Room temperature surface acoustic wave formaldehyde sensor and its preparation method and application

A room temperature surface acoustic wave formaldehyde sensor is prepared through poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide/indium oxide composite material, which solves the problem of using formaldehyde sensors in the existing technology. The problem of harsh conditions, low sensitivity and insufficient development of composite materials has been achieved to achieve high sensitivity and rapid response to formaldehyde detection.

CN118566334BActive Publication Date: 2024-10-29HUNAN UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411044600.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-29
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

Existing formaldehyde sensors are used at high temperatures, have low sensitivity, slow response, high detection limits, and are expensive. Moreover, the gas-sensing properties of graphene and its derivatives rely on the oxidation process, which leads to structural damage and reduced gas sensing performance. There is a lack of high-performance composite material development in the surface acoustic wave gas sensor field.

Method used

Using poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide/indium oxide composite materials, a uniform solution was prepared by ultrasonic method, and combined with photolithography and evaporated aluminum processes, the lithium niobate was An interdigital transducer is prepared on the substrate to form a room temperature surface acoustic wave formaldehyde sensor.

Benefits of technology

It achieves high sensitivity, fast response and excellent repeatability to ultra-low concentration formaldehyde gas at room temperature. It is suitable for mass production, reduces the response time of the sensor, and improves the selectivity to formaldehyde.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118566334B_ABST
    Figure CN118566334B_ABST
Patent Text Reader

Abstract

The invention discloses a room temperature surface acoustic wave formaldehyde sensor and a preparation method and application thereof, belonging to the technical field of gas sensors. The room temperature surface acoustic wave formaldehyde sensor comprises a lithium niobate substrate, two parallel and spaced interdigital transducers arranged on the lithium niobate substrate, and a poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide sensitive layer coated on the lithium niobate substrate and located between the two interdigital transducers. The invention can have excellent gas-sensing performance to formaldehyde gas at room temperature, and significantly improves the sensitivity of the surface acoustic wave formaldehyde sensor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of gas sensors, and in particular relates to a room temperature surface acoustic wave formaldehyde sensor and a preparation method and application thereof. Background Art

[0002] In recent years, air pollution has become a topic of concern to most people. At present, there are many types of air pollutants that have been recognized by humans and are affecting the environment. Among them, the most common and most frequently mentioned is formaldehyde. Formaldehyde can be produced in many ways, such as exhaust gas from gasoline combustion, waste gas from power plants, and by-products from chemical plants. Excessive formaldehyde not only affects the environment, but also causes irreversible damage to the human body.

[0003] According to the principle of formaldehyde detection, the common formaldehyde sensors are mainly divided into optical, electrochemical, field effect transistor, quartz crystal microbalance, and chemical resistance sensors. However, these sensors often have serious application problems such as harsh use conditions (such as must be used at high temperatures), low sensitivity, slow response, high detection limit, and high price. In order to solve these problems and meet the needs of human health detection and wearable technology, smart sensors came into being. The emergence of surface acoustic wave technology, with its advantages of high sensitivity, low detection limit, wireless passive detection, and easy integration of photolithography process, provides solutions to these problems. There is no doubt that the development of a surface acoustic wave formaldehyde sensor with outstanding performance can meet the needs of formaldehyde gas detection.

[0004] The key to developing high-performance surface acoustic wave formaldehyde sensors is to select suitable sensing materials. As a representative of two-dimensional materials, graphene and its derivatives are undoubtedly the most widely used. However, the gas-sensing properties of graphene and its derivatives are highly dependent on the oxidation process of functional groups. Such an oxidation process will destroy the large specific surface area structure of graphene itself, which will reduce the gas sensing performance and increase the response and recovery time. In addition, graphene and its derivatives show sensitive characteristics to many gases, which is contrary to the need for gas sensors to have good gas selectivity. Therefore, people try to find new formaldehyde gas-sensitive materials. Common additives include polymers (such as PEI, PANI), nanometal materials (such as silver nanoparticles, palladium nanowires, gold nanorods), metal compounds (such as tungsten oxide, titanium dioxide, zinc sulfide, molybdenum disulfide), organic multidimensional materials (such as MOF, MXene), etc. However, a single formaldehyde gas-sensitive material often has great defects in performance. For this reason, researchers try to combine different formaldehyde gas-sensitive materials in a reasonable way, learn from each other's strengths and weaknesses, and prepare new composite materials with excellent formaldehyde sensing performance.

