A kind of comfortable biological crystal powder composite filling foam material for automobile seats and preparation method thereof
By using components such as polyether polyols, polymer polyols, biocrystal powders and magnesium hydroxide-silica composite particles in car seat foam materials, combined with vinyl trimethoxysilane and graft coupling agents, It solves the problem that the existing car seat cushions lack flame retardant performance, realizes the flame retardant, comfort and health benefits of the material, and significantly improves the flame retardant effect.
Patent Information
- Application Number
- CN202411064345.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-05
AI Technical Summary
The existing automotive seat cushion polyurethane foam lacks flame retardant properties and cannot have both flame retardant, ride comfort and human health benefits.
Using polyether polyols, polymer polyols, toluene diisocyanate, bio-crystal powder and composite flame retardant components, the car seat comfort bio-crystal powder composite fill foam material is prepared through the foaming process, and magnesium hydroxide-dioxide The synergistic effect of silicon oxide composite particles and vinyl trimethoxysilane enhances flame retardant properties and improves the uniformity of the material through graft coupling agent modification treatment.
The material has good flame retardant properties, comfort and health benefits, which can reduce muscle tension, slow down heartbeat, relax breathing, increase oxygen levels and improve sleep quality, and at the same time, it evenly distributes composite particles in polyurethane foam, significantly improving the flame retardant effect.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of foam materials, and in particular to a comfortable biological crystal powder composite filling foam material for automobile seats and a preparation method thereof. Background Art
[0002] With the continuous development of the automobile industry and people's constant pursuit of improving automobile quality, the requirements for automobile parts materials are also increasing. For automobile seat cushions, due to the consideration of vehicle driving economy and the safety and comfort of drivers and passengers, many requirements are put forward for soft polyurethane foam materials as raw materials of seat cushions.
[0003] Chinese patent publication number CN106496492 discloses a fully water polyurethane car seat foam molding process, wherein polyether polyol, silicone oil foam stabilizer, amine catalyst, tin catalyst and distilled water are mixed evenly as component A; toluene diisocyanate is used as component B, and during foaming, the mold temperature is adjusted to 60°C-65°C, and components A and B are mixed and stirred for 5-10s, and then immediately poured into a reactor to allow free foaming, and demolded after the foam is fully matured. Based on 100 parts by weight of polyether polyol, it contains 40-45 parts by weight of toluene diisocyanate, 0.40-0.45 parts by weight of amine catalyst, 0.20-0.25 parts by weight of tin catalyst, 1-1.5 parts by weight of silicone oil foam stabilizer, and 3-3.5 parts by weight of water. The invention greatly improves the physical properties of the obtained car seat by improving and optimizing the formula.
[0004] Chinese patent publication number CN112480366 discloses a low-odor polyurethane car seat cushion and a preparation method thereof. The seat cushion is formed by mixing and foaming component A and component B. Component A includes polyether polyol A, polyether polyol B, water, foam stabilizer, and delayed amine catalyst, and component B includes modified isocyanate.
[0005] The polyurethane car seat cushion material prepared in the above technical solution does not have flame retardant properties. With the improvement of people's living standards, it is urgent to develop a car seat cushion foam material that is flame retardant, comfortable to ride and beneficial to human health. Summary of the invention
[0006] In order to overcome the above existing technical problems, the present invention provides a comfortable biological crystal powder composite filling foam material for automobile seats and a preparation method thereof. The automobile seat cushion foam material of the present invention has good flame retardant properties, comfortable riding, and the functions of relieving pressure and promoting relaxation.
[0007] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0008] A comfortable biological crystal powder composite filling foam material for automobile seats, comprising the following components in parts by weight:
[0009] 50-60 parts of polyether polyol, 20-30 parts of polymer polyol, 30-40 parts of toluene diisocyanate, 15-20 parts of biological crystal powder, 5-10 parts of composite flame retardant, 0.5-1 parts of triethanolamine, 3-6 parts of water, and 1-3 parts of silicone oil.
