A kind of underwater ceramic coating and preparation method thereof
By combining modified graphene and anti-corrosion monomers with polysiloxane resin in underwater ceramic coatings, the problem of insufficient water resistance and corrosion resistance of traditional underwater coatings is solved, and long-term use and corrosion resistance in underwater environments are achieved. High wear resistance.
Patent Information
- Application Number
- CN202411060532.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-08-05
AI Technical Summary
Traditional underwater coatings have poor water resistance, corrosion resistance and wear resistance in water parks, aquariums, hot springs and other places, which makes the waterproof coating easy to fall off and corrode. The construction is complex, the maintenance cost is high, and the service life is short.
Using a ceramic coating for underwater use, modified graphene and anti-corrosion monomers are combined with polysiloxane resin to form an anti-corrosion emulsion, which is stirred and reacted in an underwater environment to form an anti-corrosion emulsion with excellent water resistance and corrosion resistance. coating.
The water resistance, corrosion resistance and wear resistance of the coating are significantly improved, allowing the coating to remain intact for a long time in harsh underwater environments and not easy to fall off or fade, extending the service life.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of coatings, and in particular to underwater ceramic coating and a preparation method thereof. Background Art
[0002] Traditional water-related places such as water parks, oceanariums, hot springs, bathrooms, etc., the underwater parts are mostly decorated and protected with ceramic tile veneers or waterproof coatings. Ceramic tile veneers are prone to cracking and falling off due to water penetration, temperature changes, and erosion by corrosive media during long-term use, affecting the appearance and safety. The use of waterproof coatings can greatly improve the appearance and safety. However, traditional underwater coatings often have the disadvantages of poor water resistance, corrosion resistance, and wear resistance, resulting in the formation of waterproof coatings that are easy to fall off, easy to corrode, and easy to wear and break, resulting in the need for repeated application of waterproof coatings, complex construction, high maintenance costs, and short service life. Therefore, it is particularly important to develop a ceramic coating for underwater use and a preparation method thereof, especially for the aesthetics and durability of underwater facilities in water parks, oceanariums, hot springs, bathrooms, etc. Summary of the invention
[0003] In order to overcome the above-mentioned technical problems, the purpose of the present invention is to provide an underwater ceramic coating and a preparation method thereof, which solves the shortcomings of traditional underwater coatings, such as poor water resistance, corrosion resistance and wear resistance, which leads to the need for repeated application of waterproof coatings, complex construction, high maintenance costs and short service life.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A ceramic coating for underwater use, comprising a component A and a component B, wherein the mass ratio of the component A to the component B is 4:1;
[0006] Wherein, component A comprises the following components in parts by weight:
[0007] 40-50 parts of mixed resin monomer, 55-65 parts of xylene, 22-30 parts of trimethylolpropane triacrylate, 2-6 parts of azobisisobutyronitrile, 2.5-8.5 parts of modified graphene, 3-6 parts of sodium silicate, 2.2-4.4 parts of boron nitride, 1.3-2.5 parts of silicon carbide, 3-7 parts of titanium dioxide, 11-19 parts of cobalt blue pigment, 2-4 parts of ultraviolet absorber, 2-4 parts of antioxidant, 3-7 parts of dispersant and 0.8-1.6 parts of defoaming agent;
[0008] Wherein, the modified graphene is prepared by the following steps:
[0009] Step a1: adding graphite powder and sodium nitrate to a three-necked flask equipped with a stirrer and a thermometer, stirring the reaction for 5-15 minutes at a temperature of -5-5°C and a stirring rate of 300-400r / min, then adding concentrated sulfuric acid and continuing to stir the reaction for 15-20 minutes, then adding potassium permanganate and continuing to stir the reaction for 15-20 minutes, then adding deionized water and heating to 95-100°C and continuing to stir the reaction for 2-3 hours, after the reaction is completed, pouring the reaction product into a hydrogen peroxide solution and stirring the reaction for 20-30 minutes, then centrifuging, washing the precipitate with saturated brine and distilled water for 2-3 times in sequence, then placing it in a vacuum drying oven, and drying it at a temperature of 55-60°C for 1.5-2.5 hours to obtain graphene oxide;
[0010] Step a2: adding graphene oxide and anhydrous toluene to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, ultrasonically dispersing for 20-30 minutes at an ultrasonic frequency of 40-50kHz, then adding the coupling agent solution dropwise while stirring at a temperature of 25-30°C and a stirring rate of 300-400r / min, and controlling the dropping rate to be 1-2 drops / s. After the dropwise addition is completed, the temperature is raised to 70-75°C and the stirring reaction is continued for 4-5 hours. After the reaction is completed, the reaction product is cooled to room temperature, then centrifuged, and the precipitate is placed in a vacuum drying oven and dried at a temperature of 55-60°C for 2-3 hours to obtain modified graphene;
[0011] Wherein, component B is polysiloxane resin;
[0012] The polysiloxane resin is a polysiloxane resin with a model number of SH-1151.
[0013] As a further solution of the present invention: the usage ratio of the graphite powder, sodium nitrate, concentrated sulfuric acid, potassium permanganate and deionized water in step a1 is 2g:0.8-1g:40-45mL:6-8g:40-45mL.
[0014] As a further solution of the present invention: the mass fraction of the concentrated sulfuric acid is 97-98%.
[0015] As a further solution of the present invention: the mass fraction of the hydrogen peroxide solution is 21-25%.
[0016] As a further solution of the present invention: the usage ratio of the graphene oxide, anhydrous toluene and coupling agent solution in step a2 is 3g:30-35mL:10-15mL.