[0005] At present, in other categories of sensor fields, there have been several cases of combining high molecular polymers and metal compounds for high-performance formaldehyde sensing. However, in the emerging field of surface acoustic wave gas sensors, the development of such new composite materials is still too small and is in a state of urgent need for development. Summary of the invention

[0006] The present invention discloses a room temperature surface acoustic wave formaldehyde sensor and a preparation method and application thereof. The sensor can have excellent gas-sensing performance to formaldehyde gas at room temperature, and the preparation process is simple, repeatability is good, and it is suitable for mass production, thereby effectively solving at least one technical problem involved in the background technology.

[0007] To achieve the above object, the technical solution of the present invention is:

[0008] A method for preparing a room temperature surface acoustic wave formaldehyde sensor comprises the following steps:

[0009] Step 1, dissolving molybdenum disulfide powder in deionized water to form a molybdenum disulfide dispersion, and then ultrasonicating the dispersion at a certain power for a period of time to obtain a uniform molybdenum disulfide solution;

[0010] Step 2, dissolving indium oxide powder in deionized water to form an indium oxide dispersion, and then ultrasonicating the dispersion at a certain power for a period of time to obtain a uniform indium oxide solution;

[0011] Step 3, taking a poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid) solution, adding a molybdenum disulfide solution, an indium oxide solution and deionized water, and then stirring for a period of time to obtain a uniform poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide solution;

[0012] Step 4, using photolithography, aluminum evaporation and lift-off processes to prepare two interdigital transducers spaced apart on a lithium niobate substrate;

[0013] Step 5, using a drop casting method, drop the poly (3,4-ethylenedioxythiophene): poly (styrenesulfonic acid) - molybdenum disulfide / indium oxide solution onto the area between the two interdigital transducers on the lithium niobate substrate, dry it at a certain temperature for a period of time, and then stabilize it at room temperature to obtain a room temperature surface acoustic wave formaldehyde sensor based on the poly (3,4-ethylenedioxythiophene): poly (styrenesulfonic acid) - molybdenum disulfide / indium oxide composite material.

[0014] As a preferred improvement of the present invention, in step 1, 100-500 mg of molybdenum disulfide powder is dissolved in 20-100 mL of deionized water to form a molybdenum disulfide dispersion with a concentration of 5 mg / mL, and then the dispersion is ultrasonicated at a power of 200-400 W for 1-3 h at room temperature to obtain a uniform molybdenum disulfide solution.

[0015] As a preferred improvement of the present invention, in step 2, 100-500 mg of indium oxide powder is dissolved in 25-125 mL of deionized water to form an indium oxide dispersion with a concentration of 4 mg / mL, and then the dispersion is ultrasonicated at a power of 100-200 W for 2-4 hours at room temperature to obtain a uniform indium oxide solution.

[0016] As a preferred improvement of the present invention, in step 3, 10 to 50 mL of a 1.5 wt% poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid) solution is taken, 20 to 100 mL of a molybdenum disulfide solution, 25 to 125 mL of an indium oxide solution and 45 to 225 mL of deionized water are added, and then stirred for 6 to 12 hours to obtain a uniform poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid)-molybdenum disulfide / indium oxide solution.

[0017] As a preferred improvement of the present invention, the ratio of the poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid) solution, molybdenum disulfide solution, indium oxide solution and deionized water is controlled to be 2:4:5:9.

[0018] As a preferred improvement of the present invention, in step 5, after drying at 60°C for 2 hours and then stabilizing at room temperature for 24 hours, a room temperature surface acoustic wave formaldehyde sensor based on poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide composite material is obtained.

[0019] The present invention also provides a room-temperature surface acoustic wave formaldehyde sensor, which includes a lithium niobate substrate, two parallel and spaced interdigital transducers arranged on the lithium niobate substrate, and a poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide sensitive layer coated on the lithium niobate substrate and located between the two interdigital transducers.

