherical magnesium oxide powder, a highly densified spherical magnesium oxide powder is formed, which solves the quality problem in the existing process. solve the problems of instability and high cost, and achieve efficient and low-cost production.
Patent Information
- Application Number
- CN202411034690.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The existing preparation process of spherical magnesium oxide powder has problems such as unstable strength, densification degree, crystallinity, and purity, high porosity, large specific surface area, high production cost, high energy consumption, and high raw material requirements.
Magnesium oxide ceramic powder, soluble magnesium ion salt, magnesium ion surfactant, reaction aid and water are used to form spherical agglomerates through ionic solution, and then calcined after ion precipitation reaction and drying to produce low-cost, high-purity and high-densification products Spherical magnesium oxide powder.
The preparation of magnesium oxide powder with high purity, high densification and high sphericity is achieved, reducing production costs and energy consumption, overcoming the problems of unstable quality and high cost of the existing process, and is suitable for industrial-scale production.
Smart Images

Figure CN118561303B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of spherical magnesium oxide powder, and in particular to low-cost, high-purity and high-densification spherical magnesium oxide powder and a preparation method thereof. Background Art
[0002] In the prior art, the spray granulation process of spherical magnesium oxide powder is to premix the raw material slurry and then spray granulate it through a spray granulator to obtain spherical powder. However, due to the particle docking agglomeration state, that is, the uncontrolled spontaneous agglomeration phenomenon occurs between the powder particles due to various interactions (such as electrostatic force, van der Waals force, capillary force, etc.); the strength, densification degree, crystallinity, purity, etc. of the spherical magnesium oxide powder obtained are difficult to be effectively guaranteed, and the product quality is unstable. At the same time, if Figure 1 As shown, the spherical magnesium oxide powder particles produced by the existing spray granulation process are not tightly packed and there is a problem of difference in particle packing density, which leads to defects of high porosity and large specific surface area, affecting the subsequent use performance of the spherical magnesium oxide powder.
[0003] At the same time, the existing spherical magnesium oxide powder can also be prepared by melt spraying, which is to melt and mix raw materials such as magnesium oxide powder, spray molten droplets, and cool them into balls to obtain spherical magnesium oxide powder. Since the melting temperature of magnesium oxide powder is as high as 3000°C, the energy consumption required by the melt spraying method is extremely high; and the melt spraying process has high requirements for magnesium oxide raw materials, and has strict requirements on raw material particle size, particle size distribution and other aspects. The price of raw materials is high, and the comprehensive production cost remains high. In addition, adding low-melting materials to reduce the melting temperature of magnesium chloride will cause the introduction of undesirable impurities and reduce the quality of the spherical magnesium oxide powder obtained. Furthermore, the spherical magnesium oxide powder prepared by the melt spraying method is inert and has low reaction activity, which is not conducive to subsequent processing and application.
[0004] Thus, a low-cost, high-purity, high-densification spherical magnesium oxide powder and a preparation method thereof are provided, which overcome the problems of unstable strength, degree of densification, crystallinity, purity, high porosity and large specific surface area of the spherical magnesium oxide powder prepared by the existing process; as well as the problems of high production cost, high production energy consumption and high raw material requirements in the existing spherical magnesium oxide powder preparation process, which has important technical significance. Summary of the invention
[0005] In order to solve the technical problems existing in the prior art, the present invention provides a low-cost, high-purity and high-densification spherical magnesium oxide powder and a preparation method thereof, which effectively overcomes the problems of unstable strength, degree of densification, crystallinity and purity of the spherical magnesium oxide powder prepared by the existing process, and high porosity and large specific surface area, and can produce high-purity and high-densification spherical magnesium oxide powder; at the same time, it can overcome the problems of high production cost, high production energy consumption and high raw material requirements in the existing spherical magnesium oxide powder preparation process, and effectively reduce production energy consumption and production cost.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0007] A method for preparing a low-cost, high-purity, and high-densification spherical magnesium oxide powder, which is prepared by using the following raw materials: magnesium oxide ceramic powder, soluble magnesium ion salt, magnesium ion surfactant, reaction aid, and water;
[0008] The soluble magnesium ion salt is at least one of the following: magnesium chloride, magnesium sulfate, and magnesium acetate;
[0009] The magnesium ion surfactant is at least one of the following: octadecyl magnesium chloride, cyclohexyl magnesium chloride, tridecyl magnesium sulfate;
[0010] The reaction aid is at least one of the following: ammonium oxalate, ammonium acetate, ammonium formate, ammonium citrate, and ammonium phosphate;
[0011] The water is not particularly limited and can be tap water or deionized water.
