A lithium ion battery negative electrode material and preparation method thereof

Through graphene-boehmite aerogel and chemical vapor deposition technology, a lithium-ion battery negative electrode material with high porosity and uniform deposition characteristics was prepared, which solved the structure caused by volume expansion of the lithium-ion battery negative electrode material during charging and discharging. The damage problem significantly improves the cycle life of the battery.

CN118579770BActive Publication Date: 2024-11-05QINGDAO TEDA CHINA RESOURCES NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411073749.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-05
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The volume expansion of the negative electrode material of existing lithium-ion batteries during charging and discharging leads to structural collapse and SEI film rupture, resulting in a decrease in battery life, and a single core-shell structure is difficult to continuously resist structural damage caused by expansion.

Method used

Graphene-Boehmite aerogel as carbon matrix is ​​used to prepare lithium-ion battery negative electrode material through hydrothermal reaction and chemical vapor deposition. Graphene aerogel provides porosity and pressure buffering, and nano-flake boehmite forms diffusion The channel is uniformly deposited with silicon particles, reducing internal stress inhomogeneity.

Benefits of technology

It effectively reduces structural damage caused by the expansion of silicon particles, uniformly deposits silicon particles, avoids structural collapse and continuous growth of SEI film, and significantly improves the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118579770B_ABST
    Figure CN118579770B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of secondary battery materials. More specifically, it relates to a negative electrode material for a lithium ion battery and a preparation method thereof. The preparation method of the present invention comprises: ultrasonically dispersing graphene oxide and water to obtain a graphene oxide aqueous solution; adding the graphene oxide aqueous solution to a hydrothermal reactor, and adding nano-flaky boehmite, hydrothermally reacting to obtain a graphene oxide-boehmite hydrogel; soaking the graphene oxide-boehmite hydrogel in ammonia water for a long time, drying it, and then heat treating it to obtain a graphene-boehmite aerogel; immersing the graphene-boehmite aerogel in a sodium hydroxide solution, ultrasonically etching it, filtering, washing and drying it to obtain a carbon matrix; using silane as a gas source, chemically vapor depositing silicon particles in the pores of the carbon matrix to obtain an aerogel deposited with silicon particles; then introducing a carbon source gas to deposit amorphous carbon on the surface of the silicon particles, and then cooling it to obtain a negative electrode material for a lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of secondary battery materials, and more specifically, relates to a negative electrode material for a lithium ion battery and a preparation method thereof. Background Art

[0002] With the rapid development of the new energy industry, lithium-ion batteries are widely used as energy storage devices, with advantages such as high energy density, safety, environmental protection, and long cycle life. Currently, more than 95% of commercial lithium-ion batteries use graphite as the negative electrode material. However, the energy density of graphite has almost reached the theoretical limit, and the effective capacity can no longer meet the growing high-performance needs of users for lithium-ion batteries.

[0003] The theoretical specific capacity of silicon is as high as 4200mAh·h / g, and silicon has a lower operating voltage, which can avoid the hidden danger of lithium deposition on the surface during charging and discharging. However, the rapid expansion of silicon in the process of charging and discharging will lead to the pulverization of active materials and the continuous rupture and repeated formation of SEI film, resulting in a decrease in battery life.

[0004] Structural design can alleviate the volume expansion of the negative electrode of lithium batteries, which is one of the key methods to improve the electrochemical performance of batteries. For example, silicon or its composite particles are used as the core body as the lithium storage material, and then a layer of carbon is coated on the surface of the silicon substrate by some chemical or mechanical means. Carbon is used as the shell or protective layer of silicon to prevent direct contact between silicon and electrolyte, promote the formation of a uniform, strong and stable SEI film, and then the initial coulomb efficiency is improved. Naturally, the conductivity can also be improved.