[0020] As a preferred improvement of the present invention, the wavelength of the IDT is 16 μm, it is composed of 50-200 nm aluminum metal, the metallization rate is 0.5, the aperture is 3.2 mm, and the distance between the two IDTs is 2.4 mm.

[0021] As a preferred improvement of the present invention, the IDT includes interdigital electrodes, a reflection grid arranged outside the interdigital electrodes, and a metal electrode connected to the interdigital electrodes and used as a lead.

[0022] The present invention also provides an application of a room temperature surface acoustic wave formaldehyde sensor, which can be used to detect formaldehyde.

[0023] The beneficial effects of the present invention are as follows:

[0024] 1. The sensor prepared by the present invention can have excellent gas-sensing performance to ultra-low concentration formaldehyde gas at room temperature, including high sensitivity, fast response, and excellent repeatability, and has extremely high commercial value;

[0025] 2. The raw materials required by the present invention are all commercialized chemical materials, so the microstructure of the raw materials has good consistency;

[0026] 3. The room temperature surface acoustic wave formaldehyde sensor based on poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide composite material prepared by the present invention has a simple preparation process and good repeatability, and is suitable for mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work, among which:

[0028] Figure 1 A schematic diagram of the structure of a room temperature surface acoustic wave formaldehyde sensor provided by the present invention;

[0029] Figure 2 A repeatability curve diagram of the room temperature surface acoustic wave formaldehyde sensor of the poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide composite material provided in Example 1 to 500 ppm formaldehyde at room temperature;

[0030] Figure 3 The single-cycle response curve of the room-temperature surface acoustic wave formaldehyde sensor of the poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide composite material prepared according to Examples 1-5 to 500 ppm formaldehyde at room temperature.

[0031] In the figure: 1. lithium niobate substrate; 2. interdigital transducer; 21. interdigital electrode; 22. reflective grid; 23. metal electrode; 3. poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide sensitive layer. DETAILED DESCRIPTION

[0032] The technical solutions in the embodiments of the present invention will be described clearly and completely below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] It should be noted that all directional indications (such as up, down, left, right, front, back, etc.) in the embodiments of the present invention are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.

[0034] In addition, in the present invention, descriptions such as "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0035] In the present invention, unless otherwise clearly specified and limited, the terms "connection", "fixation", etc. should be understood in a broad sense. For example, "fixation" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0036] In addition, the technical solutions between the various embodiments of the present invention can be combined with each other, but it must be based on the fact that ordinary technicians in the field can implement it. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0037] The present invention provides a method for preparing a room temperature surface acoustic wave formaldehyde sensor, which specifically comprises the following steps:

[0038] Step 1, dissolving 100-500 mg of molybdenum disulfide powder in 20-100 mL of deionized water to form a molybdenum disulfide dispersion with a concentration of 5 mg / mL, and then ultrasonicating the dispersion at room temperature with a power of 200-400 W for 1-3 h to obtain a uniform molybdenum disulfide solution;

[0039] Step 2, dissolving 100-500 mg of indium oxide powder in 25-125 mL of deionized water to form an indium oxide dispersion with a concentration of 4 mg / mL, and then ultrasonicating the dispersion at room temperature at a power of 100-200 W for 2-4 hours to obtain a uniform indium oxide solution;

[0040] Step 3, taking 10-50 mL of a 1.5 wt% poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid) solution, adding 20-100 mL of a molybdenum disulfide solution, 25-125 mL of an indium oxide solution and 45-225 mL of deionized water, and then stirring for 6-12 hours to obtain a uniform poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid)-molybdenum disulfide / indium oxide solution;

[0041] The ratio of the added poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid) solution, molybdenum disulfide solution, indium oxide solution and deionized water is controlled to be 2:4:5:9.

[0042] Step 4, using photolithography, aluminum evaporation and lift-off processes, two interdigital transducers with a wavelength of 16 μm and a spacing of 50-200 nm aluminum metal are prepared on a 4-inch lithium niobate substrate with a thickness of 0.5 mm;

[0043] Step 5, in order to form a sensitive layer on the surface acoustic wave sensor, the poly (3,4-ethylenedioxythiophene): poly (styrenesulfonic acid) - molybdenum disulfide / indium oxide solution is dropped on the area between the two interdigital transducers on the lithium niobate substrate by a drop casting method, dried at 60 ° C for 2 hours, and then placed at room temperature for 24 hours to stabilize, thereby obtaining a room temperature surface acoustic wave formaldehyde sensor based on poly (3,4-ethylenedioxythiophene): poly (styrenesulfonic acid) - molybdenum disulfide / indium oxide composite material.