[0012] The method for preparing low-cost, high-purity and high-densification spherical magnesium oxide powder comprises the following steps: a soluble magnesium ion salt is dissolved in water to form an ionic solution, magnesium oxide ceramic powder is dispersed in the ionic solution, and under the action of a magnesium ion surfactant, the magnesium oxide ceramic powder forms spherical agglomerates and forms a spherical micelle powder agglomeration state, and the soluble magnesium ion salt is enriched on the polar bond surface of the magnesium element-containing surfactant, and under the action of a reaction aid, an ion precipitation reaction is performed to form MgO / Mg(OH) x (CO) y (NH2) z ; After drying, spherical MgO / Mg(OH) x (CO) y (NH2) z After the powder is formed, it is calcined to obtain low-cost, high-purity and high-density spherical magnesium oxide powder;
[0013] The spherical MgO / Mg(OH) x (CO) y (NH2) zIn the powder, x is any number from 1 to 3, y is any number from 1 to 2, and z is any number from 1 to 3.
[0014] Furthermore, the magnesium chloride salt is at least one of the following: anhydrous magnesium chloride, magnesium chloride hexahydrate, and ethyl magnesium chloride; the magnesium sulfate salt is at least one of the following: anhydrous magnesium sulfate, magnesium sulfate heptahydrate, magnesium sulfate trihydrate, and magnesium sulfate hexahydrate; the magnesium acetate salt is at least one of the following: magnesium acetate and magnesium oxalate dihydrate.
[0015] The soluble magnesium ion salt promotes the densification and low-temperature sintering of spherical slurry during ion reaction and spheroidization agglomeration; the magnesium ion surfactant can form spherical micelles in water, further promote the enrichment of metal magnesium ions, and form Mg-OH bond bonding, further improving the sphericity and spherical densification of magnesium oxide; the reaction aid is soluble in water, and under the action of ion reaction, ammonium ions react with magnesium ions and anion roots to form Mg-OH-NH bonds, effectively forming a precipitate of magnesium oxide with high bonding strength, filling the pores of the particles, and further improving the sphericity and spherical densification of magnesium oxide.
[0016] Preferably, the mass ratio of the magnesium oxide ceramic powder, the soluble magnesium ion salt, and water is 15-35:10-15:55-75;
[0017] The dosage of magnesium ion surfactant is 0.1-0.5% of the mass of soluble magnesium ion salt;
[0018] The dosage of the reaction aid is 1-5% of the mass of the soluble magnesium ion salt.
[0019] Preferably, the magnesium oxide ceramic powder has a purity of 99wt%, a particle size d50≤10μm, a pH≤10, a Mohs hardness of 6, and a specific surface area of <15.6m 2 / g.
[0020] The method for preparing low-cost, high-purity and high-densification spherical magnesium oxide powder comprises the following steps:
[0021] Step S001, adding magnesium oxide ceramic powder and soluble magnesium ion salt into deionized water, mixing evenly, and preparing a white low-viscosity slurry with a viscosity of ≤500 mPa·s;
[0022] Step S002, adding a magnesium ion surfactant to the white low-viscosity slurry, mixing and stirring at a speed of 300-1000 r / min, and standing at room temperature to obtain a white medium-viscosity solution with a viscosity of 1000-2000 mPa·s;
[0023] Step S003, adding a reaction aid to the white medium-viscosity solution, mixing and stirring at a speed of 80-150 r / min to react, to obtain a milky white low-viscosity solution with a viscosity of ≤700 mPa·s;
[0024] Step S004, spray drying the milky white low-viscosity solution to obtain white spherical powder;
[0025] Step S005: the white spherical powder is calcined at 800-1280° C. to obtain low-cost, high-purity, and high-densification spherical magnesium oxide powder.
[0026] Furthermore, in step S004, the inlet air temperature of the spray drying is controlled to be ≥180°C, the outlet air temperature is 60°C, and the atomizing disk rotation speed is ≥180Hz.
