A zinc tin oxide target material and preparation method thereof
By adding zinc oxide whiskers, graphene and other substances during the preparation process of the zinc oxide tin target, the problem of insufficient electrical conductivity of the existing zinc oxide tin target is solved, and the electrical conductivity and structural compactness are significantly improved.
Patent Information
- Application Number
- CN202411045970.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-08-01
AI Technical Summary
The existing zinc-tin oxide target materials have insufficient electrical conductivity and are difficult to meet the increasing technical needs.
By mixing zinc oxide, tin oxide, zinc powder, and tin powder evenly, and adding zinc oxide whiskers, sodium dodecyl benzene sulfonate, polyethylene glycol, graphene, polyvinylpyrrolidone, and carboxylic acid after plasma treatment Methylcellulose and other substances are used to form a modified liquid. After ultrasonic treatment, molding and sintering, a zinc-tin oxide target with excellent conductive properties is prepared.
It significantly improves the conductive properties of zinc-tin oxide targets, reduces porosity, increases carrier mobility and conduction speed, and forms a denser and uniformly sized structure.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of semiconductor materials, and in particular to a zinc tin oxide target material and a preparation method thereof. Background Art
[0002] In the semiconductor, optoelectronics, display technology and new energy industries, conductive films have become indispensable key materials because of their good conductivity. Zinc tin oxide films have been widely used due to their excellent optical, electrical properties and environmental stability. Zinc tin oxide targets are important raw materials for the preparation of such films, and their performance directly determines the quality and performance of the final product.
[0003] The zinc oxide tin targets currently available on the market still have many deficiencies in their electrical conductivity and are unable to meet the increasing technological demands. Summary of the invention
[0004] The invention provides a zinc tin oxide target material and a preparation method thereof. The zinc tin oxide target material has excellent electrical conductivity.
[0005] The present invention solves the technical problem by adopting the following technical solutions:
[0006] A method for preparing a zinc tin oxide target comprises the following steps:
[0007] (1) zinc oxide, tin oxide, zinc powder and tin powder are uniformly mixed, and the mixed powder is subjected to plasma treatment to obtain a precursor;
[0008] (2) adding zinc oxide whiskers, sodium dodecylbenzene sulfonate, and polyethylene glycol to a sulfuric acid solution and stirring the mixture to obtain a first modified solution;
[0009] (3) adding graphene, polyvinyl pyrrolidone and carboxymethyl cellulose into a phosphoric acid solution and dispersing them evenly to obtain a second modified solution;
[0010] (4) Adding the precursor and the first modified liquid into the second modified liquid, stirring evenly, ultrasonically treating, drying, compression molding, and sintering to obtain a zinc tin oxide target.
[0011] The invention firstly mixes zinc oxide, tin oxide, zinc powder and tin powder uniformly, and adds zinc powder and tin powder into the mixed powder to play an activation role, effectively improve the activity of the mixed powder, improve the overall stability, promote the refinement of grains, and improve the compactness of the powder; the invention introduces zinc oxide whiskers and graphene into the mixed powder in the form of solutions, respectively, and sodium dodecylbenzene sulfonate, polyethylene glycol, polyvinyl pyrrolidone, carboxymethyl cellulose, sulfuric acid and phosphoric acid can further improve the activity of the system, improve the plasticity of the mixed powder, effectively inhibit the growth of grains, promote the formation of a more compact and uniform-sized structure, reduce porosity, improve the mobility of carriers, increase the conduction speed and efficiency, and effectively improve the conductive performance of the target material.
[0012] As a preferred embodiment of the present invention, the mass ratio of zinc oxide, tin oxide, zinc powder and tin powder is (45-55): (45-55): (2-8): (2-8).
[0013] As a preferred embodiment of the present invention, the voltage of the plasma treatment is 220V, the power is 300-600W, and the time is 4-8min.
[0014] As a preferred embodiment of the present invention, the mass ratio of the zinc oxide whisker, sodium dodecylbenzene sulfonate, polyethylene glycol, and sulfuric acid solution is 1: (0.1-0.3): (0.1-0.3): (15-22).
[0015] As a preferred embodiment of the present invention, the mass ratio of the graphene, polyvinyl pyrrolidone, carboxymethyl cellulose and phosphoric acid solution is 1: (0.1-0.3): (0.1-0.3): (15-22).