[0044] like Figure 1 As shown, the present invention also provides a room temperature surface acoustic wave formaldehyde sensor prepared by the above method, comprising a lithium niobate substrate 1, two parallel and spaced interdigital transducers 2 arranged on the lithium niobate substrate 1, and a poly (3,4-ethylenedioxythiophene): poly (styrene sulfonic acid) - molybdenum disulfide / indium oxide sensitive layer 3 coated on the lithium niobate substrate 1 and located between the two interdigital transducers 2. The interdigital transducer 2 comprises an interdigital electrode 21, a reflective grating 22 arranged outside the interdigital electrode 21, and a metal electrode 23 used for lead wires and connected to the interdigital electrode 21.

[0045] The lithium niobate substrate 1 has a diameter of 4 inches and a thickness of 0.5 mm.

[0046] Specifically, the IDT 2 has a wavelength of 16 μm, is made of 50-200 nm aluminum metal, has a metallization rate of 0.5, an aperture of 3.2 mm, and a distance between two IDTs 2 of 2.4 mm; the IDT 2 includes 50 pairs of interdigital electrodes 21 and 100 pairs of reflection gratings 22 .

[0047] The room temperature surface acoustic wave formaldehyde sensor provided by the present invention can be applied to the detection of formaldehyde gas.

[0048] The present invention successfully combines poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid), molybdenum disulfide and indium oxide. By utilizing the high conductivity of the organic matter poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid) and the inorganic semiconductor pn heterostructure formed by combining molybdenum disulfide and indium oxide, not only the sensitivity, selectivity and repeatability of the sensor to formaldehyde are greatly improved, but also the response time of the sensor to formaldehyde is greatly reduced, and the sensor is more suitable for rapid detection of formaldehyde.

[0049] The present invention is described in detail below with reference to specific embodiments 1-5.

[0050] Example 1

[0051] Embodiment 1 provides a method for preparing a room temperature surface acoustic wave formaldehyde sensor, comprising:

[0052] (1) dissolving 100 mg of molybdenum disulfide powder in 20 mL of deionized water to form a molybdenum disulfide dispersion, and then ultrasonicating the dispersion at room temperature at a power of 200 W for 1 h to obtain a uniform molybdenum disulfide solution;

[0053] (2) dissolving 100 mg of indium oxide powder in 25 mL of deionized water to form an indium oxide dispersion, and then ultrasonicating the dispersion at room temperature at a power of 100 W for 2 h to obtain a uniform indium oxide solution;

[0054] (3) Take 10 mL of a 1.5 wt% poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid) solution, add 20 mL of molybdenum disulfide solution, 25 mL of indium oxide solution and 45 mL of deionized water, and then stir for 6 hours to obtain a uniform poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid)-molybdenum disulfide / indium oxide solution;

[0055] (4) The IDT was fabricated on a 4-inch lithium niobate wafer (0.5 mm thick). Using photolithography, aluminum evaporation, and lift-off processes, an IDT with a wavelength of 16 μm and composed of 50 nm aluminum metal was fabricated on the surface of the lithium niobate wafer. The IDT contained 50 pairs of interdigital electrodes and 100 pairs of reflective gratings, with a metallization rate of 0.5 and an aperture of 3.2 mm. The area distance between adjacent double-ended IDTs was 2.4 mm.

[0056] (5) In order to form a sensitive layer on the surface acoustic wave sensor, 2.5 μL of the prepared poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide solution was dropped on the area between the two interdigital transducers by the drop casting method, dried at 60 °C for 1 h, and then placed at room temperature for 24 h to stabilize, thereby obtaining a room temperature surface acoustic wave formaldehyde sensor based on the poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide composite material.

[0057] like Figure 2 As shown in FIG. 1 , the repeatability curve of the room temperature surface acoustic wave formaldehyde sensor based on poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide composite material prepared in Example 1 at room temperature for 500 ppm formaldehyde is shown in FIG. Figure 2 It can be seen that the prepared surface acoustic wave formaldehyde sensor has almost no change in response to low concentration of formaldehyde in multiple repeated cycle tests, indicating that the sensor has good repeated response performance.