[0027] Furthermore, in step S005, the heating rate to 800-1280°C is 1.5°C-3°C / min;
[0028] The calcination time at 800-1280°C is not less than 3h.
[0029] A low-cost, high-purity, high-densification spherical magnesium oxide powder is prepared by the above-mentioned preparation method; the low-cost, high-purity, high-densification spherical magnesium oxide powder has a particle size d50 of 5-120 μm, a magnesium oxide content of ≥98wt%, a sphericity of ≥96%, and a specific surface area of <0.3cm 2 / g, conductivity ≤40μS / cm, pH ≤9, compressive strength ≥18MPa.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) The method for preparing low-cost, high-purity, and high-density spherical magnesium oxide powder of the present invention comprises the following steps: uniformly dispersing magnesium oxide ceramic powder in the ionic solution, and under the action of a magnesium ion surfactant, the magnesium oxide ceramic powder forms spherical agglomerates and forms a spherical micelle powder agglomeration state, and soluble magnesium ion salts are enriched on the polar bond surface of the magnesium-containing surfactant, and further under the action of a reaction aid, an ion precipitation reaction is performed, and the precipitate fills the pores of the particles and is firmly combined to form MgO / Mg(OH) x (CO) y (NH2) z After drying, spherical MgO / Mg(OH) x (CO) y (NH2) zThe powder is then calcined to obtain low-cost, high-purity and high-density spherical magnesium oxide powder. Relying on the mature granulation-sintering process, the spherical magnesium oxide powder can be prepared at low cost and efficiently, and through modification and pre-reaction technology, the strength, densification degree, crystallinity and purity of the spherical magnesium oxide powder prepared by the existing process are effectively overcome. The problems of high porosity, large specific surface area and poor density can be overcome, and high-purity, high-density and high-sphericity magnesium oxide powder can be obtained; at the same time, it can overcome the problems of high production cost, high production energy consumption and high raw material requirements in the existing spherical magnesium oxide powder preparation process, and effectively reduce production energy consumption and production cost.
[0032] (2) The method for preparing low-cost, high-purity and high-density spherical magnesium oxide powder of the present invention adopts a granulation-sintering process, and through the composite reaction technology of powder and ion solution, the ion reaction precipitate is filled into the pores of the powder granulation particles, and finally a high-purity and high-density spherical magnesium oxide powder is obtained; compared with the melt spraying method, it can greatly reduce the production cost and production energy consumption of spherical magnesium oxide powder, and effectively avoid the disadvantages of ordinary granulation balls with large specific surface area and many pores. The product technical indicators reach the international advanced level.
[0033] (3) The method for preparing the low-cost, high-purity, and high-densification spherical magnesium oxide powder of the present invention has a simple process flow and has better engineering capabilities than the existing chemical synthesis method, melt spraying method, etc., and is suitable for industrial-scale production. At the same time, compared with the existing production methods, the production cost of the low-cost, high-purity, and high-densification spherical magnesium oxide powder of the present invention can be controlled below RMB 10,000 / t.
[0034] (4) The low-cost, high-purity, high-density spherical magnesium oxide powder of the present invention has a particle size d50 of 5-120 μm, a magnesium oxide content ≥ 98 wt%, a sphericity ≥ 96%, and a specific surface area < 0.3 m 2 / g, conductivity ≤40μS / cm, pH ≤9, compressive strength (10% breakage rate) ≥18MPa. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a spherical magnesium oxide powder made by the existing spray granulation process.
[0036] Figure 2 This is a 1500x electron microscope photograph of the spherical magnesium oxide powder obtained in Example 1.
[0037] Figure 3 This is a 95x electron microscope photograph of the spherical magnesium oxide powder prepared in Example 1. DETAILED DESCRIPTION
[0038] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.
[0039] Example 1
[0040] like Figure 2-3 As shown, this embodiment provides a low-cost, high-purity, and high-densification spherical magnesium oxide powder, the particles of which have a highly densified near-perfect spherical structure. The specific specifications of the low-cost, high-purity, and high-densification spherical magnesium oxide powder are shown in Table 1:
[0041] Table 1 Specifications of low-cost, high-purity, high-densification spherical magnesium oxide powder of Example 1
[0042]
[0043] The low-cost, high-purity and high-densification spherical magnesium oxide powder is prepared from the following raw materials: magnesium oxide ceramic powder, soluble magnesium ion salt, magnesium ion surfactant, reaction aid and water.