[0016] As a preferred embodiment of the present invention, the molar concentration of the sulfuric acid solution is 1 to 5 mol / L;
[0017] The molar concentration of the phosphoric acid solution is 1-5 mol / L.
[0018] As a preferred embodiment of the present invention, the mass ratio of the precursor, the first modifying liquid, and the second modifying liquid is 1:(3-6):(0.5-2).
[0019] As a preferred embodiment of the present invention, the compression molding pressure is 45-60 MPa, and the compression molding time is 4-8 min.
[0020] As a preferred embodiment of the present invention, the sintering temperature is 1380-1420° C., and the sintering time is 3-6 hours.
[0021] As a preferred embodiment of the present invention, the power of the ultrasonic treatment is 300-500W, and the time of the ultrasonic treatment is 20-40min.
[0022] As a preferred embodiment of the present invention, the purity of the zinc oxide is 3N (99.9%, the same below) to 5N (99.999%, the same below).
[0023] As a preferred embodiment of the present invention, the purity of the tin oxide is 3N (99.9%) to 5N (99.999%).
[0024] As a preferred embodiment of the present invention, the purity of the zinc powder is 3N (99.9%) to 5N (99.999%).
[0025] As a preferred embodiment of the present invention, the purity of the tin powder is 3N (99.9%) to 5N (99.999%).
[0026] It should be noted that the plasma treatment is carried out in a conventional plasma reaction vessel.
[0027] The present invention also provides a zinc tin oxide target material, which is prepared by the above-mentioned preparation method.
[0028] The beneficial effects of the present invention are as follows: the present invention firstly mixes zinc oxide, tin oxide, zinc powder and tin powder uniformly, and adds zinc powder and tin powder into the mixed powder to play an activation role, effectively improve the activity of the mixed powder, improve the overall stability, promote the refinement of grains, and improve the compactness of the powder; the present invention introduces zinc oxide whiskers and graphene into the mixed powder in the form of solutions, respectively, and sodium dodecylbenzene sulfonate, polyethylene glycol, polyvinyl pyrrolidone, carboxymethyl cellulose, sulfuric acid and phosphoric acid can further improve the activity of the system, improve the plasticity of the mixed powder, effectively inhibit the growth of grains, promote the formation of a more compact and uniformly sized structure, reduce porosity, improve the mobility of carriers, improve the conduction speed and efficiency, and effectively improve the conductive performance of the target material. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0031] In the present invention, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0032] In the present invention, there is no particular limitation on the specific dispersion and stirring treatment methods.
[0033] The reagents or instruments used in the present invention without indicating the manufacturer are all conventional products that can be obtained commercially. The raw materials used in the comparative examples and the raw materials used in the parallel experiments of the embodiments are the same commercially available products unless otherwise specified.
[0034] Example 1
[0035] A method for preparing a zinc tin oxide target comprises the following steps:
[0036] (1) 3N pure zinc oxide, 3N pure tin oxide, 3N pure zinc powder, and 3N pure tin powder are mixed uniformly in a mass ratio of 50:50:5:5, and the mixed powder is placed in a plasma reaction vessel, and treated at a voltage of 220V, normal temperature and pressure (one atmosphere) and a power of 500W for 5 minutes, and then taken out to obtain a precursor;
[0037] (2) Add zinc oxide whiskers, sodium dodecylbenzene sulfonate, and polyethylene glycol to a 4 mol / L sulfuric acid solution, and stir evenly at a speed of 300 rpm to obtain a first modified solution; the mass ratio of the zinc oxide whiskers, sodium dodecylbenzene sulfonate, polyethylene glycol, and sulfuric acid solution is 1:0.2:0.2:20.
[0038] (3) Adding graphene, polyvinyl pyrrolidone and carboxymethyl cellulose to a 4 mol / L phosphoric acid solution, dispersing the mixture evenly at a speed of 300 rpm to obtain a second modified solution; the mass ratio of the graphene, polyvinyl pyrrolidone, carboxymethyl cellulose and phosphoric acid solution is 1:0.2:0.2:20.
[0039] (4) Add the precursor and the first modifying liquid to the second modifying liquid, stir evenly at a speed of 300 rpm, perform ultrasonic treatment at 400 W for 30 min, dry, mold at a pressure of 50 MPa for 6 min, and then sinter at 1400° C. for 4 h to obtain a zinc tin oxide target. The mass ratio of the precursor, the first modifying liquid, and the second modifying liquid is 1:4:1.