[0010] The present invention uses polyether polyol, polymer polyol and toluene diisocyanate as reaction monomers, triethanolamine as a catalyst, water as a foaming agent, and silicone oil as a foam stabilizer to prepare a foam polyurethane material. Biocrystal powder can produce a unique and stable frequency, can enhance the human immune system, promote the rapid discharge of body toxins and increase oxygen levels. Since this special frequency is at the same vibration frequency as humans, it has the functions of reducing muscle tension, slowing down the heartbeat, relaxing breathing, increasing body oxygen content, and releasing pressure to improve sleep. The present invention improves the health level of the human body by adding biocrystal powder to the foam polyurethane material. In addition, foam polyurethane is a flammable material. By adding a composite flame retardant to the foam polyurethane material, the foam polyurethane material is given excellent flame retardant properties.
[0011] Preferably, the biocrystal powder is mixed with the following substances:
[0012] Orange crystal calcite powder, bloodstone powder, gypsum powder, fluorite powder, white crystal powder, citrine powder, amethyst powder, red jasper powder, rose crystal powder, aventurine powder, serpentine powder.
[0013] Preferably, the preparation method of the composite flame retardant comprises the following steps:
[0014] S1, mixing anhydrous ethanol and water to form a mixed solution, adding tetraethyl orthosilicate to the mixed solution, dropping an ammonia solution to adjust the pH of the solution to neutral, heating and stirring to be uniform, aging, and setting aside;
[0015] S2, adding magnesium hydroxide powder to the above solution, stirring evenly to form a suspension, adding concentrated ammonia water dropwise to the suspension, letting it stand, filtering and drying to obtain an intermediate product;
[0016] S3, calcining the intermediate product in a muffle furnace to obtain magnesium hydroxide-silicon dioxide composite particles;
[0017] S4, adding vinyl trimethoxysilane to an anhydrous ethanol solution, stirring to obtain an alcoholysis solution, adding magnesium hydroxide-silicon dioxide composite particles to the alcoholysis solution, dropping ammonia water to adjust the pH to 10-11, keeping the temperature for reaction, filtering, washing, and drying to obtain a composite flame retardant.
[0018] The present invention uses magnesium hydroxide and silicon dioxide as flame retardants for foam polyurethane materials. Magnesium hydroxide will undergo a decomposition reaction when heated. This process is endothermic and can absorb heat from the surface of the burning object, thereby reducing the temperature and playing a flame retardant role. In addition, magnesium hydroxide will release water vapor when it decomposes. The water vapor forms a steam curtain in the air, which can dilute the combustible gas and reduce the oxygen concentration, thereby inhibiting the combustion reaction. Silicon dioxide increases the refractory deposits on the surface of the carbon layer when the polyurethane foam material burns, reduces the contact area between the polyurethane foam and oxygen, and thus plays a flame retardant role. The synergistic effect of magnesium hydroxide and silicon dioxide can play a good flame retardant role on polyurethane foam.
[0019] However, silicon dioxide and magnesium hydroxide are not evenly dispersed in polyurethane foam, and the two cannot be evenly distributed in the polyurethane foam (more magnesium hydroxide exists in one area of the polyurethane, and more silicon dioxide exists in another area). The present invention combines nano-silicon dioxide on the surface of magnesium hydroxide particles to prepare magnesium hydroxide-silicon dioxide composite particles, so that silicon dioxide and magnesium hydroxide are evenly distributed in the polyurethane foam, which has a better flame retardant effect.
[0020] During the experiment, the study found that: during the preparation of polyurethane foam, magnesium hydroxide-silicon dioxide composite particles are doped into polyurethane foam, and a large amount of biological crystal powder in the components is combined and coated on the surface of magnesium hydroxide-silicon dioxide composite particles, which has a great impact on the flame retardant properties of polyurethane foam. This may be because the hydroxyl groups on the surface of magnesium hydroxide-silicon dioxide composite particles and the hydroxyl groups on the surface of biological crystal powder have strong hydrogen bonding forces, so that the biological crystal powder is coated on the surface of magnesium hydroxide-silicon dioxide composite particles. In order to solve this problem, the present invention further modifies the magnesium hydroxide-silicon dioxide composite particles, grafts vinyl silane coupling agents on the magnesium hydroxide-silicon dioxide composite particles, and the silane coupling agent consumes the hydroxyl groups on the surface of magnesium hydroxide-silicon dioxide composite particles during the grafting process, reducing the hydrogen bonding forces between magnesium hydroxide-silicon dioxide composite particles and biological crystal powder, thereby solving the problem of the surface of magnesium hydroxide-silicon dioxide composite particles binding and coating biological crystal powder, and improving the flame retardant properties of polyurethane foam.