[0005] Although the core-shell structure can relieve stress to a certain extent, it cannot completely avoid the volume expansion of silicon-based negative electrode materials during the process of lithium insertion and extraction. Therefore, once it occurs and acts repeatedly, the carbon shell breaks when the negative electrode expands back and forth, and the material performance will rapidly decay. Summary of the invention

[0006] The technical problem to be solved by the present invention is: in the re-preparation process of existing conventional silicon-carbon negative electrode materials, although a single core-shell structure can relieve stress to a certain extent, as the negative electrode continues to expand back and forth, the structure is difficult to continuously resist the structural collapse caused by the expansion, as well as the rupture of the SEI film. The present invention provides a lithium ion battery negative electrode material and a preparation method thereof.

[0007] The purpose of the present invention is to provide a negative electrode material for a lithium ion battery.

[0008] Another object of the present invention is to provide a method for preparing a negative electrode material for a lithium ion battery.

[0009] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0010] A method for preparing a negative electrode material for a lithium ion battery, the specific preparation steps comprising:

[0011] Preparation of graphene-boehmite aerogel:

[0012] Ultrasonic dispersion of graphene oxide and water to obtain a graphene oxide aqueous solution with a concentration of 4-6 g / L;

[0013] The graphene oxide aqueous solution is added into a hydrothermal reactor, and 0.12-0.15% of the mass of the graphene oxide aqueous solution of nano-flaky boehmite is added, and then the temperature is 140-160° C. and the pressure is 6-8 MPa. The hydrothermal reaction is carried out for 24-36 hours to obtain a graphene oxide-boehmite hydrogel;

[0014] The graphene oxide-boehmite hydrogel is continuously immersed in ammonia water with a mass fraction of 6-8% for 28-36 hours, washed with water, and then freeze-dried in vacuum, and then heat-treated at a temperature of 380-400° C. for 4-8 hours under an inert gas protection state to obtain a graphene-boehmite aerogel;

[0015] Chemical Vapor Deposition:

[0016] The graphene-boehmite aerogel is immersed in a sodium hydroxide solution with a concentration of 10-15%, and after ultrasonic etching, filtered, washed and dried to obtain a carbon matrix;

[0017] Using silane as a gas source, at 900-920°C, chemical vapor deposition of silicon particles is performed in the pores of a carbon matrix to obtain an aerogel with silicon particles deposited thereon; then, a carbon source gas is introduced to deposit amorphous carbon on the surface of the silicon particles, and then the material is cooled and discharged to obtain a negative electrode material for a lithium-ion battery.

[0018] The above technical solution uses graphene aerogel as the carbon matrix for depositing silicon particles. The aerogel has a high porosity and can not only serve as a deposition site for silicon particles in the chemical vapor deposition process, but also provide space for the volume expansion of silicon particles during use. In addition, graphene is selected as the matrix material, and its lamellar structure receives the pressure generated by the expansion of granular silicon particles, which is a point-to-surface transmission process. In this way, for the same pressure, the pressure is significantly reduced, thereby significantly reducing the damage to the material structure itself. In addition, since there are gaps between the graphene oxide layers, this gap can also buffer the pressure to a certain extent, thereby further reducing the impact of pressure changes.

[0019] Although the introduction of graphene oxide aerogel can achieve the above-mentioned effects, the inventors found that when graphene oxide aerogel is used alone as the carbon matrix, the mass transfer path inside the aerogel is easily blocked. Then, during the chemical vapor deposition process, it is difficult for silane gas to effectively diffuse and penetrate into the interior of the aerogel, and the deposition of nano-silicon particles inside is also uneven, thereby causing uneven expansion stress inside the product. Based on this, the inventors introduced boehmite during the preparation of the aerogel. Before chemical vapor deposition, the boehmite was gradually dissolved by using sodium hydroxide solution under the action of ultrasonic cavitation, thereby forming a diffusion channel, so that the silicon particles can be evenly deposited inside. The reason for using flaky boehmite is that the flaky boehmite is flat, and after being dissolved by the sodium hydroxide solution, the damage to the physical stability of the aerogel structure constructed by graphene oxide is relatively small.