[0017] As a further solution of the present invention: the coupling agent solution is a solution prepared by mixing the coupling agent, anhydrous ethanol and deionized water in the proportion of 0.8-2.4 g: 20-25 mL: 2-5 mL.
[0018] As a further solution of the present invention: the coupling agent is one of silane coupling agent KH-580 and silane coupling agent KH-590.
[0019] As a further solution of the present invention: a method for preparing underwater ceramic coating comprises the following steps:
[0020] Step 1: weigh 40-50 parts of mixed resin monomer, 55-65 parts of xylene, 22-30 parts of trimethylolpropane triacrylate, 2-6 parts of azobisisobutyronitrile, 2.5-8.5 parts of modified graphene, 3-6 parts of sodium silicate, 2.2-4.4 parts of boron nitride, 1.3-2.5 parts of silicon carbide, 3-7 parts of titanium dioxide, 11-19 parts of cobalt blue pigment, 2-4 parts of ultraviolet absorber, 2-4 parts of antioxidant, 3-7 parts of dispersant and 0.8-1.6 parts of defoaming agent according to weight parts, and set aside;
[0021] Step 2: Add the mixed resin monomer, xylene, trimethylolpropane triacrylate and azobisisobutyronitrile into a mixer, and then stir and react for 4-5 hours at a temperature of 70-90° C. and a stirring rate of 300-400 r / min to obtain an anti-corrosion emulsion;
[0022] Step 3: Add modified graphene, sodium silicate, boron nitride, silicon carbide, titanium dioxide and cobalt blue pigment to the anti-corrosion emulsion in turn, continue stirring and reacting for 20-30 minutes, then add ultraviolet absorber, antioxidant, dispersant and defoamer in turn, continue stirring and reacting for 1-1.5 hours to obtain component A, and mix component A and component B in a mass ratio of 4:1 to obtain underwater ceramic coating; wherein component B is polysiloxane resin;
[0023] The polysiloxane resin is a polysiloxane resin with a model number of SH-1151.
[0024] As a further solution of the present invention: the mixed resin monomer includes methyl methacrylate, butyl acrylate, acrylamide and an anti-corrosion monomer;
[0025] As a further solution of the present invention: the mass ratio of the methyl methacrylate, butyl acrylate, acrylamide and anti-corrosion monomer is 2.2-3.2:6.8-9.8:1.4-3.6:0.5-5.5.
[0026] As a further solution of the present invention: the ultraviolet absorber is ultraviolet absorber UV329.
[0027] As a further solution of the present invention: the antioxidant is antioxidant 1010.
[0028] As a further solution of the present invention: the dispersant is dispersant NNO.
[0029] As a further solution of the present invention: the defoamer is defoamer BYK-024.
[0030] As a further solution of the present invention: the anti-corrosion monomer is prepared by the following steps:
[0031] Step b1: Add 3,5-di(trifluoromethyl)nitrobenzene, 1,3-dibromo-5,5-dimethylhydantoin and anhydrous acetic acid to a three-necked flask equipped with a stirrer and a thermometer, stir and react for 10-15 minutes at a temperature of -5-0°C and a stirring rate of 300-400 r / min, then heat to 15-20°C and continue stirring and reacting for 3-5 hours. After the reaction is completed, pour the reaction product into ice water, let it stand and precipitate, then vacuum filter, place the filter cake in a vacuum drying oven, and dry it at a temperature of 50-55°C for 2-3 hours to obtain intermediate 1;
[0032] Step b2: magnesium powder, methyltriethoxysilane, iodine particles and anhydrous tetrahydrofuran are added to a three-necked flask equipped with a stirrer, a thermometer, a gas duct and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 25-30° C. and a stirring rate of 300-400 r / min for 20-30 min. Then, intermediate 1 is added and the mixture is heated to 65-70° C. and stirred for reaction for 8-10 h. After the reaction is completed, the reaction product is cooled to room temperature, and then vacuum filtered. The filtrate is rotary evaporated to remove the solvent to obtain intermediate 2;
[0033] Step b3: Add intermediate 2, 10% palladium carbon and anhydrous ethanol to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, introduce hydrogen to maintain the pressure at 1.1-1.3 MPa, then stir the reaction at a temperature of 25-30°C and a stirring rate of 300-400 r / min for 20-30 min, then heat to reflux and continue stirring the reaction for 2-3 h. After the reaction is completed, cool the reaction product to room temperature, then vacuum filter, and rotary evaporate the filtrate to remove the solvent to obtain intermediate 3;
[0034] Step b4: Add intermediate 3, cesium carbonate and dimethyl sulfoxide to a three-necked flask equipped with a stirrer, a thermometer and an air duct, introduce nitrogen protection, stir and react for 15-25 minutes at a temperature of 25-30°C and a stirring rate of 300-400r / min, then add acryloyl chloride dropwise while stirring, and control the dropping rate to 1-2 drops / s. After the addition is completed, heat the temperature to 55-60°C and continue stirring and reacting for 3-5 hours. After the reaction is completed, cool the reaction product to room temperature, add it to distilled water, and then extract it with dichloromethane 2-3 times. The combined extracts are washed with sodium carbonate solution 2-3 times, and then dried with anhydrous sodium sulfate. After vacuum filtration, the filtrate is rotary evaporated to remove the solvent to obtain an anti-corrosion monomer.
[0035] As a further solution of the present invention: the usage ratio of the 3,5-di(trifluoromethyl)nitrobenzene, 1,3-dibromo-5,5-dimethylhydantoin and anhydrous acetic acid in step b1 is 10 mmol: 5-6 mmol: 50-55 mL.