[0021] Preferably, in step S1, the heating temperature is 40-50°C.
[0022] Preferably, in step S2, the mass ratio of magnesium hydroxide to tetraethyl orthosilicate is 1:0.2-0.5.
[0023] Preferably, in step S3, the calcination temperature is 280-300°C.
[0024] Preferably, step S4 is carried out under the following reaction conditions:
[0025] The reaction temperature was 50°C and the reaction time was 2h;
[0026] The mass ratio of the magnesium hydroxide-silicon dioxide composite particles to vinyltrimethoxysilane is ≤1:0.3.
[0027] The present invention controls the mass ratio of the magnesium hydroxide-silicon dioxide composite particles to vinyl trimethoxysilane to be ≤1:0.3. When the mass ratio is greater than 1:0.3, a certain amount of hydroxyl groups still remain on the surface of the magnesium hydroxide-silicon dioxide composite particles. Under the action of hydrogen bonds, the natural spar powder will still be combined with the surface of the magnesium hydroxide-silicon dioxide composite particles. Therefore, the present invention controls the mass ratio of the magnesium hydroxide-silicon dioxide composite particles to vinyl trimethoxysilane to be ≤1:0.3.
[0028] The preparation method of the comfortable biological crystal powder composite filling foam material for automobile seats comprises the following steps:
[0029] Heat and stir polyether polyol, polymer polyol, biocrystal powder, composite flame retardant, triethanolamine, water and silicone oil to mix evenly, then add toluene diisocyanate, continue to stir and mix evenly, and then inject into a mold for foaming to obtain a comfortable biocrystal powder composite filling foam material for car seats.
[0030] The present invention has the following beneficial effects:
[0031] 1) Biocrystal powder can produce a unique and stable frequency. Since this special frequency is at the same vibration frequency as humans, it has the functions of reducing muscle tension, slowing down heartbeat, relaxing breathing, increasing body oxygen content, releasing pressure and improving sleep. The present invention improves human health by adding biocrystal powder to foamed polyurethane materials;
[0032] 2) The synergistic effect of magnesium hydroxide and silicon dioxide can provide good flame retardant effect on polyurethane foam;
[0033] 3) By combining nano-silicon dioxide on the surface of magnesium hydroxide particles, magnesium hydroxide-silicon dioxide composite particles are prepared, so that silicon dioxide and magnesium hydroxide are evenly distributed in the polyurethane foam, achieving a better flame retardant effect;
[0034] 4) Vinyl silane coupling agent is grafted onto magnesium hydroxide-silicon dioxide composite particles. During the grafting process, the silane coupling agent consumes hydroxyl groups on the surface of the magnesium hydroxide-silicon dioxide composite particles, reducing the hydrogen bonding force between the magnesium hydroxide-silicon dioxide composite particles and the biological crystal powder, thereby solving the problem of the magnesium hydroxide-silicon dioxide composite particle surface binding and coating biological crystal powder, and improving the flame retardant properties of polyurethane foam. DETAILED DESCRIPTION
[0035] The present invention is further described in detail below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.
[0036] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.
[0037] The polyether polyol used in the examples of the present invention is F3135 (hydroxyl value 35 mgKOH / g), produced by Wanhua Chemical Group Co., Ltd. The polymer polyol is LP-H45 (hydroxyl value 28 mgKOH / g), produced by Shandong Longhua New Materials Co., Ltd.
[0038] Example 1
[0039] A comfortable biological crystal powder composite filling foam material for automobile seats, comprising the following components in parts by weight:
[0040]
[0041] The above-mentioned biological crystal powder is mixed by the following substances of equal mass:
[0042] Orange crystal calcite powder, bloodstone powder, gypsum powder, fluorite powder, white crystal powder, citrine powder, amethyst powder, red jasper powder, rose crystal powder, aventurine powder, serpentine powder.