[0020] Furthermore, the D50 of the graphene oxide is 30-35 um, and the particle size distribution range of the graphene oxide is 10-60 um.

[0021] Furthermore, the D50 of the nano-flaky boehmite is 120-125 nm, and the particle size distribution range of the nano-flaky boehmite is 40-180 nm.

[0022] Furthermore, by regulating the D50 and particle size distribution range of graphene oxide and nano-flaky boehmite, firstly, the particle size of graphene oxide is significantly larger than that of flake boehmite. Thus, on the one hand, with the same addition amount, more flake boehmite can be present, thereby forming more diffusion pathways during the dissolution process. On the other hand, the difference in particle size between the two can also make the dispersion of boehmite in the system more uniform. Regardless of graphene oxide or boehmite, particles with a relatively narrow particle size distribution range are selected. Thus, the internal pores and pathways will not differ too much, thereby avoiding excessive non-uniformity of internal stress.

[0023] Furthermore, the graphene oxide aqueous solution also includes 8-10% of the mass of the graphene oxide in a silane coupling agent.

[0024] Furthermore, the silane coupling agent is selected from any one of silane coupling agent KH-550, silane coupling agent KH-560 and silane coupling agent KH-570.

[0025] Furthermore, the ultrasonic etching comprises: ultrasonic etching for 80-120 minutes at a temperature of 75-80°C and an ultrasonic frequency of 160-180kHz.

[0026] Furthermore, the carbon source gas is selected from any one of acetylene and ethylene.

[0027] Furthermore, in the negative electrode material of the lithium-ion battery, the silicon content accounts for 15-20% of the mass of the negative electrode material of the lithium-ion battery.

[0028] A lithium ion battery negative electrode material is prepared by the above-mentioned preparation method. Beneficial Effects

[0029] The preparation method of the present invention can effectively reduce the structural damage of the negative electrode material caused by the expansion of silicon particles during use, and the silicon particles can be uniformly deposited inside the system, so the stress distribution caused by the volume change is also more uniform. Therefore, the structural collapse or continuous growth of the SIE film caused by uneven internal stress distribution can be effectively avoided, and the cycle life of the product can be effectively improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The present invention is a flow chart of the preparation method of the embodiment. DETAILED DESCRIPTION

[0031] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0032] Unless otherwise specified, the reagents and materials used in the following examples are commercially available. Example 1

[0033] Preparation of graphene-boehmite aerogel:

[0034] After mixing graphene oxide and water, ultrasonically disperse them for 45 minutes at an ultrasonic frequency of 100 kHz to obtain a graphene oxide aqueous solution with a concentration of 4 g / L, and then add a silane coupling agent of 8% by mass of the graphene oxide to the graphene oxide aqueous solution;

[0035] The graphene oxide aqueous solution is added into a hydrothermal reactor, and 0.12% of the mass of the graphene oxide aqueous solution of nano-sheet boehmite is added, and then the hydrothermal reaction is carried out at a temperature of 140° C. and a pressure of 6 MPa for 24 hours to obtain a graphene oxide-boehmite hydrogel;

[0036] The D50 of the graphene oxide is 30 um, and the particle size distribution range of the graphene oxide is 10-60 um;

[0037] The D50 of the nano-flaky boehmite is 120 nm, and the particle size distribution range of the nano-flaky boehmite is 40-180 nm;

[0038] The silane coupling agent is selected from silane coupling agent KH-550;

[0039] The graphene oxide-boehmite hydrogel is immersed in 6% ammonia water for 28 hours, washed with water, and then freeze-dried in vacuum, and then heat-treated at 380° C. for 4 hours under inert gas protection to obtain a graphene-boehmite aerogel;

[0040] Chemical Vapor Deposition:

[0041] The graphene-boehmite aerogel is immersed in a sodium hydroxide solution with a concentration of 10%, and ultrasonically eroded for 80 minutes at a temperature of 75° C. and an ultrasonic frequency of 160 kHz, and then filtered to collect the filter cake, and the filter cake is washed with deionized water for 4 times, and then the washed filter cake is transferred to an oven and dried to a constant weight at a temperature of 90° C. to obtain a carbon matrix;

[0042] Using silane as a gas source, chemical vapor deposition of silicon particles in the pores of the carbon matrix at 900°C for 2.2 hours to obtain an aerogel with silicon particles deposited thereon; then, a carbon source gas is introduced to deposit amorphous carbon on the surface of the silicon particles, and the reaction is continued for 30 minutes, and then the material is cooled and discharged to obtain a negative electrode material for a lithium-ion battery;

[0043] By adjusting the deposition time of the silicon particles and the introduction time of the carbon source gas, the silicon content is adjusted to account for 15% of the mass of the negative electrode material of the lithium-ion battery;

[0044] The carbon source gas is selected from acetylene. Example 2

[0045] Preparation of graphene-boehmite aerogel:

[0046] After mixing graphene oxide and water, ultrasonically disperse them at an ultrasonic frequency of 100 kHz for 45 minutes to obtain a graphene oxide aqueous solution with a concentration of 5 g / L, and then add a silane coupling agent of 9% by mass of the graphene oxide to the graphene oxide aqueous solution;

[0047] The graphene oxide aqueous solution is added into a hydrothermal reactor, and 0.13% of the mass of the graphene oxide aqueous solution of nano-sheet boehmite is added, and then the hydrothermal reaction is carried out at a temperature of 150° C. and a pressure of 7 MPa for 28 hours to obtain a graphene oxide-boehmite hydrogel;

[0048] The D50 of the graphene oxide is 32 um, and the particle size distribution range of the graphene oxide is 10-60 um;

[0049] The D50 of the nano-flaky boehmite is 122 nm, and the particle size distribution range of the nano-flaky boehmite is 40-180 nm;

[0050] The silane coupling agent is selected from silane coupling agent KH-560;

[0051] The graphene oxide-boehmite hydrogel was immersed in 7% ammonia water for 32 hours, washed with water, and then freeze-dried under vacuum, and then heat-treated at 390° C. for 6 hours under inert gas protection to obtain the graphene-boehmite aerogel.

[0052] Chemical Vapor Deposition:

[0053] The graphene-boehmite aerogel is immersed in a sodium hydroxide solution with a concentration of 12%, and ultrasonically eroded for 100 minutes at a temperature of 78° C. and an ultrasonic frequency of 170 kHz, and then filtered to collect the filter cake, and the filter cake is washed with deionized water for 5 times, and then the washed filter cake is transferred to an oven and dried to constant weight at a temperature of 90° C. to obtain a carbon matrix;

[0054] Using silane as a gas source, chemical vapor deposition of silicon particles in the pores of the carbon matrix at 910°C for 2.5 hours to obtain an aerogel with silicon particles deposited thereon; then, a carbon source gas is introduced to deposit amorphous carbon on the surface of the silicon particles, and the reaction is continued for 38 minutes, and then the material is cooled and discharged to obtain a negative electrode material for a lithium-ion battery;

[0055] By adjusting the deposition time of the silicon particles and the introduction time of the carbon source gas, the silicon content is adjusted to account for 17% of the mass of the negative electrode material of the lithium-ion battery;

[0056] The carbon source gas is selected from acetylene. Example 3

[0057] Preparation of graphene-boehmite aerogel:

[0058] After mixing graphene oxide and water, ultrasonically disperse them at an ultrasonic frequency of 100 kHz for 45 minutes to obtain a graphene oxide aqueous solution with a concentration of 6 g / L, and then add a silane coupling agent in an amount of 10% by mass of the graphene oxide to the graphene oxide aqueous solution;

[0059] The graphene oxide aqueous solution is added into a hydrothermal reactor, and 0.15% of the mass of the graphene oxide aqueous solution of nano-sheet boehmite is added, and then the hydrothermal reaction is carried out for 36 hours at a temperature of 160° C. and a pressure of 8 MPa to obtain a graphene oxide-boehmite hydrogel;