[0036] As a further solution of the present invention: the dosage ratio of the magnesium powder, methyltriethoxysilane, iodine particles, anhydrous tetrahydrofuran and intermediate 1 in step b2 is 0.45-0.55 g: 13-15 mmol: 0.1-0.12 g: 50-55 mL: 10 mmol.
[0037] As a further solution of the present invention: the usage ratio of the intermediate 2, 10% palladium carbon and anhydrous ethanol in step b3 is 10 mmol: 0.12-0.16 g: 50-55 mL.
[0038] As a further solution of the present invention: the usage ratio of the intermediate 3, cesium carbonate, dimethyl sulfoxide and acryloyl chloride in step b4 is 10mmol:13-15mmol:70-80mL:11-13mmol; the mass fraction of the sodium carbonate solution is 5-7%.
[0039] Beneficial effects of the present invention:
[0040] The invention discloses an underwater ceramic coating and a preparation method thereof. The invention comprises the following steps: adding a mixed resin monomer, xylene, trimethylolpropane triacrylate and azobisisobutyronitrile into a mixer for stirring and reacting to obtain an anti-corrosion emulsion; sequentially adding modified graphene, sodium silicate, boron nitride, silicon carbide, titanium dioxide and cobalt blue pigment into the anti-corrosion emulsion for continuous stirring and reaction; and then sequentially adding an ultraviolet absorber, an antioxidant, a dispersant and a defoaming agent for continuous stirring and reaction to obtain the underwater ceramic coating. The preparation method adopts anti-corrosion monomers and modified graphene, so that the underwater ceramic coating has extremely strong water resistance and corrosion resistance, and the formed coating has excellent anti-corrosion performance, so that the coating is resistant to water and chemical medium erosion, effectively protects the substrate from corrosion, and can keep the coating intact for a long time in an underwater environment. Moreover, after adding sodium silicate, boron nitride, silicon carbide and titanium dioxide, the hardness and wear resistance of the coating can be significantly improved, so that the coating has excellent wear resistance and weather resistance, and can be used for a long time in a harsh underwater environment without falling off or fading.
[0041] In the process of preparing underwater ceramic coating, a modified graphene is first prepared. First, graphite powder is used as a raw material to be oxidized to form graphene oxide, and then the graphene oxide is modified by a coupling agent. The siloxane on the coupling agent is hydrolyzed to form silanol, which can be grafted onto the surface of the graphene oxide. At the same time, a mercapto group is introduced to obtain modified graphene. In the process of preparing underwater ceramic coating, an anti-corrosion monomer is also prepared. First, 3,5-di(trifluoromethyl)nitrobenzene and 1,3-dibromo-5,5-dimethylhydantoin are reacted. 1,3-dibromo-5,5-dimethylhydantoin is used as The invention relates to a method for brominating 3,5-di(trifluoromethyl)nitrobenzene by using brominating agent, introducing bromine atom into the benzene ring of 3,5-di(trifluoromethyl)nitrobenzene, and obtaining intermediate 1. Then, magnesium powder, methyltriethoxysilane, iodine particles and intermediate 1 are used for Grignard reaction, and organic silicon is connected to the benzene ring instead of bromine atom, and obtaining intermediate 2. Then, the nitro group on intermediate 2 is reduced to amino group under hydrogen condition, and obtaining intermediate 3. Then, intermediate 3 and acryloyl chloride are reacted, and the amino group on intermediate 3 reacts with the acyl chloride group on acryloyl chloride, and alkenyl group is introduced to obtain anti-corrosion monomer. The anti-corrosion monomer is used as The olefinic group can undergo polymerization reaction with methyl methacrylate, butyl acrylate and acrylamide. Meanwhile, the modified graphene can undergo click chemical reaction with methyl methacrylate, butyl acrylate, acrylamide and the olefinic group on the anti-corrosion monomer by utilizing the thiol group, so that the modified graphene is connected to the polymer in the anti-corrosion emulsion in the form of chemical bonds, so that the bonding force between the two is excellent. Among them, the molecular structure of the anti-corrosion monomer contains a large number of CF bonds and Si-O bonds, which give it excellent chemical resistance, so that the prepared underwater ceramic coating has excellent water resistance and corrosion resistance. The modified graphene The stable layered structure of graphene can form a stable physical barrier to prevent the dispersion and penetration of corrosive media (water, acid, alkali, salt and bleaching agents containing strong oxidizing properties), and it itself has good chemical stability and can maintain its chemical properties unchanged in a corrosive environment. Therefore, the addition of modified graphene can protect underwater ceramic coatings from corrosive substances, further improve its water resistance and corrosion resistance, and at the same time greatly increase its hardness, greatly improving its wear resistance, so that the coating formed by underwater ceramic coatings can be used for a long time in harsh underwater environments without damage. DETAILED DESCRIPTION
[0042] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] Embodiment 1:
[0044] This embodiment is a method for preparing a ceramic coating for underwater use, comprising the following steps:
[0045] Step S1: 10 mmol 3,5-di(trifluoromethyl)nitrobenzene, 5 mmol 1,3-dibromo-5,5-dimethylhydantoin and 50 mL anhydrous acetic acid were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for reaction at -5°C and a stirring rate of 300 r / min for 10 min, then heated to 15°C and continued to stir for 3 h. After the reaction was completed, the reaction product was poured into ice water, and then allowed to stand and precipitate, and then vacuum filtered, and the filter cake was placed in a vacuum drying oven and dried at 50°C for 2 h to obtain intermediate 1;
[0046] Step S2: 0.45 g of magnesium powder, 13 mmol of methyltriethoxysilane, 0.1 g of iodine particles and 50 mL of anhydrous tetrahydrofuran were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at 25° C. and a stirring rate of 300 r / min for 20 min, and then 10 mmol of intermediate 1 was added and the mixture was heated to 65° C. and continued to stir for 8 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 2;
[0047] Step S3: 10 mmol of intermediate 2, 0.12 g of 10% palladium carbon and 50 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and hydrogen was introduced to maintain the pressure at 1.1 MPa. Then, the reaction was stirred at 25°C and a stirring rate of 300 r / min for 20 min, and then the temperature was raised to reflux and the stirring reaction was continued for 2 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 3;
[0048] Step S4: 10 mmol of intermediate 3, 13 mmol of cesium carbonate and 70 mL of dimethyl sulfoxide were added to a three-necked flask equipped with a stirrer, a thermometer and an air duct, and nitrogen was introduced for protection. The mixture was stirred for reaction at a temperature of 25°C and a stirring rate of 300 r / min for 15 min, and then 11 mmol of acryloyl chloride was added dropwise while stirring, and the dropping rate was controlled to be 1 drop / s. After the addition was completed, the temperature was raised to 55°C and the stirring reaction was continued for 3 h. After the reaction was completed, the reaction product was cooled to room temperature, and then added to distilled water, and then extracted with dichloromethane twice. The combined extracts were washed twice with a sodium carbonate solution with a mass fraction of 5%, and then dried with anhydrous sodium sulfate. After vacuum filtration, the filtrate was rotary evaporated to remove the solvent to obtain an anti-corrosion monomer;
[0049] Step S5: 2 g of graphite powder and 0.8 g of sodium nitrate are added to a three-necked flask equipped with a stirrer and a thermometer, and the mixture is stirred for reaction at a temperature of -5 ° C and a stirring rate of 300 r / min for 5 min, and then 40 mL of 97% concentrated sulfuric acid is added and the stirring reaction is continued for 15 min, and then 6 g of potassium permanganate is added and the stirring reaction is continued for 15 min, and then 40 mL of deionized water is added and the mixture is heated to 95 ° C and the stirring reaction is continued for 2 h. After the reaction is completed, the reaction product is poured into a 21% hydrogen peroxide solution and stirred for reaction for 20 min, and then centrifuged. The precipitate is washed twice with saturated brine and distilled water in sequence, and then placed in a vacuum drying oven and dried at a temperature of 55 ° C for 1.5 h to obtain graphene oxide;
[0050] Step S6: 3 g of graphene oxide and 30 mL of anhydrous toluene are added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and ultrasonically dispersed for 20 min at an ultrasonic frequency of 40 kHz, and then 10 mL of a coupling agent solution prepared by mixing anhydrous ethanol and deionized water in a ratio of 0.8 g: 20 mL: 2 mL is added dropwise while stirring at a temperature of 25 ° C and a stirring rate of 300 r / min, wherein the coupling agent is a silane coupling agent KH-580, and the dropping rate is controlled to be 1 drop / s. After the dropwise addition is completed, the temperature is raised to 70 ° C and the stirring reaction is continued for 4 h. After the reaction is completed, the reaction product is cooled to room temperature, and then centrifuged. The precipitate is placed in a vacuum drying oven and dried at a temperature of 55 ° C for 2 h to obtain modified graphene;
[0051] Step S7: 40 parts of mixed resin monomer, 55 parts of xylene, 22 parts of trimethylolpropane triacrylate, 2 parts of azobisisobutyronitrile, 2.5 parts of modified graphene, 3 parts of sodium silicate, 2.2 parts of boron nitride, 1.3 parts of silicon carbide, 3 parts of titanium dioxide, 11 parts of cobalt blue pigment, 2 parts of ultraviolet absorber, 2 parts of antioxidant, 3 parts of dispersant and 0.8 parts of defoamer are weighed according to weight parts for standby use; the mixed resin monomer includes methyl methacrylate, butyl acrylate, acrylamide and anti-corrosion monomer; the mass ratio of methyl methacrylate, butyl acrylate, acrylamide and anti-corrosion monomer is 2.2:6.8:1.4:0.5; the ultraviolet absorber is ultraviolet absorber uv329; the antioxidant is antioxidant 1010; the dispersant is dispersant NNO; the defoamer is defoamer BYK-024;
[0052] Step S8: adding the mixed resin monomer, xylene, trimethylolpropane triacrylate and azobisisobutyronitrile into a mixer, and then stirring the mixture for 4 hours at a temperature of 70° C. and a stirring rate of 300 r / min to obtain an anti-corrosion emulsion;
[0053] Step S9: Add modified graphene, sodium silicate, boron nitride, silicon carbide, titanium dioxide and cobalt blue pigment to the anti-corrosion emulsion in turn and continue to stir and react for 20 minutes, then add ultraviolet absorber, antioxidant, dispersant and defoaming agent in turn and continue to stir and react for 1 hour to obtain component A, and mix component A and component B in a mass ratio of 4:1 to obtain underwater ceramic coating; wherein component B is polysiloxane resin.