[0043] The preparation of the composite flame retardant comprises the following steps:
[0044] S1, 80 mL of anhydrous ethanol and 30 mL of water were mixed to form a mixed solution, 15 mL of tetraethyl orthosilicate was added to the mixed solution, and an ammonia solution was added dropwise to adjust the pH of the solution to neutral, heated to 45° C., stirred evenly, aged for 2 h, and set aside;
[0045] S2, adding magnesium hydroxide powder to the above solution, the mass ratio of magnesium hydroxide to tetraethyl orthosilicate is 1:0.45, stirring evenly to form a suspension, adding 2 mL of concentrated ammonia water with a mass concentration of 15% to the suspension, letting it stand for 5 hours, filtering and drying to obtain an intermediate product;
[0046] S3, placing the intermediate product in a muffle furnace and calcining it at 300° C. for 5 h to obtain magnesium hydroxide-silicon dioxide composite particles;
[0047] S4, adding 2 g of vinyltrimethoxysilane to 300 mL of anhydrous ethanol solution, stirring to obtain an alcoholysis solution, adding magnesium hydroxide-silicon dioxide composite particles to the alcoholysis solution, the mass ratio of magnesium hydroxide-silicon dioxide composite particles to vinyltrimethoxysilane is 1:0.7, adding ammonia water dropwise to adjust the pH to 11, keeping the reaction at 50°C for 2 hours, filtering, washing and drying to obtain a composite flame retardant.
[0048] A method for preparing a comfortable biological crystal powder composite filling foam material for automobile seats, comprising the following steps:
[0049] Heat and stir polyether polyol, polymer polyol, biocrystal powder, composite flame retardant, triethanolamine, water and silicone oil to mix evenly, then add toluene diisocyanate, continue to stir and mix evenly, pre-adjust the mold temperature to 50°C, inject the above mixture into the mold for foaming for 100s, and obtain a comfortable biocrystal powder composite filling foam material for car seats.
[0050] Example 2
[0051] A comfortable biological crystal powder composite filling foam material for automobile seats, comprising the following components in parts by weight:
[0052]
[0053] The above-mentioned biological crystal powder is mixed by the following substances of equal mass:
[0054] Orange crystal calcite powder, bloodstone powder, gypsum powder, fluorite powder, white crystal powder, citrine powder, amethyst powder, red jasper powder, rose crystal powder, aventurine powder, serpentine powder.
[0055] The preparation of the composite flame retardant comprises the following steps:
[0056] S1, 80 mL of anhydrous ethanol and 30 mL of water were mixed to form a mixed solution, 15 mL of ethyl orthosilicate was added to the mixed solution, and an ammonia solution was added dropwise to adjust the pH of the solution to neutral, heated to 40° C., stirred evenly, aged for 2 h, and set aside;
[0057] S2, adding magnesium hydroxide powder to the above solution, the mass ratio of magnesium hydroxide to tetraethyl orthosilicate is 1:0.25, stirring evenly to form a suspension, adding 2 mL of concentrated ammonia water with a mass concentration of 15% to the suspension, letting it stand for 5 hours, filtering and drying to obtain an intermediate product;
[0058] S3, placing the intermediate product in a muffle furnace and calcining it at 300° C. for 5 h to obtain magnesium hydroxide-silicon dioxide composite particles;
[0059] S4, adding 2 g of vinyltrimethoxysilane to 300 mL of anhydrous ethanol solution, stirring to obtain an alcoholysis solution, adding magnesium hydroxide-silicon dioxide composite particles to the alcoholysis solution, the mass ratio of magnesium hydroxide-silicon dioxide composite particles to vinyltrimethoxysilane is 1:0.4, adding ammonia water dropwise to adjust the pH to 10, keeping the reaction at 50°C for 2 hours, filtering, washing and drying to obtain a composite flame retardant.
[0060] A method for preparing a comfortable biological crystal powder composite filling foam material for automobile seats, comprising the following steps:
[0061] Heat and stir polyether polyol, polymer polyol, biocrystal powder, composite flame retardant, triethanolamine, water and silicone oil to mix evenly, then add toluene diisocyanate, continue to stir and mix evenly, pre-adjust the mold temperature to 50°C, inject the above mixture into the mold for foaming for 100s, and obtain a comfortable biocrystal powder composite filling foam material for car seats.