[0060] The D50 of the graphene oxide is 35 um, and the particle size distribution range of the graphene oxide is 10-60 um;

[0061] The D50 of the nano-flaky boehmite is 125 nm, and the particle size distribution range of the nano-flaky boehmite is 40-180 nm;

[0062] The silane coupling agent is selected from silane coupling agent KH-570;

[0063] The graphene oxide-boehmite hydrogel was immersed in 8% ammonia water for 36 hours, washed with water, and then freeze-dried in vacuum, and then heat-treated at 400° C. for 8 hours under inert gas protection to obtain graphene-boehmite aerogel;

[0064] Chemical Vapor Deposition:

[0065] The graphene-boehmite aerogel is immersed in a sodium hydroxide solution with a concentration of 15%, and ultrasonically eroded for 120 minutes at a temperature of 80° C. and an ultrasonic frequency of 180 kHz, and then filtered to collect the filter cake, and the filter cake is washed with deionized water for 6 times, and then the washed filter cake is transferred to an oven and dried to constant weight at a temperature of 90° C. to obtain a carbon matrix;

[0066] Using silane as a gas source, chemical vapor deposition of silicon particles in the pores of the carbon matrix at 920°C for 2.6 hours to obtain an aerogel with silicon particles deposited thereon; then, a carbon source gas is introduced to deposit amorphous carbon on the surface of the silicon particles, and the reaction is continued for 45 minutes, and then the material is cooled and discharged to obtain a negative electrode material for a lithium-ion battery;

[0067] By adjusting the deposition time of the silicon particles and the introduction time of the carbon source gas, the silicon content is adjusted to account for 20% of the mass of the negative electrode material of the lithium-ion battery;

[0068] The carbon source gas is selected from ethylene. Example 4

[0069] Compared with Example 1, this embodiment is different in that:

[0070] The D50 of the graphene oxide is 20 um, and the particle size distribution range of the graphene oxide is 8-65 um; the other conditions remain unchanged. Example 5

[0071] Compared with Example 1, this embodiment is different in that:

[0072] The D50 of the graphene oxide is 40 um, and the particle size distribution range of the graphene oxide is 12-75 um; the other conditions remain unchanged.

[0073] Comparative Example 1

[0074] Compared with Example 1, this comparative example has the following differences:

[0075] The nano-spherical boehmite particles with the same mass were used to replace the nano-flaky boehmite, and the other conditions remained unchanged.

[0076] Comparative Example 2

[0077] Compared with Example 1, this comparative example has the following differences:

[0078] No nano-platelet boehmite was added, and the other conditions remained unchanged.

[0079] The performance tests were performed on the products obtained in Examples 1-5 and Comparative Examples 1-2. The specific test methods and test results are as follows:

[0080] The product obtained in the above embodiment or comparative example is used as the active material, and the active material, the conductive agent acetylene black, and the binder sodium carboxymethyl cellulose are mixed in a mass ratio of 9:0.8:0.2, poured into deionized water, adjusted into a uniform slurry, and then coated on a copper foil with a thickness of 6um, and then dried in a vacuum drying oven at a temperature of 70°C for 24 hours, and then cut into pole pieces with a diameter of 10mm;

[0081] Metallic lithium was used as the counter electrode and Celgard 2400 microporous polypropylene membrane was used as the separator;

[0082] Lithium hexafluorophosphate is dissolved in a solvent at a concentration of 1 mol / L. The solvent is prepared by mixing ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate at a volume ratio of 1:1:1, and then adding 2% by volume of fluoroethylene carbonate;

[0083] The electrodes, separators and electrolytes were assembled into CR2025 button cells in an argon glove box;

[0084] At a temperature of 25°C, a voltage of 0.01-2V, and a current density of 5A / g and 0.5A / g, constant current charge and discharge cycles were performed in a Xinwei test cabinet to test the capacity retention rate after 100 cycles; see Table 1 for details;