[0054] Embodiment 2:
[0055] This embodiment is a method for preparing underwater ceramic coating, comprising the following steps:
[0056] Step S1: 10 mmol 3,5-di(trifluoromethyl)nitrobenzene, 5.5 mmol 1,3-dibromo-5,5-dimethylhydantoin and 52 mL anhydrous acetic acid were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for reaction at -3°C and a stirring rate of 350 r / min for 12 min, then heated to 18°C and continued to stir for 4 h. After the reaction was completed, the reaction product was poured into ice water, and then allowed to stand and precipitate, and then vacuum filtered, and the filter cake was placed in a vacuum drying oven and dried at 52°C for 2.5 h to obtain intermediate 1;
[0057] Step S2: 0.5 g of magnesium powder, 14 mmol of methyltriethoxysilane, 0.11 g of iodine particles and 52 mL of anhydrous tetrahydrofuran were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred for reaction at a temperature of 28° C. and a stirring rate of 350 r / min for 25 min, and then 10 mmol of intermediate 1 was added and the mixture was heated to 68° C. and continued to stir for reaction for 9 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 2;
[0058] Step S3: 10 mmol of intermediate 2, 0.14 g of 10% palladium carbon and 52 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and hydrogen was introduced to maintain the pressure at 1.2 MPa. The reaction was stirred for 25 min at a temperature of 28 ° C and a stirring rate of 350 r / min, and then the temperature was raised to reflux and the stirring reaction was continued for 2.5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 3;
[0059] Step S4: 10 mmol of intermediate 3, 14 mmol of cesium carbonate and 75 mL of dimethyl sulfoxide were added to a three-necked flask equipped with a stirrer, a thermometer and an air duct, and nitrogen was introduced for protection. The reaction was stirred for 20 min at a temperature of 28°C and a stirring rate of 350 r / min, and then 12 mmol of acryloyl chloride was added dropwise while stirring, and the dropping rate was controlled to be 1 drop / s. After the addition was completed, the temperature was raised to 58°C and the stirring reaction was continued for 4 h. After the reaction was completed, the reaction product was cooled to room temperature and then added to distilled water, and then extracted with dichloromethane twice. The combined extracts were washed with a sodium carbonate solution with a mass fraction of 6% for 3 times, and then dried with anhydrous sodium sulfate. After vacuum filtration, the filtrate was rotary evaporated to remove the solvent to obtain an anti-corrosion monomer;
[0060] Step S5: 2 g of graphite powder and 0.9 g of sodium nitrate are added to a three-necked flask equipped with an agitator and a thermometer, and stirred for reaction at a temperature of 0°C and a stirring rate of 350 r / min for 10 min, and then 42 mL of 97.5% concentrated sulfuric acid is added and stirred for reaction for 18 min, and then 7 g of potassium permanganate is added and stirred for reaction for 18 min, and then 42 mL of deionized water is added and stirred for reaction for 2.5 h at a temperature of 98°C, and after the reaction, the reaction product is poured into a 23% hydrogen peroxide solution and stirred for reaction for 25 min, and then centrifuged, and the precipitate is washed twice with saturated brine and distilled water in sequence, and then placed in a vacuum drying oven and dried at a temperature of 58°C for 2 h to obtain graphene oxide;
[0061] Step S6: 3 g of graphene oxide and 32 mL of anhydrous toluene are added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and ultrasonically dispersed for 25 min at an ultrasonic frequency of 45 kHz, and then 12 mL of a coupling agent, anhydrous ethanol and deionized water are added dropwise while stirring at a temperature of 28 ° C and a stirring rate of 350 r / min. The coupling agent is a silane coupling agent KH-580, and the dropping rate is controlled to be 1 drop / s. After the dropwise addition is completed, the temperature is raised to 72 ° C and the stirring reaction is continued for 4.5 hours. After the reaction is completed, the reaction product is cooled to room temperature, and then centrifuged. The precipitate is placed in a vacuum drying oven and dried at a temperature of 58 ° C for 2.5 hours to obtain modified graphene;
[0062] Step S7: weigh 45 parts of mixed resin monomer, 60 parts of xylene, 26 parts of trimethylolpropane triacrylate, 4 parts of azobisisobutyronitrile, 5.5 parts of modified graphene, 4.5 parts of sodium silicate, 3.3 parts of boron nitride, 1.9 parts of silicon carbide, 5 parts of titanium dioxide, 15 parts of cobalt blue pigment, 3 parts of ultraviolet absorber, 3 parts of antioxidant, 5 parts of dispersant and 1.2 parts of defoamer according to weight parts, and set aside; the mixed resin monomer includes methyl methacrylate, butyl acrylate, acrylamide and anti-corrosion monomer; the mass ratio of methyl methacrylate, butyl acrylate, acrylamide and anti-corrosion monomer is 2.7:8.3:2.5:3; the ultraviolet absorber is ultraviolet absorber uv329; the antioxidant is antioxidant 1010; the dispersant is dispersant NNO; the defoamer is defoamer BYK-024;
[0063] Step S8: adding the mixed resin monomer, xylene, trimethylolpropane triacrylate and azobisisobutyronitrile into a mixer, and then stirring the mixture for 4.5 hours at a temperature of 80° C. and a stirring rate of 350 r / min to obtain an anti-corrosion emulsion;
[0064] Step S9: Add modified graphene, sodium silicate, boron nitride, silicon carbide, titanium dioxide and cobalt blue pigment to the anti-corrosion emulsion in turn and continue to stir and react for 25 minutes, then add ultraviolet absorber, antioxidant, dispersant and defoaming agent in turn and continue to stir and react for 1.2 hours to obtain component A, and mix component A and component B in a mass ratio of 4:1 to obtain underwater ceramic coating; wherein component B is polysiloxane resin.