[0040] Example 2
[0041] A method for preparing a zinc tin oxide target comprises the following steps:
[0042] (1) 3N pure zinc oxide, 3N pure tin oxide, 3N pure zinc powder, and 3N pure tin powder are mixed uniformly in a mass ratio of 45:55:2:8, and the mixed powder is placed in a plasma reaction vessel, and treated at a voltage of 220V, normal temperature and pressure (one atmosphere) and a power of 500W for 5 minutes, and then taken out to obtain a precursor;
[0043] (2) Add zinc oxide whiskers, sodium dodecylbenzene sulfonate, and polyethylene glycol to a 4 mol / L sulfuric acid solution, and stir evenly at a speed of 300 rpm to obtain a first modified solution; the mass ratio of the zinc oxide whiskers, sodium dodecylbenzene sulfonate, polyethylene glycol, and sulfuric acid solution is 1:0.2:0.2:20.
[0044] (3) Adding graphene, polyvinyl pyrrolidone and carboxymethyl cellulose to a 4 mol / L phosphoric acid solution, dispersing the mixture evenly at a speed of 300 rpm to obtain a second modified solution; the mass ratio of the graphene, polyvinyl pyrrolidone, carboxymethyl cellulose and phosphoric acid solution is 1:0.2:0.2:20.
[0045] (4) Add the precursor and the first modifying liquid to the second modifying liquid, stir evenly at a speed of 300 rpm, perform ultrasonic treatment at 400 W for 30 min, dry, mold at a pressure of 50 MPa for 6 min, and then sinter at 1400° C. for 4 h to obtain a zinc tin oxide target. The mass ratio of the precursor, the first modifying liquid, and the second modifying liquid is 1:4:1.
[0046] Example 3
[0047] A method for preparing a zinc tin oxide target comprises the following steps:
[0048] (1) 3N pure zinc oxide, 3N pure tin oxide, 3N pure zinc powder, and 3N pure tin powder are mixed uniformly in a mass ratio of 55:45:8:2, and the mixed powder is placed in a plasma reaction vessel, and treated at a voltage of 220V, normal temperature and pressure (one atmosphere) and a power of 500W for 5 minutes, and then taken out to obtain a precursor;
[0049] (2) Add zinc oxide whiskers, sodium dodecylbenzene sulfonate, and polyethylene glycol to a 4 mol / L sulfuric acid solution, and stir evenly at a speed of 300 rpm to obtain a first modified solution; the mass ratio of the zinc oxide whiskers, sodium dodecylbenzene sulfonate, polyethylene glycol, and sulfuric acid solution is 1:0.2:0.2:20.
[0050] (3) Adding graphene, polyvinyl pyrrolidone and carboxymethyl cellulose to a 4 mol / L phosphoric acid solution, dispersing the mixture evenly at a speed of 300 rpm to obtain a second modified solution; the mass ratio of the graphene, polyvinyl pyrrolidone, carboxymethyl cellulose and phosphoric acid solution is 1:0.2:0.2:20.
[0051] (4) Add the precursor and the first modifying liquid to the second modifying liquid, stir evenly at a speed of 300 rpm, perform ultrasonic treatment at 400 W for 30 min, dry, mold at a pressure of 50 MPa for 6 min, and then sinter at 1400° C. for 4 h to obtain a zinc tin oxide target. The mass ratio of the precursor, the first modifying liquid, and the second modifying liquid is 1:4:1.
[0052] Example 4
[0053] A method for preparing a zinc tin oxide target comprises the following steps:
[0054] (1) 3N pure zinc oxide, 3N pure tin oxide, 3N pure zinc powder, and 3N pure tin powder are mixed uniformly in a mass ratio of 50:50:5:5, and the mixed powder is placed in a plasma reaction vessel, and treated at a voltage of 220V, normal temperature and pressure (one atmosphere) and a power of 500W for 5 minutes, and then taken out to obtain a precursor;
[0055] (2) Add zinc oxide whiskers, sodium dodecylbenzene sulfonate, and polyethylene glycol to a 4 mol / L sulfuric acid solution, and stir evenly at a speed of 300 rpm to obtain a first modified solution; the mass ratio of the zinc oxide whiskers, sodium dodecylbenzene sulfonate, polyethylene glycol, and sulfuric acid solution is 1:0.1:0.3:16.
