Modified sodium ion battery positive electrode material and preparation method thereof, sodium ion battery

By using the nickel-ferromanganese hydroxide precursor and sodium source to sinter and dry ice treatment in the sodium ion battery positive electrode material, a modified positive electrode material with O3 and P3 composite phase was prepared, which solved the structural changes in the prior art The problem of electrochemical performance degradation improves cycling performance and energy density, is suitable for large-scale production and reduces costs.

CN118561341BActive Publication Date: 2024-11-05GANZHOU NOVA TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411035844.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-05
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The existing sodium ion battery positive electrode materials have irreversible structural changes during charging and discharging, resulting in a decrease in electrochemical performance. The specific capacity of P-type layered oxides is relatively low, making it difficult to meet the needs of high energy density and long life.

Method used

The nickel ferromanganese hydroxide precursor and sodium source were sintered under an oxidative atmosphere, and cooled to a specified temperature and stayed in dry ice to prepare a sodium ion battery positive electrode material with O3 and P3 composite phases, and the co-precipitation method was used. Preparation of the precursor and control the sintering temperature and time to form a modified positive electrode material with spherical or spherical secondary particles morphology.

Benefits of technology

The cycling performance and energy density of the cathode material are improved, the high capacity of the O3 phase and the rapid dynamic characteristics of the P3 phase are achieved, the overall performance of the battery is enhanced, suitable for large-scale production and reduced costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118561341B_ABST
    Figure CN118561341B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a modified sodium ion battery positive electrode material, comprising: mixing a precursor with a sodium source, sintering in an oxidizing atmosphere, and transferring the obtained product to dry ice for a period of time after cooling to a specified temperature with a furnace to obtain a modified sodium ion battery positive electrode material. The modified sodium ion battery positive electrode material prepared by the method of the present invention has better cycle performance, and the method has the advantages of simple process and low cost, and can meet the needs of large-scale production. The present invention also provides a modified sodium ion battery positive electrode material prepared by the aforementioned method, which has a composite phase structure of O3 phase and P3 phase, the O3 phase can ensure the high capacity of the material, the P3 phase can ensure the characteristics of the rapid kinetics of sodium ions in the material, and realize the complementary effect of the two phases, and after the sintered material stays in dry ice, the obtained positive electrode material has better electrochemical performance. The provided modified sodium ion battery positive electrode material has excellent performance for sodium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of sodium ion batteries, and in particular relates to a modified sodium ion battery positive electrode material and a preparation method thereof, and a sodium ion battery. Background Art

[0002] As the environmental crisis caused by fossil fuel consumption becomes increasingly serious, it is imperative to achieve sustainable development by using renewable clean energy such as solar energy, wind energy, tidal energy, and geothermal energy. However, due to the instability and intermittent output of these renewable clean energy sources, their practical applications are severely limited. Among many energy storage technologies, electrochemical energy storage has broad application prospects in the energy field due to its advantages such as high energy density, high energy conversion efficiency, and simple maintenance. Compared with lead-acid batteries and zinc-silver batteries containing toxic heavy metals, environmentally friendly lithium-ion batteries and sodium-ion batteries have attracted widespread attention. Due to the uneven distribution of precious metals such as lithium and cobalt, the production cost of lithium-ion batteries has continued to rise. Sodium-ion batteries, which are abundant in resources and low in cost, are expected to play an important role in new energy storage applications.

[0003] In sodium-ion batteries, positive electrode materials, as key components, have a considerable impact on the energy density of the battery. Positive electrode materials include O-type and P-type layered oxides, polyanionic compounds, Prussian blue and its analogs. Among them, layered oxides have high specific capacity, synthesis technology is close to the lithium battery positive electrode process route, and there are relatively many types of active sodium-ion battery layered oxides, so they have significant advantages in industrial-scale production. O-type layered oxides have become the most promising material for large-scale production due to their high specific capacity and easy synthesis, but they have complex phase changes during the charge and discharge process, resulting in irreversible structural changes and a significant decrease in electrochemical performance. P-type layered oxides have the advantages of high structural stability and rapid sodium ion kinetics, but their low Na content leads to a low specific capacity. Therefore, it is urgent to develop high-energy-density and long-life positive electrode materials for sodium-ion batteries. Summary of the invention

[0004] In response to the above technical problems, the present application provides a modified sodium ion battery positive electrode material and a preparation method thereof, and a sodium ion battery.