[0065] Embodiment 3:
[0066] This embodiment is a method for preparing underwater ceramic coating, comprising the following steps:
[0067] Step S1: 10 mmol 3,5-di(trifluoromethyl)nitrobenzene, 6 mmol 1,3-dibromo-5,5-dimethylhydantoin and 55 mL anhydrous acetic acid were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for reaction at 0°C and a stirring rate of 400 r / min for 15 min, and then heated to 20°C and continued to stir for 5 h. After the reaction was completed, the reaction product was poured into ice water, and then allowed to stand and precipitate, and then vacuum filtered, and the filter cake was placed in a vacuum drying oven and dried at 55°C for 3 h to obtain intermediate 1;
[0068] Step S2: 0.55 g of magnesium powder, 15 mmol of methyltriethoxysilane, 0.12 g of iodine particles and 55 mL of anhydrous tetrahydrofuran were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at a temperature of 30° C. and a stirring rate of 400 r / min for 30 min. Then, 10 mmol of intermediate 1 was added and the mixture was heated to 70° C. and the stirring reaction was continued for 10 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered. The filtrate was rotary evaporated to remove the solvent to obtain intermediate 2;
[0069] Step S3: 10 mmol of intermediate 2, 0.16 g of 10% palladium carbon and 55 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and hydrogen was introduced to maintain the pressure at 1.3 MPa. Then, the mixture was stirred at 30°C and a stirring rate of 400 r / min for 30 min, and then the mixture was heated to reflux and continued to stir for 3 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 3;
[0070] Step S4: 10 mmol of intermediate 3, 15 mmol of cesium carbonate and 80 mL of dimethyl sulfoxide were added to a three-necked flask equipped with a stirrer, a thermometer and an air duct, and nitrogen was introduced for protection. The mixture was stirred for reaction at a temperature of 30°C and a stirring rate of 400 r / min for 25 min, and then 13 mmol of acryloyl chloride was added dropwise while stirring, and the dropping rate was controlled to be 2 drops / s. After the addition was completed, the temperature was raised to 60°C and the stirring reaction was continued for 5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then added to distilled water, and then extracted with dichloromethane for 3 times. The combined extracts were washed with a sodium carbonate solution with a mass fraction of 7% for 3 times, and then dried with anhydrous sodium sulfate. After vacuum filtration, the filtrate was rotary evaporated to remove the solvent to obtain an anti-corrosion monomer;
[0071] Step S5: Add 2g of graphite powder and 1g of sodium nitrate to a three-necked flask equipped with a stirrer and a thermometer, stir and react for 15min at a temperature of 5°C and a stirring rate of 400r / min, then add 45mL of 98% concentrated sulfuric acid and continue to stir and react for 20min, then add 8g of potassium permanganate and continue to stir and react for 20min, then add 45mL of deionized water and continue to stir and react for 3h at a temperature of 100°C, after the reaction is completed, pour the reaction product into a 25% hydrogen peroxide solution and stir and react for 30min, then centrifuge, wash the precipitate with saturated brine and distilled water three times in sequence, then place it in a vacuum drying oven, and dry it at a temperature of 60°C for 2.5h to obtain graphene oxide;
[0072] Step S6: 3 g of graphene oxide and 35 mL of anhydrous toluene are added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and ultrasonically dispersed for 30 min at an ultrasonic frequency of 50 kHz, and then 15 mL of a coupling agent solution prepared by mixing anhydrous ethanol and deionized water in a ratio of 2.4 g: 25 mL: 5 mL is added dropwise while stirring at a temperature of 30 ° C and a stirring rate of 400 r / min, wherein the coupling agent is a silane coupling agent KH-590, and the dropping rate is controlled to be 2 drops / s. After the dropwise addition is completed, the temperature is raised to 75 ° C and the stirring reaction is continued for 5 h. After the reaction is completed, the reaction product is cooled to room temperature, and then centrifuged. The precipitate is placed in a vacuum drying oven and dried at a temperature of 60 ° C for 3 h to obtain modified graphene;
[0073] Step S7: weigh 50 parts of mixed resin monomer, 65 parts of xylene, 30 parts of trimethylolpropane triacrylate, 6 parts of azobisisobutyronitrile, 8.5 parts of modified graphene, 6 parts of sodium silicate, 4.4 parts of boron nitride, 2.5 parts of silicon carbide, 7 parts of titanium dioxide, 19 parts of cobalt blue pigment, 4 parts of ultraviolet absorber, 4 parts of antioxidant, 7 parts of dispersant and 1.6 parts of defoamer according to weight parts, and set aside; the mixed resin monomer includes methyl methacrylate, butyl acrylate, acrylamide and anti-corrosion monomer; the mass ratio of methyl methacrylate, butyl acrylate, acrylamide and anti-corrosion monomer is 3.2:9.8:3.6:5.5; the ultraviolet absorber is ultraviolet absorber uv329; the antioxidant is antioxidant 1010; the dispersant is dispersant NNO; the defoamer is defoamer BYK-024;
[0074] Step S8: adding the mixed resin monomer, xylene, trimethylolpropane triacrylate and azobisisobutyronitrile into a mixer, and then stirring the mixture for 5 hours at a temperature of 90° C. and a stirring rate of 400 r / min to obtain an anti-corrosion emulsion;
[0075] Step S9: Add modified graphene, sodium silicate, boron nitride, silicon carbide, titanium dioxide and cobalt blue pigment to the anti-corrosion emulsion in turn and continue to stir and react for 30 minutes, then add ultraviolet absorber, antioxidant, dispersant and defoaming agent in turn and continue to stir and react for 1.5 hours to obtain component A, and mix component A and component B in a mass ratio of 4:1 to obtain underwater ceramic coating; wherein component B is polysiloxane resin.