[0056] (3) Adding graphene, polyvinyl pyrrolidone and carboxymethyl cellulose to a 4 mol / L phosphoric acid solution and dispersing them evenly at a speed of 300 rpm to obtain a second modified solution; the mass ratio of the graphene, polyvinyl pyrrolidone, carboxymethyl cellulose and phosphoric acid solution is 1:0.3:0.1:22.
[0057] (4) Add the precursor and the first modifying liquid to the second modifying liquid, stir evenly at a speed of 300 rpm, perform ultrasonic treatment at 400 W for 30 min, dry, mold at a pressure of 50 MPa for 6 min, and then sinter at 1400° C. for 4 h to obtain a zinc tin oxide target. The mass ratio of the precursor, the first modifying liquid, and the second modifying liquid is 1:4:1.
[0058] Example 5
[0059] A method for preparing a zinc tin oxide target comprises the following steps:
[0060] (1) 3N pure zinc oxide, 3N pure tin oxide, 3N pure zinc powder, and 3N pure tin powder are mixed uniformly in a mass ratio of 50:50:5:5, and the mixed powder is placed in a plasma reaction vessel, and treated at a voltage of 220V, normal temperature and pressure (one atmosphere) and a power of 500W for 5 minutes, and then taken out to obtain a precursor;
[0061] (2) Add zinc oxide whiskers, sodium dodecylbenzene sulfonate, and polyethylene glycol to a 4 mol / L sulfuric acid solution, and stir evenly at a speed of 300 rpm to obtain a first modified solution; the mass ratio of the zinc oxide whiskers, sodium dodecylbenzene sulfonate, polyethylene glycol, and sulfuric acid solution is 1:0.3:0.1:22.
[0062] (3) Adding graphene, polyvinyl pyrrolidone and carboxymethyl cellulose to a 4 mol / L phosphoric acid solution, dispersing the mixture evenly at a speed of 300 rpm to obtain a second modified solution; the mass ratio of the graphene, polyvinyl pyrrolidone, carboxymethyl cellulose and phosphoric acid solution is 1:0.1:0.3:16.
[0063] (4) Add the precursor and the first modifying liquid to the second modifying liquid, stir evenly at a speed of 300 rpm, perform ultrasonic treatment at 400 W for 30 min, dry, mold at a pressure of 50 MPa for 6 min, and then sinter at 1400° C. for 4 h to obtain a zinc tin oxide target. The mass ratio of the precursor, the first modifying liquid, and the second modifying liquid is 1:4:1.
[0064] Example 6
[0065] A method for preparing a zinc tin oxide target comprises the following steps:
[0066] (1) 3N pure zinc oxide, 3N pure tin oxide, 3N pure zinc powder, and 3N pure tin powder are mixed uniformly in a mass ratio of 50:50:5:5, and the mixed powder is placed in a plasma reaction vessel, and treated at a voltage of 220V, normal temperature and pressure (one atmosphere) and a power of 500W for 5 minutes, and then taken out to obtain a precursor;
[0067] (2) Add zinc oxide whiskers, sodium dodecylbenzene sulfonate, and polyethylene glycol to a 4 mol / L sulfuric acid solution, and stir evenly at a speed of 300 rpm to obtain a first modified solution; the mass ratio of the zinc oxide whiskers, sodium dodecylbenzene sulfonate, polyethylene glycol, and sulfuric acid solution is 1:0.2:0.2:20.
[0068] (3) Adding graphene, polyvinyl pyrrolidone and carboxymethyl cellulose to a 4 mol / L phosphoric acid solution, dispersing the mixture evenly at a speed of 300 rpm to obtain a second modified solution; the mass ratio of the graphene, polyvinyl pyrrolidone, carboxymethyl cellulose and phosphoric acid solution is 1:0.2:0.2:20.
[0069] (4) Add the precursor and the first modifying liquid to the second modifying liquid, stir evenly at a speed of 300 rpm, perform ultrasonic treatment at 400 W for 30 min, dry, mold at a pressure of 50 MPa for 6 min, and then sinter at 1400° C. for 4 h to obtain a zinc tin oxide target. The mass ratio of the precursor, the first modifying liquid, and the second modifying liquid is 1:3:2.