[0005] To achieve the above objectives, this application proposes the following technical solutions:

[0006] In a first aspect, a method for preparing a modified sodium ion battery positive electrode material is provided, comprising:

[0007] The nickel-iron-manganese hydroxide precursor is mixed with a sodium source and sintered in an oxidizing atmosphere. After the sintering is completed, it is cooled to a specified temperature in the furnace and then transferred to dry ice for a period of time to obtain a sodium ion battery positive electrode material with an O3 and P3 composite phase.

[0008] Furthermore, the specified temperature is 100-900° C.; and the residence time is 10-60 min.

[0009] Furthermore, the dry ice is located in a sealed container; and the mass ratio of the theoretical amount of the sintered product to the dry ice is 1:0.8-1.5.

[0010] Furthermore, the molar ratio of sodium in the sodium source to the precursor is 1.05-1.30:1.

[0011] Furthermore, the sodium source is one or more of sodium carbonate, sodium bicarbonate, and sodium oxalate.

[0012] Furthermore, the chemical formula of the nickel-iron-manganese hydroxide precursor is Ni a Fe b Mn c (OH) 2 , where 0≤a≤1, 0≤b≤1, 0≤c≤1.

[0013] Furthermore, the sintering temperature is 700-950° C.; the sintering time is 10-24 hours; the heating rate during the sintering process is 2-5° C. / min; and the atmosphere during the sintering process is an oxygen atmosphere.

[0014] Furthermore, the nickel-iron-manganese hydroxide precursor is prepared by a co-precipitation method.

[0015] Furthermore, the preparation method of the nickel-iron-manganese hydroxide precursor comprises:

[0016] (1) A mixed metal salt solution of nickel, iron and manganese, an alkali solution and an ammonia solution are introduced into a reaction kettle in parallel, heated and stirred to carry out a coprecipitation reaction, and obtain a reaction slurry;

[0017] (2) After aging, solid-liquid separation, washing and drying the reaction slurry, a precursor material is obtained.

[0018] Furthermore, in step (1), the temperature of the coprecipitation reaction system is controlled to be 60-80°C, the pH is 8-13, the stirring speed is 400-1000 r / min, and the ammonia concentration is 10-20 g / L.

[0019] In a second aspect, a modified sodium ion battery positive electrode material is provided, which is prepared using the aforementioned preparation method.

[0020] Furthermore, the modified positive electrode material has a spherical or quasi-spherical secondary particle morphology; the average diameter of the secondary particles is 3-5 μm; and the modified positive electrode material has O3 and P3 phases.

[0021] In a third aspect, a sodium ion battery is provided, comprising the aforementioned modified sodium ion battery positive electrode material.

[0022] Compared with the prior art, one or more of the above technical solutions can achieve at least one of the following beneficial effects:

[0023] Preparation of NaNi by sintering a Fe b Mn c O 2 When the sintering is completed, the positive electrode material is transferred to dry ice and kept for a period of time after the furnace is cooled to the specified temperature. The modified sodium ion battery positive electrode material obtained has better cycle performance. This method has the advantages of simple process and low cost, and can meet the needs of large-scale production.

[0024] The cathode material prepared by this method has a composite phase structure of O3 phase and P3 phase. The O3 phase can ensure the high capacity of the material, and the P3 phase can ensure the rapid kinetics of sodium ions in the material, thereby achieving the complementary effect of the two phases and ultimately improving the performance of the cathode material. a Fe b Mn c O 2 After staying at a specified temperature for a period of time, it is beneficial to improve the performance of the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1 This is the X-ray diffraction pattern of the positive electrode material prepared in Example 1.

[0027] Figure 2 This is the SEM image of the positive electrode material prepared in Example 1.

[0028] Figure 3 This is the X-ray diffraction pattern of the positive electrode material prepared in Comparative Example 1.

[0029] Figure 4 This is the SEM image of the positive electrode material prepared in Comparative Example 1.

[0030] Figure 5 Cycling curves of batteries assembled with the positive electrode materials of Example 1 and Comparative Example 1 at a current density of 130 mA / g.

[0031] Figure 6 This is the X-ray diffraction pattern of the positive electrode material prepared in Comparative Example 2.

[0032] Figure 7 This is a cycle curve diagram of a battery assembled with the positive electrode material prepared in Comparative Example 2 at a current density of 130 mA / g.

[0033] Figure 8 This is the SEM image of the positive electrode material prepared in Example 2.

[0034] Fig. 9 This is the SEM image of the positive electrode material prepared in Example 3.