[0044] The magnesium oxide ceramic powder has a purity of 99 wt%, a particle size d50 of 8 μm, a pH of 10, a Mohs hardness of 6, and a specific surface area of 15 m 2 / g.
[0045] The soluble magnesium ion salt is anhydrous magnesium chloride, magnesium sulfate heptahydrate, and magnesium acetate.
[0046] The magnesium ion surfactant is octadecyl magnesium chloride and cyclohexyl magnesium chloride.
[0047] The reaction aid is ammonium oxalate.
[0048] The specific weight portions of the above-mentioned raw materials are as follows:
[0049] 25 parts of magnesium oxide ceramic powder;
[0050] 5 parts of anhydrous magnesium chloride;
[0051] 8 parts of magnesium sulfate heptahydrate;
[0052] 2 parts of magnesium acetate;
[0053] 60 parts of water;
[0054] Magnesium ion surfactant: 0.015 parts of octadecyl magnesium chloride; 0.01 parts of cyclohexyl magnesium chloride;
[0055] Reaction aid: 0.75 parts of ammonium oxalate.
[0056] The present embodiment also provides a method for preparing the aforementioned low-cost, high-purity, and high-densification spherical magnesium oxide powder. A soluble magnesium ion salt is dissolved in water to form an ionic solution. The magnesium oxide ceramic powder is uniformly dispersed in the ionic solution. Under the action of a magnesium ion surfactant, the magnesium oxide ceramic powder forms spherical agglomerates and forms a spherical micelle powder agglomeration state. The soluble magnesium ion salt is enriched on the surface of the polar bond of the magnesium-containing surfactant, and under the action of a reaction aid, an ion precipitation reaction is performed to form MgO / Mg(OH) x (CO) y (NH2) z After drying, spherical MgO / Mg(OH) x (CO) y (NH2) z The powder is then calcined to obtain low-cost, high-purity and high-density spherical magnesium oxide powder.
[0057] The spherical MgO / Mg(OH) x (CO) y (NH2) z In powder, x=1, y=1, z=2.
[0058] The method for preparing the low-cost, high-purity and high-densification spherical magnesium oxide powder is specifically as follows:
[0059] Step S001, premix anhydrous magnesium chloride into water to dissolve, add magnesium oxide ceramic powder after the heat of dissolution is completely released, stir at a high speed of 1000 r / min for 0.5 h at 40°C, and let stand for 3 h to obtain a white colloidal slurry; continue to add magnesium sulfate heptahydrate and magnesium acetate to the white colloidal slurry, mix and stir for 0.5 h, and obtain a white low-viscosity slurry with a viscosity of 500 mPa·s.
[0060] Step S002, adding octadecyl magnesium chloride and cyclohexyl magnesium chloride to the white low-viscosity slurry obtained in step S001, stirring at 800 r / min for 0.5 h to obtain a milky white uniform solution; standing for 1 h to obtain a white medium-viscosity solution with a viscosity of 1200 mPa·s.
[0061] Step S003, adding ammonium oxalate to the white medium-viscosity solution obtained in step S002, mixing and stirring at 120 r / min for 0.5 h, to obtain a milky white low-viscosity solution with a viscosity of 700 mPa·s.
[0062] Step S004, spray drying the milky white low-viscosity solution obtained in step S003, controlling the air inlet temperature to 180° C., the air outlet temperature to 60° C., and the atomizing disk speed to 300 Hz, to obtain white spherical powder.
[0063] Step S005, calcining the white spherical powder obtained in step S004, controlling the heating rate to 2°C / min, heating to a sintering temperature of 1280°C, and calcining for 3 hours to obtain low-cost, high-purity, and high-densification spherical magnesium oxide powder.
[0064] Example 2
[0065] This embodiment provides a low-cost, high-purity, high-densification spherical magnesium oxide powder, the particles of which have a highly densified near-perfect spherical structure. The specific specifications of the low-cost, high-purity, high-densification spherical magnesium oxide powder are shown in Table 2:
[0066] Table 2 Specifications of low-cost, high-purity, high-density spherical magnesium oxide powder of Example 2
[0067]
[0068] The low-cost, high-purity and high-densification spherical magnesium oxide powder is prepared from the following raw materials: magnesium oxide ceramic powder, soluble magnesium ion salt, magnesium ion surfactant, reaction aid and water.