[0058] Example 2

[0059] Embodiment 2 provides a method for preparing a room temperature surface acoustic wave formaldehyde sensor, comprising:

[0060] (1) dissolving 500 mg of molybdenum disulfide powder in 100 mL of deionized water to form a molybdenum disulfide dispersion, and then ultrasonicating the dispersion at room temperature at a power of 400 W for 3 h to obtain a uniform molybdenum disulfide solution;

[0061] (2) dissolving 500 mg of indium oxide powder in 125 mL of deionized water to form an indium oxide dispersion, and then ultrasonicating the dispersion at room temperature at a power of 200 W for 4 h to obtain a uniform indium oxide solution;

[0062] (3) Take 50 mL of a 1.5 wt% poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid) solution, add 100 mL of molybdenum disulfide solution, 125 mL of indium oxide solution and 225 mL of deionized water, and then stir for 12 h to obtain a uniform poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid)-molybdenum disulfide / indium oxide solution;

[0063] (4) The IDT was fabricated on a 4-inch lithium niobate wafer (0.5 mm thick). Using photolithography, aluminum evaporation, and lift-off processes, an IDT with a wavelength of 16 μm and composed of 200 nm aluminum metal was fabricated on the surface of the lithium niobate wafer. The IDT contained 50 pairs of interdigital electrodes and 100 pairs of reflective gratings, with a metallization rate of 0.5 and an aperture of 3.2 mm. The area distance between adjacent double-ended IDTs was 2.4 mm.

[0064] (5) In order to form a sensitive layer on the surface acoustic wave sensor, 2 μL of the prepared poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide solution was dropped on the area between the two interdigital transducers by the drop casting method, dried at 60 °C for 1 h, and then placed at room temperature for 24 h to stabilize, thereby obtaining a room temperature surface acoustic wave formaldehyde sensor based on the poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide composite material.

[0065] Example 3

[0066] Embodiment 3 provides a method for preparing a room temperature surface acoustic wave formaldehyde sensor, comprising:

[0067] (1) dissolving 300 mg of molybdenum disulfide powder in 60 mL of deionized water to form a molybdenum disulfide dispersion, and then ultrasonicating the dispersion at room temperature at a power of 300 W for 2 h to obtain a uniform molybdenum disulfide solution;

[0068] (2) dissolving 300 mg of indium oxide powder in 75 mL of deionized water to form an indium oxide dispersion, and then ultrasonicating the dispersion at room temperature at a power of 200 W for 2 h to obtain a uniform indium oxide solution;

[0069] (3) Take 30 mL of a 1.5 wt% poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid) solution, add 60 mL of molybdenum disulfide solution, 75 mL of indium oxide solution and 135 mL of deionized water, and then stir for 9 hours to obtain a uniform poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid)-molybdenum disulfide / indium oxide solution;

[0070] (4) The IDT was fabricated on a 4-inch lithium niobate wafer (0.5 mm thick). Using photolithography, aluminum evaporation, and lift-off processes, an IDT with a wavelength of 16 μm and composed of 100 nm aluminum metal was fabricated on the surface of the lithium niobate wafer. The IDT contained 50 pairs of interdigital electrodes and 100 pairs of reflective gratings, with a metallization rate of 0.5 and an aperture of 3.2 mm. The area distance between adjacent double-ended IDTs was 2.4 mm.

[0071] (5) In order to form a sensitive layer on the surface acoustic wave sensor, 1.5 μL of the prepared poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide solution was dropped on the area between the two interdigital transducers by the drop casting method, dried at 60 °C for 0.75 h, and then placed at room temperature for 24 h to stabilize, thereby obtaining a room temperature surface acoustic wave formaldehyde sensor based on the poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide composite material.