[0035] Fig.10 Cycling curve of a battery assembled with the positive electrode material prepared in Example 2 at a current density of 130 mA / g.

[0036] Fig.11 Cycling curve of a battery assembled with the positive electrode material prepared in Example 3 at a current density of 130 mA / g.

[0037] Fig.12 Cycling curve of a battery assembled with the positive electrode material prepared in Example 4 at a current density of 130 mA / g.

[0038] Fig.13 This is the SEM image of the positive electrode material prepared in Example 5.

[0039] Fig.14 Cycling curve of a battery assembled with the positive electrode material prepared in Example 5 at a current density of 130 mA / g. DETAILED DESCRIPTION

[0040] The present invention provides a method for preparing a modified sodium ion battery positive electrode material, comprising:

[0041] The nickel-iron-manganese hydroxide precursor is mixed with a sodium source and sintered in an oxidizing atmosphere. The sintered product is cooled to a specified temperature in a furnace and then transferred to dry ice for a period of time to obtain a sodium ion battery positive electrode material having an O3 and P3 composite phase.

[0042] In some preferred embodiments, the designated temperature is 100-900°C, more preferably 300-900°C, and even more preferably 500-900°C, for example, 500°C, 600°C, 700°C, 800°C, 900°C, etc.; the residence time is 10-60 min, for example, 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, etc.

[0043] In the above technical scheme, more specifically, the sintered product after being cooled to a specified temperature in the furnace is transferred to a closed container filled with dry ice; in some preferred embodiments, the dry ice is located in a closed container; the mass ratio of the theoretical amount of the sintered product to the dry ice is 1:0.8~1.5, for example, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, etc., and the average particle size of the dry ice is 3~5 mm.

[0044] In some preferred embodiments, the molar ratio of sodium in the sodium source to the precursor is 1.05-1.30:1, for example, 1.05:1, 1.1:1, 1.15:1, 1.2:1, 1.25:1, 1.3:1, etc.

[0045] In some preferred embodiments, the sodium source is one or more of sodium carbonate, sodium bicarbonate, and sodium oxalate.

[0046] In some preferred embodiments, the chemical formula of the precursor is Ni a Fe b Mn c (OH) 2 , where 0≤a≤1, 0≤b≤1, 0≤c≤1.

[0047] In some preferred embodiments, the sintering temperature is 700~950 ℃, for example, 700℃, 750℃, 800℃, 850℃, 900℃, 950℃, etc.; the sintering time is 10~24 h, for example, 10h, 12h, 14h, 16h, 18h, 20h, 22h, 24h, etc.; the heating rate during the sintering process is 2~5 ℃ / min; the atmosphere during the sintering process is an oxygen atmosphere.

[0048] In some embodiments, the nickel-iron-manganese hydroxide precursor is prepared by a co-precipitation method.

[0049] In some preferred embodiments, the method for preparing the nickel-iron-manganese hydroxide precursor comprises:

[0050] (1) A mixed metal salt solution of nickel, iron and manganese, an alkali solution and an ammonia solution are introduced into a reaction kettle in parallel, heated and stirred to carry out a coprecipitation reaction, and obtain a reaction slurry;

[0051] (2) After aging, solid-liquid separation, washing and drying the reaction slurry, a precursor material is obtained.

[0052] During the coprecipitation process, the process parameters can be conventionally controlled. For example, in step (1), the temperature of the coprecipitation reaction system can be controlled to be 50-70 °C, the pH to be 8-13, the stirring speed to be 400-1000 r / min, and the ammonia concentration to be 10-20 g / L.

[0053] The nickel source used to prepare the mixed metal salt solution can be one or more of nickel sulfate, nickel chloride, nickel nitrate, and nickel acetate; the iron source used to prepare the mixed metal salt solution can be one or more of iron sulfate, iron chloride, and iron nitrate; the manganese source used to prepare the mixed metal salt solution can be one or more of manganese nitrate, manganese sulfate, and manganese chloride. Based on cost and impurity content, sulfate is more preferred.

[0054] The concentration of the mixed metal salt solution of nickel, iron and manganese can adopt the conventional mixed metal salt concentration of the precursor prepared by coprecipitation reaction in the art; in some embodiments, the total metal concentration in the mixed metal salt solution of nickel, iron and manganese is 1-5 mol / L.