[0062] Example 3
[0063] A comfortable biological crystal powder composite filling foam material for automobile seats, comprising the following components in parts by weight:
[0064]
[0065] The above-mentioned biological crystal powder is mixed by the following substances of equal mass:
[0066] Orange crystal calcite powder, bloodstone powder, gypsum powder, fluorite powder, white crystal powder, citrine powder, amethyst powder, red jasper powder, rose crystal powder, aventurine powder, serpentine powder.
[0067] The preparation of the composite flame retardant comprises the following steps:
[0068] S1, 80 mL of anhydrous ethanol and 30 mL of water were mixed to form a mixed solution, 15 mL of tetraethyl orthosilicate was added to the mixed solution, and an ammonia solution was added dropwise to adjust the pH of the solution to neutral, heated to 45° C., stirred evenly, aged for 2 h, and set aside;
[0069] S2, adding magnesium hydroxide powder to the above solution, the mass ratio of magnesium hydroxide to tetraethyl orthosilicate is 1:0.3, stirring evenly to form a suspension, adding 2 mL of concentrated ammonia water with a mass concentration of 15% to the suspension, letting it stand for 5 hours, filtering and drying to obtain an intermediate product;
[0070] S3, placing the intermediate product in a muffle furnace and calcining it at 290° C. for 5 h to obtain magnesium hydroxide-silicon dioxide composite particles;
[0071] S4, adding 2 g of vinyltrimethoxysilane to 300 mL of anhydrous ethanol solution, stirring to obtain an alcoholysis solution, adding magnesium hydroxide-silicon dioxide composite particles to the alcoholysis solution, the mass ratio of magnesium hydroxide-silicon dioxide composite particles to vinyltrimethoxysilane is 1:0.6, adding ammonia water dropwise to adjust the pH to 10, keeping the reaction at 50°C for 2 hours, filtering, washing and drying to obtain a composite flame retardant.
[0072] A method for preparing a comfortable biological crystal powder composite filling foam material for automobile seats, comprising the following steps:
[0073] Heat and stir polyether polyol, polymer polyol, biocrystal powder, composite flame retardant, triethanolamine, water and silicone oil to mix evenly, then add toluene diisocyanate, continue to stir and mix evenly, pre-adjust the mold temperature to 50°C, inject the above mixture into the mold for foaming for 100s, and obtain a comfortable biocrystal powder composite filling foam material for car seats.
[0074] Example 4
[0075] A comfortable biological crystal powder composite filling foam material for automobile seats, comprising the following components in parts by weight:
[0076]
[0077] The above-mentioned biological crystal powder is mixed by the following substances of equal mass:
[0078] Orange crystal calcite powder, bloodstone powder, gypsum powder, fluorite powder, white crystal powder, citrine powder, amethyst powder, red jasper powder, rose crystal powder, aventurine powder, serpentine powder.
[0079] The preparation of the composite flame retardant comprises the following steps:
[0080] S1, 80 mL of anhydrous ethanol and 30 mL of water were mixed to form a mixed solution, 15 mL of tetraethyl orthosilicate was added to the mixed solution, and an ammonia solution was added dropwise to adjust the pH of the solution to neutral, heated to 50° C., stirred evenly, aged for 2 h, and set aside;
[0081] S2, adding magnesium hydroxide powder to the above solution, the mass ratio of magnesium hydroxide to tetraethyl orthosilicate is 1:0.5, stirring evenly to form a suspension, adding 2 mL of concentrated ammonia water with a mass concentration of 15% to the suspension, standing for 5 hours, filtering and drying to obtain an intermediate product;
[0082] S3, placing the intermediate product in a muffle furnace and calcining it at 300° C. for 5 h to obtain magnesium hydroxide-silicon dioxide composite particles;
[0083] S4, adding 2 g of vinyltrimethoxysilane to 300 mL of anhydrous ethanol solution, stirring to obtain an alcoholysis solution, adding magnesium hydroxide-silicon dioxide composite particles to the alcoholysis solution, the mass ratio of magnesium hydroxide-silicon dioxide composite particles to vinyltrimethoxysilane is 1:0.9, adding ammonia water dropwise to adjust the pH to 11, keeping the reaction at 50°C for 2 hours, filtering, washing and drying to obtain a composite flame retardant.