[0069] The magnesium oxide ceramic powder has a purity of 99 wt%, a particle size d50 of 8 μm, a pH of 10, a Mohs hardness of 6, and a specific surface area of 15 m 2 / g.
[0070] The soluble magnesium ion salt is magnesium chloride hexahydrate, anhydrous magnesium sulfate, magnesium sulfate heptahydrate, and magnesium oxalate dihydrate.
[0071] The magnesium ion surfactant is magnesium tridecyl sulfate.
[0072] The reaction aid is ammonium citrate.
[0073] The specific weight portions of the above-mentioned raw materials are as follows:
[0074] 35 parts of magnesium oxide ceramic powder;
[0075] 3 parts of magnesium chloride hexahydrate;
[0076] 1 part of anhydrous magnesium sulfate;
[0077] 5 parts of magnesium sulfate heptahydrate;
[0078] 1 part of magnesium oxalate dihydrate;
[0079] 55 parts water;
[0080] Magnesium ion surfactant: 0.01 parts of tridecyl magnesium sulfate;
[0081] Reaction aid: 0.1 part of ammonium citrate.
[0082] The present embodiment also provides a method for preparing the aforementioned low-cost, high-purity, and high-densification spherical magnesium oxide powder. A soluble magnesium ion salt is dissolved in water to form an ionic solution. The magnesium oxide ceramic powder is uniformly dispersed in the ionic solution. Under the action of a magnesium ion surfactant, the magnesium oxide ceramic powder forms spherical agglomerates and forms a spherical micelle powder agglomeration state. The soluble magnesium ion salt is enriched on the surface of the polar bond of the magnesium-containing surfactant, and under the action of a reaction aid, an ion precipitation reaction is performed to form MgO / Mg(OH) x (CO) y (NH2) z After drying, spherical MgO / Mg(OH) x (CO) y (NH2) z The powder is then calcined to obtain low-cost, high-purity and high-density spherical magnesium oxide powder.
[0083] The spherical MgO / Mg(OH) x (CO) y (NH2) z In powder, x=1.5, y=2, z=2.
[0084] The method for preparing the low-cost, high-purity and high-densification spherical magnesium oxide powder is specifically as follows:
[0085] Step S001, premix anhydrous magnesium sulfate and magnesium oxalate dihydrate into water and dissolve them. After the heat of dissolution is completely released, magnesium oxide ceramic powder is added, and at a temperature of 40°C, high-speed stirring is performed at 1000 r / min for 0.5 h, and then the mixture is allowed to stand for 3 h to obtain a white dispersed slurry; magnesium chloride hexahydrate and magnesium sulfate heptahydrate are continuously added to the white dispersed slurry, and the mixture is mixed and stirred for 0.5 h to obtain a white low-viscosity slurry with a viscosity of 400 mPa·s.
[0086] Step S002, adding tridecyl magnesium sulfate to the white low-viscosity slurry obtained in step S001, stirring at a low speed of 300 r / min for 0.5 h to obtain a milky white uniform solution; standing for 1 h to obtain a white medium-viscosity solution with a viscosity of 1360 mPa·s.
[0087] Step S003, adding ammonium oxalate to the white medium-viscosity solution obtained in step S002, mixing and stirring at 150 r / min for 0.5 h, to obtain a milky white low-viscosity solution with a viscosity of 650 mPa·s.
[0088] Step S004, spray drying the milky white low-viscosity solution obtained in step S003, controlling the air inlet temperature to 190° C., the air outlet temperature to 60° C., and the atomizing disk speed to 200 Hz, to obtain white spherical powder.
[0089] Step S005, calcining the white spherical powder obtained in step S004, controlling the heating rate to 1.5°C / min, heating to a sintering temperature of 1200°C, and calcining for 3.5 hours to obtain low-cost, high-purity, and high-densification spherical magnesium oxide powder.
[0090] Example 3
[0091] This embodiment provides a low-cost, high-purity, high-densification spherical magnesium oxide powder, the particles of which have a highly densified near-perfect spherical structure. The specific specifications of the low-cost, high-purity, high-densification spherical magnesium oxide powder are shown in Table 3:
[0092] Table 3 Specifications of low-cost, high-purity, high-density spherical magnesium oxide powder of Example 3
[0093]
[0094] The low-cost, high-purity and high-densification spherical magnesium oxide powder is prepared from the following raw materials: magnesium oxide ceramic powder, soluble magnesium ion salt, magnesium ion surfactant, reaction aid and water.