[0055] The alkali solution can be a sodium hydroxide solution or a potassium hydroxide solution. In order to reduce costs, a sodium hydroxide solution can be used. The concentration of the alkali solution can be the concentration of the alkali solution used to prepare the precursor by coprecipitation reaction in the art. In some embodiments, the concentration of the alkali solution is 5-10 mol / L.

[0056] The concentration of the ammonia solution can be the concentration of the ammonia solution of the precursor prepared by the coprecipitation reaction in the art; in some embodiments, the concentration of the ammonia solution is 6-12 mol / L.

[0057] In step (2), the aging time can be a conventional aging time. Specifically, in some implementation methods, the aging time is 12 to 24 hours.

[0058] The present invention provides a modified sodium ion battery positive electrode material, which is prepared by the above-mentioned preparation method.

[0059] In some preferred embodiments, the modified positive electrode material has a spherical or quasi-spherical secondary particle morphology; the average diameter of the secondary particles is 3~5 μm; the modified positive electrode material has O3 and P3 phases, specifically, in the modified positive electrode material, the P3 phase is located in the surface area of ​​the modified positive electrode material.

[0060] The present invention provides a sodium ion battery, comprising the aforementioned modified sodium ion battery positive electrode material.

[0061] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the specification, but the protection scope of the present invention is not limited to the following specific embodiments.

[0062] Example 1

[0063] (1) preparing a soluble mixed metal sulfate solution of nickel, iron and manganese according to a molar ratio of Ni:Fe:Mn=1:1:1, wherein the total molar concentration of metal ions of nickel, iron and manganese is 2.5 mol / L;

[0064] (2) Prepare 5 mol / L sodium hydroxide solution and 6 mol / L ammonia solution;

[0065] (3) Add the mixed metal salt solution, sodium hydroxide solution and ammonia water into the reactor in parallel, control the pH value to 10, the reaction temperature to 55 °C, the stirring speed to 450 r / min, and the ammonia concentration to 15 g / L. When the addition of the mixed metal salt solution is completed, stop adding the sodium hydroxide solution and ammonia water at the same time, continue stirring, stir and age the reaction for 10 h, and then stop the reaction;

[0066] (4) filtering the slurry obtained by the reaction, washing it with pure water for multiple times, and drying it in an oven at 120°C to obtain a precursor material;

[0067] (5) The obtained precursor material and sodium carbonate are proportioned and mixed at a molar ratio of precursor to sodium of 1:1.15, and then sintered at 950°C for 12 h in an oxygen atmosphere. After cooling to about 700°C, the powder is immediately transferred to a sealed container containing 10 g of dry ice with a particle size of about 3 mm (the theoretical calculated amount of the obtained powder and the mass ratio of dry ice is 1:0.9), and reacted with the dry ice for 20 min to obtain a positive electrode material. In this embodiment, the dry ice is initially placed in a thermos bottle. After the sintered product is cooled to about 705°C, the required amount of dry ice is weighed and placed in a sealed container, and then the sintered product is quickly transferred to the sealed container.

[0068] Figure 1 The X-ray diffraction pattern of the sample prepared in Example 1 is as follows: Figure 1 It can be seen that the positive electrode composite material has O3 and P3 phases. Figure 2 This is a SEM image of the sample prepared in Example 1. It can be seen from the image that the positive electrode composite material is spherical with a diameter of about 3-5 μm.

[0069] Comparative Example 1

[0070] (1) A soluble mixed metal sulfate solution of nickel, iron and manganese is prepared according to a molar ratio of Ni:Fe:Mn=1:1:1, wherein the total molar concentration of metal ions of nickel, iron and manganese is 2 mol / L;

[0071] (2) Prepare 6 mol / L sodium hydroxide solution and 8 mol / L ammonia solution;

[0072] (3) Add the mixed metal salt solution, sodium hydroxide solution and ammonia water into the reactor in parallel, control the pH value to 11, the reaction temperature to 60 °C, the stirring speed to 550 r / min, and the ammonia concentration to 15 g / L. When the addition of the mixed metal salt solution is completed, stop adding the sodium hydroxide solution and ammonia water at the same time, continue stirring, and stir and age the reaction for 12 h before stopping the reaction;

[0073] (4) filtering the slurry obtained by the reaction, washing it with pure water for multiple times, and drying it in an oven at 120°C to obtain a precursor material;

[0074] (5) The obtained precursor material is mixed with sodium carbonate at a molar ratio of 1:1.2, and then sintered at 950 °C for 12 h in an oxygen atmosphere to obtain a positive electrode material NaNi 0.33 Fe 0.33 Mn 0.33 O 2 .