[0085] Table 1: Product performance test results

[0086] Capacity retention rate at 5A / g Capacity retention rate at 0.5A / g Example 1 84.2% 95.1% Example 2 84.6% 95.3% Example 3 84.7% 95.2% Example 4 82.1% 92.4% Example 5 81.5% 91.4% Comparative Example 1 78.9% 86.5% Comparative Example 2 70.4% 82.1%

[0087] It can be seen from the test results in Table 1 that, compared with the comparative example, the product obtained by the present invention has a more beneficial cycle performance. In addition, at a higher charging current density, the product obtained by the embodiment of the present invention can also obtain a relatively more beneficial cycle performance, indicating that it has better performance when charging and discharging at a large rate.

[0088] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a negative electrode material for a lithium ion battery, characterized in that: The specific preparation steps include: Preparation of graphene-boehmite aerogel: Ultrasonic dispersion of graphene oxide and water to obtain a graphene oxide aqueous solution with a concentration of 4-6 g / L; The graphene oxide aqueous solution is added into a hydrothermal reactor, and 0.12-0.15% of the mass of the graphene oxide aqueous solution of nano-flaky boehmite is added, and then the temperature is 140-160° C. and the pressure is 6-8 MPa. The hydrothermal reaction is carried out for 24-36 hours to obtain a graphene oxide-boehmite hydrogel; The graphene oxide-boehmite hydrogel is continuously immersed in ammonia water with a mass fraction of 6-8% for 28-36 hours, washed with water, and then freeze-dried in vacuum, and then heat-treated at a temperature of 380-400° C. for 4-8 hours under an inert gas protection state to obtain a graphene-boehmite aerogel; Chemical Vapor Deposition: The graphene-boehmite aerogel is immersed in a sodium hydroxide solution with a concentration of 10-15%, and after ultrasonic etching, filtered, washed and dried to obtain a carbon matrix; Using silane as a gas source, at 900-920°C, chemical vapor deposition of silicon particles is performed in the pores of a carbon matrix to obtain an aerogel with silicon particles deposited thereon; then, a carbon source gas is introduced to deposit amorphous carbon on the surface of the silicon particles, and then the material is cooled and discharged to obtain a negative electrode material for a lithium-ion battery.

2. The method for preparing a negative electrode material for a lithium ion battery according to claim 1, characterized in that: The D50 of the graphene oxide is 30-35 um, and the particle size distribution range of the graphene oxide is 10-60 um.

3. The method for preparing a negative electrode material for a lithium ion battery according to claim 2, characterized in that: The D50 of the nano-flaky boehmite is 120-125 nm, and the particle size distribution range of the nano-flaky boehmite is 40-180 nm.

4. The method for preparing a negative electrode material for a lithium ion battery according to claim 3, characterized in that: The graphene oxide aqueous solution also includes 8-10% of the mass of the graphene oxide in a silane coupling agent.

5. The method for preparing a negative electrode material for a lithium ion battery according to claim 4, characterized in that: The silane coupling agent is selected from any one of silane coupling agent KH-550, silane coupling agent KH-560 and silane coupling agent KH-570.

6. The method for preparing a negative electrode material for a lithium ion battery according to claim 1, characterized in that: The ultrasonic etching comprises: ultrasonic etching for 80-120 minutes at a temperature of 75-80° C. and an ultrasonic frequency of 160-180 kHz.

7. The method for preparing a negative electrode material for a lithium ion battery according to claim 1, characterized in that: The carbon source gas is selected from any one of acetylene and ethylene.

8. The method for preparing a negative electrode material for a lithium ion battery according to claim 1, characterized in that: In the negative electrode material of the lithium-ion battery, the silicon content accounts for 15-20% of the mass of the negative electrode material of the lithium-ion battery.

9. A negative electrode material for a lithium ion battery, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 8.