[0095] The magnesium oxide ceramic powder has a purity of 99 wt%, a particle size d50 of 8 μm, a pH of 10, a Mohs hardness of 6, and a specific surface area of 15 m 2 / g.
[0096] The soluble magnesium ion salt is anhydrous magnesium chloride, magnesium chloride hexahydrate, magnesium sulfate heptahydrate, magnesium acetate, and magnesium oxalate dihydrate.
[0097] The magnesium ion surfactant is octadecyl magnesium chloride.
[0098] The reaction aid is ammonium oxalate.
[0099] The specific weight portions of the above-mentioned raw materials are as follows:
[0100] 30 parts of magnesium oxide ceramic powder;
[0101] 1 part of anhydrous magnesium chloride;
[0102] 2 parts of magnesium chloride hexahydrate;
[0103] 6 parts of magnesium sulfate heptahydrate;
[0104] 2 parts of magnesium acetate;
[0105] 1 part of magnesium oxalate dihydrate;
[0106] Water 58 parts;
[0107] Magnesium ion surfactant: 0.05 parts of octadecyl magnesium chloride;
[0108] Reaction aid: 0.24 parts of ammonium oxalate.
[0109] The present embodiment also provides a method for preparing the aforementioned low-cost, high-purity, and high-densification spherical magnesium oxide powder. A soluble magnesium ion salt is dissolved in water to form an ionic solution. The magnesium oxide ceramic powder is uniformly dispersed in the ionic solution. Under the action of a magnesium ion surfactant, the magnesium oxide ceramic powder forms spherical agglomerates and forms a spherical micelle powder agglomeration state. The soluble magnesium ion salt is enriched on the surface of the polar bond of the magnesium-containing surfactant, and under the action of a reaction aid, an ion precipitation reaction is performed to form MgO / Mg(OH) x (CO) y (NH2) z After drying, spherical MgO / Mg(OH) x (CO) y (NH2) z The powder is then calcined to obtain low-cost, high-purity and high-density spherical magnesium oxide powder.
[0110] The spherical MgO / Mg(OH) x (CO) y (NH2) z In powder, x=2, y=3, z=2.
[0111] The method for preparing the low-cost, high-purity and high-densification spherical magnesium oxide powder is specifically as follows:
[0112] Magnesium chloride hexahydrate, magnesium sulfate heptahydrate, magnesium acetate, magnesium oxalate dihydrate
[0113] Step S001, premix anhydrous magnesium chloride into water to dissolve, and after the heat of dissolution is completely released, add magnesium oxide ceramic powder, stir at a high speed of 1000r / min for 0.5h at a temperature of 40°C, and let it stand for 3h to obtain a white colloidal slurry; continue to add magnesium chloride hexahydrate, magnesium sulfate heptahydrate, magnesium acetate, and magnesium oxalate dihydrate to the white colloidal slurry, mix and stir for 0.5h, and obtain a white low-viscosity slurry with a viscosity of 500mPa·s.
[0114] Step S002, adding octadecyl magnesium chloride to the white low-viscosity slurry obtained in step S001, stirring at a low speed of 800 r / min for 0.5 h to obtain a milky white uniform solution; standing for 1 h to obtain a white medium-viscosity solution with a viscosity of 1400 mPa·s.
[0115] Step S003, adding ammonium oxalate to the white medium-viscosity solution obtained in step S002, mixing and stirring at 110 r / min for 0.5 h, to obtain a milky white low-viscosity solution with a viscosity of 700 mPa·s.
[0116] Step S004, spray drying the milky white low-viscosity solution obtained in step S003, controlling the air inlet temperature to 190° C., the air outlet temperature to 60° C., and the atomizing disk speed to 180 Hz, to obtain white spherical powder.
[0117] Step S005, calcining the white spherical powder obtained in step S004, controlling the heating rate to 2.2°C / min, heating to a sintering temperature of 1250°C, and calcining for 3.2 hours to obtain low-cost, high-purity, and high-density spherical magnesium oxide powder.