[0075] Figure 3 The X-ray diffraction pattern of the sample prepared in Comparative Example 1 is as follows: Figure 3 It can be seen that the positive electrode material obtained in Comparative Example 1 only has O3 phase. Figure 4 This is a SEM image of the sample prepared in Comparative Example 1. It can be seen from the image that the positive electrode material obtained in Comparative Example 1 is spherical with a diameter of about 3-5 μm.

[0076] The positive electrode materials prepared in Example 1 and Comparative Example 1 were respectively prepared into positive electrode sheets, and metallic sodium was used as the negative electrode, and button batteries were respectively assembled. The button batteries were subjected to charge and discharge tests in the voltage range of 2V~4V at 25°C.

[0077] Figure 5 The cycle curves of the battery assembled with the positive electrode materials of Example 1 and Comparative Example 1 at a current density of 130 mA / g are shown in FIG. Figure 5It can be seen that the cycle performance of the battery assembled with the positive electrode material prepared in Example 1 is better than that of the battery assembled with the positive electrode material prepared in Comparative Example 1. After 300 cycles, the battery assembled with the positive electrode material of Example 1 has a specific capacity of 85.4 mAh / g and a capacity retention rate of 82.6%; while the battery assembled with the positive electrode material of Comparative Example 1 has a specific capacity of 58.4 mAh / g, and a capacity retention rate of only 47.2%. The above results show that the performance of the modified positive electrode material is significantly improved. After analysis, the reason for this phenomenon may be that the obtained positive electrode material is transferred to dry ice during the cooling process. On the one hand, it can achieve rapid cooling of the positive electrode material. On the other hand, while the dry ice rapidly cools the positive electrode material, a large amount of carbon dioxide is released. A large amount of carbon dioxide reacts with the sodium in the O3 phase material on the surface of the positive electrode material, so that part of the sodium in the O3 phase on the surface of the positive electrode material is released, the interlayer spacing is increased, and it is converted into a P3 phase sodium positive electrode material.

[0078] Comparative Example 2

[0079] (1) A soluble mixed metal sulfate solution of nickel, iron and manganese is prepared according to a molar ratio of Ni:Fe:Mn=1:1:1, wherein the total molar concentration of metal ions of nickel, iron and manganese is 2 mol / L;

[0080] (2) Prepare 6 mol / L sodium hydroxide solution and 8 mol / L ammonia solution;

[0081] (3) Add the mixed metal salt solution, sodium hydroxide solution and ammonia water into the reactor in parallel, control the pH value to 11, the reaction temperature to 60°C, the stirring speed to 550 r / min, and the ammonia concentration to 15 g / L. When the addition of the mixed metal salt solution is completed, stop adding the sodium hydroxide solution and ammonia water at the same time, continue stirring, and stir and age the reaction for 12 h before stopping the reaction;

[0082] (4) filtering the slurry obtained by the reaction, washing it with pure water for multiple times, and drying it in an oven at 120°C to obtain a precursor material;

[0083] (5) The obtained precursor material is mixed with sodium carbonate at a molar ratio of 1:1.2, and then sintered at 800 °C for 12 h in an oxygen atmosphere. The obtained material powder is transferred to a tubular furnace into which carbon dioxide gas is continuously introduced for cooling to obtain a positive electrode material.

[0084] Figure 6 The X-ray diffraction pattern of the positive electrode material prepared in Comparative Example 2 is as follows: Figure 6 It can be seen that the positive electrode material has O3 and P3 phases.

[0085] The positive electrode material prepared in Comparative Example 2 was prepared into a positive electrode sheet, and metallic sodium was used as the negative electrode, and button batteries were assembled respectively. The button batteries were subjected to charge and discharge tests in the voltage range of 2 V to 4 V at 25°C.

[0086] Figure 7 This is a cycle curve of a battery assembled with the positive electrode material prepared in Comparative Example 2 at a current density of 130 mA / g. Figure 7 It can be seen that within the voltage range of 2V~4V, after 200 cycles, it has a specific capacity of 45.6 mAh / g and a capacity retention rate of 40.7%. By comparing the cycle performance of the battery assembled with the positive electrode materials prepared in Example 1 and Comparative Examples 1 and 2, it can be seen that the cycle performance of the battery assembled with the positive electrode materials prepared in Comparative Example 2 is worse than that of the battery assembled with the positive electrode materials prepared in Example 1 and Comparative Example 1. This shows that cooling the sintered product in a carbon dioxide atmosphere, although positive electrode materials of O3 and P3 phases can be obtained, will reduce the electrochemical properties of the material. After analysis, the reason for this phenomenon may be: during the cooling process, the obtained positive electrode material is transferred into dry ice to achieve rapid cooling of the positive electrode material. The rapid cooling process may have a certain effect on the structure of the positive electrode material on the one hand, and on the other hand, it also plays a certain control role in the reaction of the surface material with the carbon dioxide released by the dry ice cooling.