[0072] Example 4

[0073] Embodiment 4 provides a method for preparing a room temperature surface acoustic wave formaldehyde sensor, comprising:

[0074] (1) dissolving 200 mg of molybdenum disulfide powder in 40 mL of deionized water to form a molybdenum disulfide dispersion, and then ultrasonicating the dispersion at room temperature at a power of 200 W for 3 h to obtain a uniform molybdenum disulfide solution;

[0075] (2) dissolving 200 mg of indium oxide powder in 50 mL of deionized water to form an indium oxide dispersion, and then ultrasonicating the dispersion at room temperature at a power of 150 W for 3 h to obtain a uniform indium oxide solution;

[0076] (3) Take 20 mL of a 1.5 wt% poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid) solution, add 40 mL of molybdenum disulfide solution, 50 mL of indium oxide solution and 90 mL of deionized water, and then stir for 8 h to obtain a uniform poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid)-molybdenum disulfide / indium oxide solution;

[0077] (4) The IDT was fabricated on a 4-inch lithium niobate wafer (0.5 mm thick). Using photolithography, aluminum evaporation, and lift-off processes, an IDT with a wavelength of 16 μm and composed of 80 nm aluminum metal was fabricated on the surface of the lithium niobate wafer. The IDT contained 50 pairs of interdigital electrodes and 100 pairs of reflective gratings, with a metallization rate of 0.5 and an aperture of 3.2 mm. The area distance between adjacent double-ended IDTs was 2.4 mm.

[0078] (5) In order to form a sensitive layer on the surface acoustic wave sensor, 1 μL of the prepared poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide solution was dropped on the area between the two interdigital transducers by the drop casting method, dried at 60 °C for 0.5 h, and then placed at room temperature for 24 h to stabilize, thereby obtaining a room temperature surface acoustic wave formaldehyde sensor based on the poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide composite material.

[0079] Example 5

[0080] Embodiment 5 provides a method for preparing a room temperature surface acoustic wave formaldehyde sensor, comprising:

[0081] (1) dissolving 400 mg of molybdenum disulfide powder in 80 mL of deionized water to form a molybdenum disulfide dispersion, and then ultrasonicating the dispersion at a power of 400 W for 1.5 h at room temperature to obtain a uniform molybdenum disulfide solution;

[0082] (2) dissolving 400 mg of indium oxide powder in 100 mL of deionized water to form an indium oxide dispersion, and then ultrasonicating the dispersion at room temperature at a power of 200 W for 3 h to obtain a uniform indium oxide solution;

[0083] (3) Take 40 mL of a 1.5 wt% poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid) solution, add 80 mL of molybdenum disulfide solution, 100 mL of indium oxide solution and 180 mL of deionized water, and then stir for 10 h to obtain a uniform poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid)-molybdenum disulfide / indium oxide solution;

[0084] (4) The IDT was fabricated on a 4-inch lithium niobate wafer (0.5 mm thick). Using photolithography, aluminum evaporation, and lift-off processes, an IDT with a wavelength of 16 μm and composed of 150 nm aluminum metal was fabricated on the surface of the lithium niobate wafer. The IDT contained 50 pairs of interdigital electrodes and 100 pairs of reflective gratings, with a metallization rate of 0.5 and an aperture of 3.2 mm. The area distance between adjacent double-ended IDTs was 2.4 mm.

[0085] (5) In order to form a sensitive layer on the surface acoustic wave sensor, 0.5 μL of the prepared poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide solution was dropped on the area between the two interdigital transducers by the drop casting method, dried at 60 °C for 0.5 h, and then placed at room temperature for 24 h to stabilize, thereby obtaining a room temperature surface acoustic wave formaldehyde sensor based on the poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide composite material.

[0086] like Figure 3 As shown in FIG. 1 , the single-cycle response curves of five room-temperature surface acoustic wave formaldehyde sensors based on poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide composite materials prepared according to Examples 1-5 to 500 ppm formaldehyde at room temperature are shown in FIG. Figure 3 It can be seen that the responses of the five surface acoustic wave formaldehyde sensors prepared according to the methods of Examples 1-5 to low concentration formaldehyde in the single cycle response test are almost the same, indicating that the sensor has good repeatability.

[0087] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation methods. The above-mentioned specific implementation methods are merely illustrative and not restrictive. Under the enlightenment of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the present invention and the claims, all of which are within the protection of the present invention.