[0084] A method for preparing a comfortable biological crystal powder composite filling foam material for automobile seats, comprising the following steps:
[0085] Heat and stir polyether polyol, polymer polyol, biocrystal powder, composite flame retardant, triethanolamine, water and silicone oil to mix evenly, then add toluene diisocyanate, continue to stir and mix evenly, pre-adjust the mold temperature to 50°C, inject the above mixture into the mold for foaming for 100s, and obtain a comfortable biocrystal powder composite filling foam material for car seats.
[0086] Example 5
[0087] A comfortable biological crystal powder composite filling foam material for automobile seats, comprising the following components in parts by weight:
[0088]
[0089] The above-mentioned biological crystal powder is mixed by the following substances of equal mass:
[0090] Orange crystal calcite powder, bloodstone powder, gypsum powder, fluorite powder, white crystal powder, citrine powder, amethyst powder, red jasper powder, rose crystal powder, aventurine powder, serpentine powder.
[0091] The preparation of the composite flame retardant comprises the following steps:
[0092] S1, 80 mL of anhydrous ethanol and 30 mL of water were mixed to form a mixed solution, 15 mL of ethyl orthosilicate was added to the mixed solution, and an ammonia solution was added dropwise to adjust the pH of the solution to neutral, heated to 40° C., stirred evenly, aged for 2 h, and set aside;
[0093] S2, adding magnesium hydroxide powder to the above solution, the mass ratio of magnesium hydroxide to tetraethyl orthosilicate is 1:0.2, stirring evenly to form a suspension, adding 2 mL of concentrated ammonia water with a mass concentration of 15% to the suspension, letting it stand for 5 hours, filtering and drying to obtain an intermediate product;
[0094] S3, placing the intermediate product in a muffle furnace and calcining it at 280° C. for 5 h to obtain magnesium hydroxide-silicon dioxide composite particles;
[0095] S4, adding 2 g of vinyltrimethoxysilane to 300 mL of anhydrous ethanol solution, stirring to obtain an alcoholysis solution, adding magnesium hydroxide-silicon dioxide composite particles to the alcoholysis solution, the mass ratio of magnesium hydroxide-silicon dioxide composite particles to vinyltrimethoxysilane is 1:0.3, adding ammonia water dropwise to adjust the pH to 10, keeping the reaction at 50°C for 2 hours, filtering, washing and drying to obtain a composite flame retardant.
[0096] A method for preparing a comfortable biological crystal powder composite filling foam material for automobile seats, comprising the following steps:
[0097] Heat and stir polyether polyol, polymer polyol, biocrystal powder, composite flame retardant, triethanolamine, water and silicone oil to mix evenly, then add toluene diisocyanate, continue to stir and mix evenly, pre-adjust the mold temperature to 50°C, inject the above mixture into the mold for foaming for 100s, and obtain a comfortable biocrystal powder composite filling foam material for car seats.
[0098] Comparative Example 1
[0099] The difference between Comparative Example 1 and Example 1 is:
[0100] The composite flame retardant was replaced with an equal mass of magnesium hydroxide.
[0101] The remaining steps are the same as those in Example 1.
[0102] Comparative Example 2
[0103] The difference between Comparative Example 2 and Example 1 is:
[0104] The composite flame retardant is replaced with an equal mass of nano-silicon dioxide.
[0105] The remaining steps are the same as those in Example 1.
[0106] Comparative Example 3
[0107] The difference between Comparative Example 3 and Example 1 is that:
[0108] Replace the composite flame retardant with equal mass of nano-silicon dioxide and magnesium hydroxide.
[0109] Nano-dioxide has the same mass as magnesium hydroxide.
[0110] The remaining steps are the same as those in Example 1.
[0111] Comparative Example 4
[0112] The difference between Comparative Example 4 and Example 5 is:
[0113] The S4 step is omitted in the preparation process of the composite flame retardant.