[0087] Example 2

[0088] (1) A soluble mixed metal sulfate solution of nickel, iron and manganese is prepared according to a molar ratio of Ni:Fe:Mn=4:4:2, wherein the total molar concentration of metal ions of nickel, iron and manganese is 3 mol / L;

[0089] (2) Prepare 5 mol / L sodium hydroxide solution and 8 mol / L ammonia solution;

[0090] (3) Add the mixed metal salt solution, sodium hydroxide solution and ammonia water into the reactor in parallel, control the pH value to 9, the reaction temperature to 65 °C, the stirring speed to 500 r / min, and the ammonia concentration to 12 g / L. When the addition of the mixed metal salt solution is completed, stop adding the sodium hydroxide solution and ammonia water at the same time, continue stirring, and stir and age the reaction for 12 h before stopping the reaction;

[0091] (4) filtering the slurry obtained by the reaction, washing it with pure water for multiple times, and drying it in an oven at 120°C to obtain a precursor material;

[0092] (5) The obtained precursor material and sodium carbonate are proportioned and mixed at a molar ratio of precursor to sodium of 1:1.25, and then sintered at 900°C for 15 h in an oxygen atmosphere. After cooling to about 500°C, the powder is immediately transferred to a sealed container containing 5 g of dry ice with a particle size of about 3 mm (the theoretical calculated amount of the obtained powder and the mass ratio of dry ice is 1:1.5), and reacted with the dry ice for 10 min to obtain a positive electrode material. In this embodiment, the dry ice is initially placed in a thermos bottle. After the sintered product is cooled to about 505°C, the required amount of dry ice is weighed and placed in a sealed container, and then the sintered product is quickly transferred to the sealed container.

[0093] Figure 8 This is a SEM image of the sample prepared in Example 2. It can be seen from the image that the positive electrode composite material is spherical with a diameter of about 3-5 μm.

[0094] Example 3

[0095] (1) A soluble mixed metal sulfate solution of nickel, iron and manganese is prepared according to a molar ratio of Ni:Fe:Mn=4:4:2, wherein the total molar concentration of metal ions of nickel, iron and manganese is 2 mol / L;

[0096] (2) Prepare 5 mol / L sodium hydroxide solution and 8 mol / L ammonia solution;

[0097] (3) Add the mixed metal salt solution, sodium hydroxide solution and ammonia water into the reactor in parallel, control the pH value to 11, the reaction temperature to 70 °C, the stirring speed to 550 r / min, and the ammonia concentration to 16 g / L. When the addition of the mixed metal salt solution is completed, stop adding the sodium hydroxide solution and ammonia water at the same time, continue stirring, and stir and age the reaction for 12 h before stopping the reaction;

[0098] (4) filtering the slurry obtained by the reaction, washing it with pure water for multiple times, and drying it in an oven at 120°C to obtain a precursor material;

[0099] (5) The obtained precursor material and sodium carbonate are proportioned and mixed at a molar ratio of precursor to sodium of 1:1.25, and then sintered at 950°C for 12 h in an oxygen atmosphere. After cooling to about 900°C, the powder is immediately transferred to a sealed container containing 5 g of dry ice with a particle size of about 3 mm (the theoretical calculated amount of the obtained powder and the mass ratio of dry ice is 1:0.8), and reacted with the dry ice for 20 min to obtain a positive electrode material. In this embodiment, the dry ice is initially placed in a thermos bottle. After the sintered product is cooled to about 910°C, the required amount of dry ice is weighed and placed in a sealed container, and then the sintered product is quickly transferred to the sealed container.

[0100] Fig. 9This is a SEM image of the sample prepared in Example 3. It can be seen from the image that the positive electrode composite material is spherical with a diameter of about 3-5 μm.

[0101] The positive electrode materials prepared in Example 2 and Example 3 were respectively prepared into positive electrode sheets, and metal sodium was used as the negative electrode, and button batteries were respectively assembled. The button batteries were subjected to charge and discharge tests at 25° C. in the voltage range of 2V to 4V.