[0118] Comparative Example 1
[0119] Comparative Example 1 adopts the technical scheme of Example 1, except that octadecyl trimethyl ammonium chloride is used instead of the magnesium ion surfactant; the weight portion of octadecyl trimethyl ammonium chloride replacing magnesium is 0.025 parts, and the weight portions of other raw materials remain unchanged.
[0120] Specifically, the preparation method of the spherical magnesium oxide powder of Comparative Example 1 is to dry to obtain spherical 5Mg(OH)2•MgSO4•7H2O powder, and then calcine to obtain spherical magnesium oxide powder.
[0121] The preparation method of the spherical magnesium oxide powder of Comparative Example 1 is specifically as follows:
[0122] Step S001, premix anhydrous magnesium chloride into water to dissolve, add magnesium oxide ceramic powder after the heat of dissolution is completely released, stir at a high speed of 1000 r / min for 0.5 h at 40°C, and let stand for 3 h to obtain a white colloidal slurry; continue to add magnesium sulfate heptahydrate and magnesium acetate to the white colloidal slurry, mix and stir for 0.5 h, and obtain a white low-viscosity slurry with a viscosity of 500 mPa·s.
[0123] Step S002, adding octadecyltrimethylammonium chloride to the white low-viscosity slurry obtained in step S001, stirring at 800 r / min for 0.5 h to obtain a milky white uniform solution; standing for 1 h to obtain a white medium-viscosity solution with a viscosity of 1400 mPa·s.
[0124] Step S003, adding ammonium oxalate to the white medium-viscosity solution obtained in step S002, mixing and stirring at 120 r / min for 0.05 h, to obtain a milky white high-viscosity solution with a viscosity of 5000 mPa·s.
[0125] Step S004, spray drying the milky white low-viscosity solution obtained in step S003, controlling the air inlet temperature to 180° C., the air outlet temperature to 60° C., and the atomizing disk speed to 300 Hz, to obtain white spherical powder.
[0126] Step S005, calcining the white spherical powder obtained in step S004, controlling the heating rate to 2°C / min, heating to a sintering temperature of 1280°C, and calcining for 3 hours to obtain low-cost, high-purity, and high-densification spherical magnesium oxide powder.
[0127] The specific specifications of the spherical magnesium oxide powder of Comparative Example 1 are shown in Table 4:
[0128] Table 4 Specifications of spherical magnesium oxide powder of Comparative Example 1
[0129]
[0130] It can be seen that the preparation method of the low-cost, high-purity and high-densification spherical magnesium oxide powder of the present invention is as follows: the magnesium oxide ceramic powder is uniformly dispersed in the ionic solution, and under the action of the magnesium ion surfactant, the magnesium oxide ceramic powder forms spherical agglomerates and forms a spherical micelle powder agglomeration state, and the soluble magnesium ion salt is enriched on the polar bond surface of the magnesium element-containing surfactant, and further under the action of the reaction aid, the precipitate is subjected to an ion precipitation reaction, and the precipitate fills the particle pores and is firmly combined to form MgO / Mg(OH) x (CO) y (NH2) z After drying, spherical MgO / Mg(OH) x (CO) y (NH2) z The powder is then calcined to obtain low-cost, high-purity and high-density spherical magnesium oxide powder. Relying on the mature granulation-sintering process, the spherical magnesium oxide powder can be prepared at low cost and efficiently, and through modification and pre-reaction technology, the strength, densification degree, crystallinity and purity of the spherical magnesium oxide powder prepared by the existing process are effectively overcome. The problems of unstable porosity and large specific surface area, high-purity, high-density and high-sphericity magnesium oxide powder can be obtained; at the same time, it can overcome the problems of high production cost, high production energy consumption and high raw material requirements in the existing spherical magnesium oxide powder preparation process, and effectively reduce production energy consumption and production cost.
[0131] Unless otherwise specified, all percentages used in the present invention are by mass.