Claims

1. A method for preparing a room temperature surface acoustic wave formaldehyde sensor, characterized in that: The following steps are involved: Step 1, dissolving molybdenum disulfide powder in deionized water to form a molybdenum disulfide dispersion, and then ultrasonicating the dispersion at a certain power for a period of time to obtain a uniform molybdenum disulfide solution; Step 2, dissolving indium oxide powder in deionized water to form an indium oxide dispersion, and then ultrasonicating the dispersion at a certain power for a period of time to obtain a uniform indium oxide solution; Step 3, taking a poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid) solution, adding a molybdenum disulfide solution, an indium oxide solution and deionized water, and then stirring for a period of time to obtain a uniform poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide solution; Step 4, using photolithography, aluminum evaporation and lift-off processes to prepare two interdigital transducers spaced apart on a lithium niobate substrate; Step 5, using a drop casting method, dropping the poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide solution onto the area between the two interdigital transducers on the lithium niobate substrate, drying at a certain temperature for a period of time, and then stabilizing at room temperature to obtain a room temperature surface acoustic wave formaldehyde sensor based on a poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide composite material; Wherein, in step 1, a molybdenum disulfide powder having a mass of 100-500 mg is dissolved in 20-100 mL of deionized water to form a molybdenum disulfide dispersion having a concentration of 5 mg / mL, and then the dispersion is ultrasonicated at a power of 200-400 W for 1-3 h at room temperature to obtain a uniform molybdenum disulfide solution; In step 2, 100-500 mg of indium oxide powder is dissolved in 25-125 mL of deionized water to form an indium oxide dispersion with a concentration of 4 mg / mL, and then the dispersion is ultrasonicated at room temperature at a power of 100-200 W for 2-4 hours to obtain a uniform indium oxide solution; In step 3, 10 to 50 mL of a 1.5 wt% poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid) solution is taken, 20 to 100 mL of a molybdenum disulfide solution, 25 to 125 mL of an indium oxide solution and 45 to 225 mL of deionized water are added, and then stirred for 6 to 12 hours to obtain a uniform poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid)-molybdenum disulfide / indium oxide solution.

2. The method for preparing a room temperature surface acoustic wave formaldehyde sensor according to claim 1, characterized in that: The volume ratio of the poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid) solution, molybdenum disulfide solution, indium oxide solution and deionized water is controlled to be 2:4:5:

9.

3. The method for preparing a room temperature surface acoustic wave formaldehyde sensor according to claim 1, characterized in that: In step 5, after drying at 60° C. for 2 h and then stabilizing at room temperature for 24 h, a room temperature surface acoustic wave formaldehyde sensor based on poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide composite material is obtained.

4. A room temperature surface acoustic wave formaldehyde sensor using the preparation method of the room temperature surface acoustic wave formaldehyde sensor according to any one of claims 1 to 3, characterized in that: The room temperature surface acoustic wave formaldehyde sensor includes a lithium niobate substrate, two parallel and spaced interdigital transducers arranged on the lithium niobate substrate, and a poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid)-molybdenum disulfide / indium oxide sensitive layer coated on the lithium niobate substrate and located between the two interdigital transducers.

5. A room temperature surface acoustic wave formaldehyde sensor according to claim 4, characterized in that: The wavelength of the IDT is 16 μm, it is made of 50-200 nm aluminum metal, the metallization rate is 0.5, the aperture is 3.2 mm, and the distance between the two IDTs is 2.4 mm.

6. A room temperature surface acoustic wave formaldehyde sensor according to claim 4, characterized in that: The interdigital transducer comprises interdigital electrodes, a reflection grid arranged outside the interdigital electrodes, and a metal electrode connected to the interdigital electrodes and used as a lead.

7. An application of the room temperature surface acoustic wave formaldehyde sensor as claimed in any one of claims 4 to 6, characterized in that: Used to detect formaldehyde.

Citation Information

Patent Citations

  • Acoustic surface wave formaldehyde gas sensor

    CN110243930A

  • Application of surface acoustic wave sensor in DMMP gas detection

    CN117969655A

  • Room-temperature surface acoustic wave formaldehyde sensor as well as preparation method and application thereof

    CN118392983A

  • Surface acoustic wave device

    JP1995131282A

  • Surface wave device and manufacturing method therefor

    JP2004228985A