[0102] Fig.10 This is a cycle curve of a battery assembled with the positive electrode material prepared in Example 2 at a current density of 130 mA / g. As can be seen from the figure, after 300 cycles, it has a specific capacity of 91.7 mAh / g and a capacity retention rate of 81.5%.

[0103] Fig.11 The cycle curve of the battery assembled with the positive electrode material prepared in Example 3 at a current density of 130 mA / g is shown in the figure. As can be seen from the figure, after 300 cycles, the specific capacity is 82.6 mAh / g, and the capacity retention rate is 79.7%.

[0104] Example 4

[0105] (1) A soluble mixed metal sulfate solution of nickel, iron and manganese was prepared according to a molar ratio of Ni:Fe:Mn=4:4:2, wherein the total molar concentration of metal ions of nickel, iron and manganese was 2.5 mol / L;

[0106] (2) Prepare 5 mol / L sodium hydroxide solution and 8 mol / L ammonia solution;

[0107] (3) Add the mixed metal salt solution, sodium hydroxide solution and ammonia water into the reactor in parallel, control the pH value to 11, the reaction temperature to 70 °C, the stirring speed to 500 r / min, and the ammonia concentration to 15 g / L. When the addition of the mixed metal salt solution is completed, stop adding the sodium hydroxide solution and ammonia water at the same time, continue stirring, and stir and age the reaction for 12 h before stopping the reaction;

[0108] (4) filtering the slurry obtained by the reaction, washing it with pure water for multiple times, and drying it in an oven at 120°C to obtain a precursor material;

[0109] (5) The obtained precursor material and sodium carbonate are proportioned and mixed at a molar ratio of precursor to sodium of 1:1.20, and then sintered at 950°C for 12 h in an oxygen atmosphere. After cooling to about 300°C, the powder is immediately transferred to a sealed container containing dry ice with a diameter of about 3 mm (the theoretical calculated amount of the obtained powder and the mass ratio of dry ice is 1:1.2), and reacted with the dry ice for 20 min to obtain a positive electrode material. In this embodiment, the dry ice is initially placed in a thermos bottle. After the sintered product is cooled to about 305°C, the required amount of dry ice is weighed and placed in a sealed container, and then the sintered product is quickly transferred to the sealed container.

[0110] The button cell was assembled in the same manner as in Example 1, and the electrochemical performance of the button cell was tested at 25° C. in a voltage range of 2 V to 4 V.

[0111] Fig.12 This is a cycle curve of a battery assembled with the positive electrode material prepared in Example 4 at a current density of 130 mA / g. As can be seen from the figure, after 300 cycles, the battery has a specific capacity of 77.5 mAh / g and a capacity retention rate of 70.8%.

[0112] Example 5

[0113] (1) A soluble mixed metal sulfate solution of nickel, iron and manganese was prepared according to a molar ratio of Ni:Fe:Mn=4:4:2, wherein the total molar concentration of metal ions of nickel, iron and manganese was 2.5 mol / L;

[0114] (2) Prepare 5 mol / L sodium hydroxide solution and 8 mol / L ammonia solution;

[0115] (3) Add the mixed metal salt solution, sodium hydroxide solution and ammonia water into the reactor in parallel, control the pH value to 11, the reaction temperature to 70 °C, the stirring speed to 500 r / min, and the ammonia concentration to 20 g / L. When the addition of the mixed metal salt solution is completed, stop adding the sodium hydroxide solution and ammonia water at the same time, continue stirring, and stir and age the reaction for 12 h before stopping the reaction;

[0116] (4) filtering the slurry obtained by the reaction, washing it with pure water for multiple times, and drying it in an oven at 120°C to obtain a precursor material;

[0117] (5) The obtained precursor material and sodium carbonate are proportioned and mixed at a molar ratio of precursor to sodium of 1:1.25, and then sintered at 950°C for 12 h in an oxygen atmosphere. After cooling to about 100°C, the powder is immediately transferred to a sealed container containing dry ice with a diameter of about 3 mm (the theoretical calculated amount of the obtained powder and the mass ratio of dry ice is 1:1.3), and reacted with the dry ice for 20 min to obtain a positive electrode material. In this embodiment, the dry ice is initially placed in a thermos bottle. After the sintered product is cooled to about 105°C, the required amount of dry ice is weighed and placed in a sealed container, and then the sintered product is quickly transferred to the sealed container.