[0076] Comparative Example 1:
[0077] This comparative example is a method for preparing a ceramic coating for underwater use, comprising the following steps:
[0078] Step S1: weigh 50 parts of mixed resin monomer, 65 parts of xylene, 30 parts of trimethylolpropane triacrylate, 6 parts of azobisisobutyronitrile, 6 parts of sodium silicate, 4.4 parts of boron nitride, 2.5 parts of silicon carbide, 7 parts of titanium dioxide, 19 parts of cobalt blue pigment, 4 parts of ultraviolet absorber, 4 parts of antioxidant, 7 parts of dispersant and 1.6 parts of defoamer according to weight parts, and set aside; the mixed resin monomer includes methyl methacrylate, butyl acrylate and acrylamide; the mass ratio of methyl methacrylate, butyl acrylate and acrylamide is 3.2:9.8:3.6; the ultraviolet absorber is ultraviolet absorber uv329; the antioxidant is antioxidant 1010; the dispersant is dispersant NNO; the defoamer is defoamer BYK-024;
[0079] Step S2: adding the mixed resin monomer, xylene, trimethylolpropane triacrylate and azobisisobutyronitrile into a mixer, and then stirring the mixture for 5 hours at a temperature of 90° C. and a stirring rate of 400 r / min to obtain an anti-corrosion emulsion;
[0080] Step S3: Sodium silicate, boron nitride, silicon carbide, titanium dioxide and cobalt blue pigment are added to the anti-corrosion emulsion in sequence and the reaction is continued with stirring for 30 minutes. Then, ultraviolet absorber, antioxidant, dispersant and defoaming agent are added in sequence and the reaction is continued with stirring for 1.5 hours to obtain component A, and component A and component B are mixed evenly at a mass ratio of 4:1 to obtain underwater ceramic coating; wherein component B is polysiloxane resin.
[0081] Comparative Example 2:
[0082] This comparative example is a method for preparing a ceramic coating for underwater use, comprising the following steps:
[0083] Step S1: 10 mmol 3,5-di(trifluoromethyl)nitrobenzene, 6 mmol 1,3-dibromo-5,5-dimethylhydantoin and 55 mL anhydrous acetic acid were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for reaction at 0°C and a stirring rate of 400 r / min for 15 min, and then heated to 20°C and continued to stir for 5 h. After the reaction was completed, the reaction product was poured into ice water, and then allowed to stand and precipitate, and then vacuum filtered, and the filter cake was placed in a vacuum drying oven and dried at 55°C for 3 h to obtain intermediate 1;
[0084] Step S2: 0.55 g of magnesium powder, 15 mmol of methyltriethoxysilane, 0.12 g of iodine particles and 55 mL of anhydrous tetrahydrofuran were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at a temperature of 30° C. and a stirring rate of 400 r / min for 30 min. Then, 10 mmol of intermediate 1 was added and the mixture was heated to 70° C. and the stirring reaction was continued for 10 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered. The filtrate was rotary evaporated to remove the solvent to obtain intermediate 2;
[0085] Step S3: 10 mmol of intermediate 2, 0.16 g of 10% palladium carbon and 55 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and hydrogen was introduced to maintain the pressure at 1.3 MPa. Then, the mixture was stirred at 30°C and a stirring rate of 400 r / min for 30 min, and then the mixture was heated to reflux and continued to stir for 3 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 3;
[0086] Step S4: 10 mmol of intermediate 3, 15 mmol of cesium carbonate and 80 mL of dimethyl sulfoxide were added to a three-necked flask equipped with a stirrer, a thermometer and an air duct, and nitrogen was introduced for protection. The mixture was stirred for reaction at a temperature of 30°C and a stirring rate of 400 r / min for 25 min, and then 13 mmol of acryloyl chloride was added dropwise while stirring, and the dropping rate was controlled to be 2 drops / s. After the addition was completed, the temperature was raised to 60°C and the stirring reaction was continued for 5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then added to distilled water, and then extracted with dichloromethane for 3 times. The combined extracts were washed with a sodium carbonate solution with a mass fraction of 7% for 3 times, and then dried with anhydrous sodium sulfate. After vacuum filtration, the filtrate was rotary evaporated to remove the solvent to obtain an anti-corrosion monomer;
[0087] Step S5: weigh 50 parts of mixed resin monomer, 65 parts of xylene, 30 parts of trimethylolpropane triacrylate, 6 parts of azobisisobutyronitrile, 6 parts of sodium silicate, 4.4 parts of boron nitride, 2.5 parts of silicon carbide, 7 parts of titanium dioxide, 19 parts of cobalt blue pigment, 4 parts of ultraviolet absorber, 4 parts of antioxidant, 7 parts of dispersant and 1.6 parts of defoamer according to weight parts, and set aside; the mixed resin monomer includes methyl methacrylate, butyl acrylate, acrylamide and anti-corrosion monomer; the mass ratio of methyl methacrylate, butyl acrylate, acrylamide and anti-corrosion monomer is 3.2:9.8:3.6:5.5; the ultraviolet absorber is ultraviolet absorber uv329; the antioxidant is antioxidant 1010; the dispersant is dispersant NNO; the defoamer is defoamer BYK-024;
[0088] Step S6: adding the mixed resin monomer, xylene, trimethylolpropane triacrylate and azobisisobutyronitrile into a mixer, and then stirring the mixture for 5 hours at a temperature of 90° C. and a stirring rate of 400 r / min to obtain an anti-corrosion emulsion;
[0089] Step S7: Sodium silicate, boron nitride, silicon carbide, titanium dioxide and cobalt blue pigment are added to the anti-corrosion emulsion in sequence and the reaction is continued with stirring for 30 minutes. Then, ultraviolet absorber, antioxidant, dispersant and defoaming agent are added in sequence and the reaction is continued with stirring for 1.5 hours to obtain component A, and component A and component B are mixed evenly at a mass ratio of 4:1 to obtain underwater ceramic coating; wherein component B is polysiloxane resin.