[0070] Example 7
[0071] A method for preparing a zinc tin oxide target comprises the following steps:
[0072] (1) 3N pure zinc oxide, 3N pure tin oxide, 3N pure zinc powder, and 3N pure tin powder are mixed uniformly in a mass ratio of 50:50:5:5, and the mixed powder is placed in a plasma reaction vessel, and treated at a voltage of 220V, normal temperature and pressure (one atmosphere) and a power of 500W for 5 minutes, and then taken out to obtain a precursor;
[0073] (2) Add zinc oxide whiskers, sodium dodecylbenzene sulfonate, and polyethylene glycol to a 4 mol / L sulfuric acid solution, and stir evenly at a speed of 300 rpm to obtain a first modified solution; the mass ratio of the zinc oxide whiskers, sodium dodecylbenzene sulfonate, polyethylene glycol, and sulfuric acid solution is 1:0.2:0.2:20.
[0074] (3) Adding graphene, polyvinyl pyrrolidone and carboxymethyl cellulose to a 4 mol / L phosphoric acid solution, dispersing the mixture evenly at a speed of 300 rpm to obtain a second modified solution; the mass ratio of the graphene, polyvinyl pyrrolidone, carboxymethyl cellulose and phosphoric acid solution is 1:0.2:0.2:20.
[0075] (4) Add the precursor and the first modifying liquid to the second modifying liquid, stir evenly at a speed of 300 rpm, perform ultrasonic treatment at 400 W for 30 min, dry, mold at a pressure of 50 MPa for 6 min, and then sinter at 1400° C. for 4 h to obtain a zinc oxide tin target. The mass ratio of the precursor, the first modifying liquid, and the second modifying liquid is 1:6:0.5.
[0076] Comparative Example 1
[0077] The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 is not treated with the first modifying liquid or the second modifying liquid, and the other aspects are the same.
[0078] A method for preparing a zinc tin oxide target comprises the following steps:
[0079] (1) 3N pure zinc oxide, 3N pure tin oxide, 3N pure zinc powder, and 3N pure tin powder are mixed uniformly in a mass ratio of 50:50:5:5, and the mixed powder is placed in a plasma reaction vessel, and treated at a voltage of 220V, normal temperature and pressure (one atmosphere) and a power of 500W for 5 minutes, and then taken out to obtain a precursor;
[0080] (2) The precursor was molded at a pressure of 50 MPa for 6 minutes, and then sintered at 1400° C. for 4 hours to obtain a zinc oxide tin target. The mass ratio of the precursor, the first modifying liquid, and the second modifying liquid was 1:4:1.
[0081] Comparative Example 2
[0082] The difference between Comparative Example 2 and Example 1 is that Comparative Example 2 is not treated with the first modifying liquid, and the other aspects are the same.
[0083] A method for preparing a zinc tin oxide target comprises the following steps:
[0084] (1) 3N pure zinc oxide, 3N pure tin oxide, 3N pure zinc powder, and 3N pure tin powder are mixed uniformly in a mass ratio of 50:50:5:5, and the mixed powder is placed in a plasma reaction vessel, and treated at a voltage of 220V, normal temperature and pressure (one atmosphere) and a power of 500W for 5 minutes, and then taken out to obtain a precursor;
[0085] (2) Adding graphene, polyvinyl pyrrolidone and carboxymethyl cellulose to a 4 mol / L phosphoric acid solution, dispersing the mixture evenly at a speed of 300 rpm to obtain a second modified solution; the mass ratio of the graphene, polyvinyl pyrrolidone, carboxymethyl cellulose and phosphoric acid solution is 1:0.2:0.2:20.
[0086] (3) Add the precursor to the second modified liquid, stir evenly at a speed of 300 rpm, perform ultrasonic treatment at 400 W for 30 min, dry, mold at a pressure of 50 MPa for 6 min, and then sinter at 1400° C. for 4 h to obtain a zinc oxide tin target. The mass ratio of the precursor, the first modified liquid, and the second modified liquid is 1:4:1.
[0087] Comparative Example 3
[0088] The difference between Comparative Example 3 and Example 1 is that Comparative Example 3 is not treated with the second modifying liquid, and the other aspects are the same.