[0132] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing low-cost, high-purity, and high-densification spherical magnesium oxide powder, characterized in that: The following raw materials are used for preparation: magnesium oxide ceramic powder, soluble magnesium ion salt, magnesium ion surfactant, reaction aid and water; The soluble magnesium ion salt is at least one of the following: magnesium chloride, magnesium sulfate, and magnesium acetate; The magnesium ion surfactant is at least one of the following: octadecyl magnesium chloride, cyclohexyl magnesium chloride, tridecyl magnesium sulfate; The reaction aid is at least one of the following: ammonium oxalate, ammonium acetate, ammonium formate, ammonium citrate, and ammonium phosphate; The method for preparing low-cost, high-purity and high-densification spherical magnesium oxide powder comprises the following steps: a soluble magnesium ion salt is dissolved in water to form an ionic solution, magnesium oxide ceramic powder is dispersed in the ionic solution, and under the action of a magnesium ion surfactant, the magnesium oxide ceramic powder forms spherical agglomerates and forms a spherical micelle powder agglomeration state, and the soluble magnesium ion salt is enriched on the polar bond surface of the magnesium element-containing surfactant, and under the action of a reaction aid, an ion precipitation reaction is performed to form MgO / Mg(OH) x (CO) y (NH2) z ; After drying, spherical MgO / Mg(OH) x (CO) y (NH2) z After the powder is formed, it is calcined to obtain low-cost, high-purity and high-density spherical magnesium oxide powder; The spherical MgO / Mg(OH) x (CO) y (NH2) z In the powder, x is any number from 1 to 3, y is any number from 1 to 2, and z is any number from 1 to 3; The method for preparing low-cost, high-purity and high-densification spherical magnesium oxide powder comprises the following steps: Step S001, adding magnesium oxide ceramic powder and soluble magnesium ion salt into deionized water, mixing evenly, and preparing a white low-viscosity slurry with a viscosity of ≤500 mPa·s; Step S002, adding a magnesium ion surfactant to the white low-viscosity slurry, mixing and stirring at a speed of 300-1000 r / min, and standing at room temperature to obtain a white medium-viscosity solution with a viscosity of 1000-2000 mPa·s; Step S003, adding a reaction aid to the white medium-viscosity solution, mixing and stirring at a speed of 80-150 r / min to react, to obtain a milky white low-viscosity solution with a viscosity of ≤700 mPa·s; Step S004, spray drying the milky white low-viscosity solution to obtain white spherical powder; Step S005: the white spherical powder is calcined at 800-1280° C. to obtain low-cost, high-purity, and high-densification spherical magnesium oxide powder.
2. The method for preparing low-cost, high-purity and high-densification spherical magnesium oxide powder according to claim 1, characterized in that: The magnesium chloride salt is at least one of the following: anhydrous magnesium chloride, magnesium chloride hexahydrate, ethyl magnesium chloride; The magnesium sulfate salt is at least one of the following: anhydrous magnesium sulfate, magnesium sulfate heptahydrate, magnesium sulfate trihydrate, and magnesium sulfate hexahydrate.
3. The method for preparing low-cost, high-purity and high-densification spherical magnesium oxide powder according to claim 1, characterized in that: The mass ratio of the magnesium oxide ceramic powder, the soluble magnesium ion salt and water is 15-35:10-15:55-75; The dosage of magnesium ion surfactant is 0.1-0.5% of the mass of soluble magnesium ion salt; The dosage of the reaction aid is 1-5% of the mass of the soluble magnesium ion salt.
4. The method for preparing low-cost, high-purity and high-densification spherical magnesium oxide powder according to claim 1, characterized in that: The magnesium oxide ceramic powder has a purity of 99wt%, a particle size d50≤10μm, a pH≤10, a Mohs hardness of 6, and a specific surface area of <15.6m 2 / g.
5. The method for preparing low-cost, high-purity and high-densification spherical magnesium oxide powder according to claim 1, characterized in that: In step S004, the inlet air temperature of the spray drying is controlled to be ≥180°C, the outlet air temperature is 60°C, and the atomizing disk rotation speed is ≥180Hz.
6. The method for preparing low-cost, high-purity and high-densification spherical magnesium oxide powder according to claim 1, characterized in that: In the step S005, the heating rate to 800-1280°C is 1.5°C-3°C / min; The calcination time at 800-1280°C is not less than 3h.
7. A low-cost, high-purity, high-densification spherical magnesium oxide powder, characterized in that: The low-cost, high-purity, high-densification spherical magnesium oxide powder is prepared by the preparation method according to any one of claims 1 to 6; the particle size d50 is 5-120 μm, the magnesium oxide content is ≥98wt%, the sphericity is ≥96%, and the specific surface area is <0.3m 2 / g, conductivity ≤40μS / cm, pH ≤9, compressive strength ≥18MPa.