[0118] Fig.13 This is a SEM image of the sample prepared in Example 5. It can be seen from the image that the positive electrode composite material is spherical with a diameter of about 3-5 μm.

[0119] The button cell was assembled in the same manner as in Example 1, and the electrochemical performance of the button cell was tested at 25° C. in a voltage range of 2 V to 4 V.

[0120] Fig.14 This is a cycle curve of a battery assembled with the positive electrode material prepared in Example 5 at a current density of 130 mA / g. As can be seen from the figure, after 300 cycles, it has a specific capacity of 71.4 mAh / g and a capacity retention rate of 64.91%.

[0121] By comparing the cycle performance of batteries assembled with the positive electrode materials prepared in each embodiment, it can be found that the cycle performance of batteries assembled with the positive electrode materials prepared in Embodiment 2 (500°C), Embodiment 1 (700°C) and Embodiment 3 (900°C) is better than that of batteries assembled with the positive electrode materials prepared in Embodiment 4 (300°C) and Embodiment 5 (100°C), and the performance of the positive electrode material prepared in Embodiment 2 is the best. After analysis, this may be because the appropriate temperature is conducive to reasonably controlling the cooling rate of the positive electrode material and the degree of reaction with the positive electrode material, which is conducive to obtaining a positive electrode material with a better structure.

[0122] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a modified sodium ion battery positive electrode material, characterized in that: include: After mixing the nickel iron manganese hydroxide precursor with the sodium source, sintering is carried out in an oxidizing atmosphere, and the sintered product is cooled to a specified temperature with the furnace and then transferred to dry ice for a period of time to obtain a sodium ion battery positive electrode material having an O3 and P3 composite phase; the specified temperature is 500-900° C.; the residence time is 10-60 min; and the molar ratio of sodium in the sodium source to the precursor is 1.05-1.30:

1.

2. The method for preparing the modified sodium ion battery positive electrode material according to claim 1, characterized in that: The dry ice is located in a sealed container; the mass ratio of the theoretical amount of the sintered product to the dry ice is 1:0.8-1.

5.

3. The method for preparing the modified sodium ion battery positive electrode material according to claim 1, characterized in that: The sodium source is one or more of sodium carbonate, sodium bicarbonate and sodium oxalate.

4. The method for preparing the modified sodium ion battery positive electrode material according to claim 1, characterized in that: The sintering temperature is 700-950° C.; the sintering time is 10-24 hours; the heating rate during the sintering process is 2-5° C. / min; and the atmosphere during the sintering process is an oxygen atmosphere.

5. The method for preparing the modified sodium ion battery positive electrode material according to claim 1, characterized in that: The nickel-iron-manganese hydroxide precursor is prepared by a coprecipitation method; The method for preparing the nickel-iron-manganese hydroxide precursor comprises: (1) A mixed metal salt solution of nickel, iron and manganese, an alkali solution and an ammonia solution are introduced into a reaction kettle in parallel, heated and stirred to carry out a coprecipitation reaction to obtain a reaction slurry; (2) After aging, solid-liquid separation, washing and drying the reaction slurry, a precursor material is obtained.

6. The method for preparing the modified sodium ion battery positive electrode material according to claim 5, characterized in that: In step (1), the temperature of the coprecipitation reaction system is controlled to be 60-80°C, the pH is 8-13, the stirring speed is 400-1000 r / min, and the ammonia concentration is 10-20 g / L.

7. Modified sodium ion battery positive electrode material, characterized in that: The method is described in any one of claims 1 to 6.

8. The modified sodium ion battery positive electrode material according to claim 7, characterized in that: The modified sodium ion battery positive electrode material has a spherical or quasi-spherical secondary particle morphology; the average diameter of the secondary particles is 3-5 μm; and the modified sodium ion battery positive electrode material has O3 and P3 phases.

9. A sodium ion battery, characterized in that Comprising the modified sodium ion battery positive electrode material as described in claim 7 or 8.

Citation Information

Patent Citations

  • Tin sulfide / graphene sodium ion battery composite cathode material and preparation method thereof

    CN106654192A

  • Sodium transition metal oxide with P3 structure and preparation method thereof, and sodium ion battery

    CN110380024A

  • O3-P2 composite phase sodium ion positive electrode material as well as preparation method and application thereof

    CN115148984A

  • Positive electrode material and preparation method thereof, positive electrode plate and sodium ion battery

    CN115611323A

  • Double-phase sodium-ion battery positive electrode material as well as preparation method and application thereof

    CN117658238A