[0089] A method for preparing a zinc tin oxide target comprises the following steps:
[0090] (1) 3N pure zinc oxide, 3N pure tin oxide, 3N pure zinc powder, and 3N pure tin powder are mixed uniformly in a mass ratio of 50:50:5:5, and the mixed powder is placed in a plasma reaction vessel, and treated at a voltage of 220V, normal temperature and pressure (one atmosphere) and a power of 500W for 5 minutes, and then taken out to obtain a precursor;
[0091] (2) Add zinc oxide whiskers, sodium dodecylbenzene sulfonate, and polyethylene glycol to a 4 mol / L sulfuric acid solution, and stir evenly at a speed of 300 rpm to obtain a first modified solution; the mass ratio of the zinc oxide whiskers, sodium dodecylbenzene sulfonate, polyethylene glycol, and sulfuric acid solution is 1:0.2:0.2:20.
[0092] (3) Add the precursor to the first modified liquid, stir evenly at a speed of 300 rpm, perform ultrasonic treatment at 400 W for 30 min, dry, mold at a pressure of 50 MPa for 6 min, and then sinter at 1400° C. for 4 h to obtain a zinc oxide tin target. The mass ratio of the precursor to the first modified liquid is 1:4.
[0093] The resistivity of the zinc tin oxide targets prepared in the examples and comparative examples is shown in Table 1.
[0094] Table 1. Test results of resistivity of zinc oxide tin target
[0095]
[0096] It can be seen from Table 1 that the zinc tin oxide target material of the present invention has excellent electrical conductivity.
[0097] By comparing Example 1 with Comparative Examples 1 to 3, it can be seen that the present invention significantly improves the conductive performance by modifying the target material with a first modifying liquid containing zinc oxide whiskers and a second modifying liquid containing graphene.
[0098] Finally, it should be noted that the above embodiments are intended to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a zinc tin oxide target, characterized in that: The following steps are involved: (1) zinc oxide, tin oxide, zinc powder and tin powder are uniformly mixed, and the mixed powder is subjected to plasma treatment to obtain a precursor; (2) adding zinc oxide whiskers, sodium dodecylbenzene sulfonate, and polyethylene glycol to a sulfuric acid solution and stirring the mixture to obtain a first modified solution; (3) adding graphene, polyvinyl pyrrolidone and carboxymethyl cellulose into a phosphoric acid solution and dispersing them evenly to obtain a second modified solution; (4) adding the precursor and the first modified liquid to the second modified liquid, stirring evenly, ultrasonically treating, drying, molding, and sintering to obtain a zinc tin oxide target; The mass ratio of the zinc oxide, tin oxide, zinc powder and tin powder is (45-55): (45-55): (2-8): (2-8); The voltage of the plasma treatment is 220V, the power is 300-600W, and the time is 4-8min; The sintering temperature is 1380-1420° C., and the sintering time is 3-6 hours.
2. The method for preparing a zinc tin oxide target according to claim 1, characterized in that: The mass ratio of the zinc oxide whisker, sodium dodecylbenzene sulfonate, polyethylene glycol and sulfuric acid solution is 1: (0.1-0.3): (0.1-0.3): (15-22).
3. The method for preparing the zinc tin oxide target according to claim 1, characterized in that: The mass ratio of the graphene, polyvinyl pyrrolidone, carboxymethyl cellulose and phosphoric acid solution is 1: (0.1-0.3): (0.1-0.3): (15-22).
4. The method for preparing a zinc tin oxide target according to claim 1, characterized in that: The molar concentration of the sulfuric acid solution is 1-5 mol / L; The molar concentration of the phosphoric acid solution is 1-5 mol / L.
5. The method for preparing a zinc tin oxide target according to claim 1, characterized in that: The mass ratio of the precursor, the first modifying liquid and the second modifying liquid is 1:(3-6):(0.5-2).
6. The method for preparing the zinc tin oxide target according to claim 1, characterized in that: The compression molding pressure is 45-60 MPa, and the compression molding time is 4-8 min.
7. A zinc tin oxide target, characterized in that: The method is prepared by any one of claims 1 to 6.
Citation Information
Patent Citations
Preparation method of graphene composite conductive oxide target and transparent conductive film thereof
CN103741094A
Composite film and preparation method thereof
CN116834413A