[0114] The remaining steps are the same as those in Example 5.
[0115] Comparative Example 5
[0116] The difference between Comparative Example 4 and Example 5 is:
[0117] In the composite flame retardant preparation process S4:
[0118] The mass ratio of magnesium hydroxide-silicon dioxide composite particles to vinyl trimethoxysilane is 1:0.2
[0119] The remaining steps are the same as those in Example 5.
[0120] Comparative Example 6
[0121] The difference between Comparative Example 6 and Example 1 is:
[0122] No biological crystal powder is added to the foam material components.
[0123] Performance Testing
[0124] 1. Flame retardant performance test: According to GB / T8333-1987-2008 "Test Method for Combustion Performance of Foam Plastics", the flame retardant performance of polyurethane foam was tested. The higher the oxygen index in the test results, the better the flame retardant performance of the sponge, and vice versa, the worse the flame retardant performance of the sponge. The test results are shown in Table 1:
[0125] Table 1
[0126]
[0127] 2. Foam rebound rate test: The foam rebound rate was tested using the method specified in GB / T10807-2006. The test results are shown in Table 2.
[0128] Table 2
[0129]
[0130] 3. Far infrared release performance test. The far infrared release performance of the foam was tested using the GB / T30127-2013 method. The test results are shown in Table 3:
[0131] Table 3
[0132]
[0133] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. A comfortable biological crystal powder composite filling foam material for car seats, characterized in that: It comprises the following components by weight: 50-60 parts of polyether polyol, 20-30 parts of polymer polyol, 30-40 parts of toluene diisocyanate, 15-20 parts of biological crystal powder, 5-10 parts of composite flame retardant, 0.5-1 parts of triethanolamine, 3-6 parts of water, 1-3 parts of silicone oil; The biological crystal powder is made by mixing the following substances in equal quantities: Orange crystal calcite powder, bloodstone powder, gypsum powder, fluorite powder, white crystal powder, citrine powder, amethyst powder, red jasper powder, rose crystal powder, aventurine powder, serpentine powder; The preparation method of the composite flame retardant comprises the following steps: S1, mixing anhydrous ethanol and water to form a mixed solution, adding tetraethyl orthosilicate to the mixed solution, dropping an ammonia solution to adjust the pH of the solution to neutral, heating and stirring to be uniform, aging, and setting aside; S2, adding magnesium hydroxide powder to the above solution, stirring evenly to form a suspension, adding concentrated ammonia water dropwise to the suspension, letting it stand, filtering and drying to obtain an intermediate product; S3, calcining the intermediate product in a muffle furnace to obtain magnesium hydroxide-silicon dioxide composite particles; S4, adding vinyl trimethoxy silane to an anhydrous ethanol solution, stirring to obtain an alcoholysis solution, adding magnesium hydroxide-silicon dioxide composite particles to the alcoholysis solution, wherein the mass ratio of the magnesium hydroxide-silicon dioxide composite particles to vinyl trimethoxy silane is ≤1:0.3, dripping ammonia water to adjust the pH to 10-11, keeping the reaction at 50°C for 2h, filtering, washing and drying to obtain a composite flame retardant.
2. The comfortable biological crystal powder composite filling foam material for automobile seats according to claim 1, characterized in that: In the step S1, the heating temperature is 40-50°C.
3. The comfortable biological crystal powder composite filling foam material for automobile seats according to claim 1, characterized in that: In the step S2, the mass ratio of magnesium hydroxide to tetraethyl orthosilicate is 1:0.2-0.
5.
4. The comfortable biological crystal powder composite filling foam material for automobile seats according to claim 1, characterized in that: In the step S3, the calcination temperature is 280-300°C.
5. A method for preparing the comfortable biological crystal powder composite filling foam material for automobile seats as claimed in any one of claims 1 to 4, characterized in that: The following steps are involved: Heat and stir polyether polyol, polymer polyol, biocrystal powder, composite flame retardant, triethanolamine, water and silicone oil to mix evenly, then add toluene diisocyanate, continue to stir and mix evenly, and then inject into a mold for foaming to obtain a comfortable biocrystal powder composite filling foam material for car seats.