[0090] Comparative Example 3:
[0091] This comparative example is a method for preparing a ceramic coating for underwater use, comprising the following steps:
[0092] Step S1: Add 2g of graphite powder and 1g of sodium nitrate to a three-necked flask equipped with a stirrer and a thermometer, stir and react for 15min at a temperature of 5°C and a stirring rate of 400r / min, then add 45mL of 98% concentrated sulfuric acid and continue to stir and react for 20min, then add 8g of potassium permanganate and continue to stir and react for 20min, then add 45mL of deionized water and continue to stir and react for 3h at a temperature of 100°C, after the reaction is completed, pour the reaction product into a 25% hydrogen peroxide solution and stir and react for 30min, then centrifuge, wash the precipitate with saturated brine and distilled water three times in sequence, then place it in a vacuum drying oven, and dry it at a temperature of 60°C for 2.5h to obtain graphene oxide;
[0093] Step S2: 3 g of graphene oxide and 35 mL of anhydrous toluene are added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and ultrasonically dispersed for 30 min at an ultrasonic frequency of 50 kHz, and then 15 mL of a coupling agent solution prepared by mixing anhydrous ethanol and deionized water in a ratio of 2.4 g: 25 mL: 5 mL is added dropwise while stirring at a temperature of 30 ° C and a stirring rate of 400 r / min, wherein the coupling agent is a silane coupling agent KH-590, and the dropping rate is controlled to be 2 drops / s. After the dropwise addition is completed, the temperature is raised to 75 ° C and the stirring reaction is continued for 5 h. After the reaction is completed, the reaction product is cooled to room temperature, and then centrifuged. The precipitate is placed in a vacuum drying oven and dried at a temperature of 60 ° C for 3 h to obtain modified graphene;
[0094] Step S3: weigh 50 parts of mixed resin monomer, 65 parts of xylene, 30 parts of trimethylolpropane triacrylate, 6 parts of azobisisobutyronitrile, 8.5 parts of modified graphene, 6 parts of sodium silicate, 4.4 parts of boron nitride, 2.5 parts of silicon carbide, 7 parts of titanium dioxide, 19 parts of cobalt blue pigment, 4 parts of ultraviolet absorber, 4 parts of antioxidant, 7 parts of dispersant and 1.6 parts of defoamer according to weight parts, and set aside; the mixed resin monomer includes methyl methacrylate, butyl acrylate and acrylamide; the mass ratio of methyl methacrylate, butyl acrylate and acrylamide is 3.2:9.8:3.6; the ultraviolet absorber is ultraviolet absorber uv329; the antioxidant is antioxidant 1010; the dispersant is dispersant NNO; the defoamer is defoamer BYK-024;
[0095] Step S4: adding the mixed resin monomer, xylene, trimethylolpropane triacrylate and azobisisobutyronitrile into a mixer, and then stirring the mixture for 5 hours at a temperature of 90° C. and a stirring rate of 400 r / min to obtain an anti-corrosion emulsion;
[0096] Step S5: Add modified graphene, sodium silicate, boron nitride, silicon carbide, titanium dioxide and cobalt blue pigment to the anti-corrosion emulsion in turn and continue to stir and react for 30 minutes, then add ultraviolet absorber, antioxidant, dispersant and defoaming agent in turn and continue to stir and react for 1.5 hours to obtain component A, and mix component A and component B in a mass ratio of 4:1 to obtain underwater ceramic coating; wherein component B is polysiloxane resin.
[0097] The underwater ceramic coatings of Examples 1-3 and Comparative Examples 1-3 were applied to the surface of horseshoes and cured to form a coating film with a thickness of 40±2 μm. The acid resistance, alkali resistance, salt resistance, hardness and water drop contact angle tests were then performed. The test results are shown in the following table:
[0098]
[0099] Among them, acid resistance A is soaked in 5wt% hydrochloric acid solution for 96 hours; acid resistance B is soaked in 5wt% nitric acid solution for 96 hours; alkali resistance is soaked in 5wt% sodium hydroxide solution for 96 hours; salt resistance is soaked in 50g / L sodium chloride solution for 500 hours; bleach resistance is soaked in 5wt% trichloroisocyanuric acid solution for 96 hours.
[0100] Referring to the data in the above table, it can be seen that adding anti-corrosion monomers and modified graphene can effectively improve the corrosion resistance, hardness and hydrophobicity of underwater ceramic coatings. Among them, the corrosion resistance, hardness and hydrophobicity of underwater ceramic coatings prepared under the synergistic effect of anti-corrosion monomers and modified graphene are the best.
[0101] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0102] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A ceramic coating for underwater use, characterized in that: Component A and component B, and the mass ratio of component A to component B is 4:1; Wherein, component A comprises the following components in parts by weight: 40-50 parts of mixed resin monomer, 55-65 parts of xylene, 22-30 parts of trimethylolpropane triacrylate, 2-6 parts of azobisisobutyronitrile, 2.5-8.5 parts of modified graphene, 3-6 parts of sodium silicate, 2.2-4.4 parts of boron nitride, 1.3-2.5 parts of silicon carbide, 3-7 parts of titanium dioxide, 11-19 parts of cobalt blue pigment, 2-4 parts of ultraviolet absorber, 2-4 parts of antioxidant, 3-7 parts of dispersant and 0.8-1.6 parts of defoamer; wherein the mixed resin monomer includes methyl methacrylate, butyl acrylate, acrylamide and anti-corrosion monomer; Wherein, the modified graphene is prepared by the following steps: Step a1: stirring graphite powder and sodium nitrate for reaction, then sequentially adding concentrated sulfuric acid, potassium permanganate and deionized water and continuing stirring the reaction, after the reaction is completed, pouring the reaction product into a hydrogen peroxide solution and stirring the reaction, then centrifuging, washing and drying the precipitate to obtain graphene oxide; Step a2: ultrasonically dispersing graphene oxide and anhydrous toluene, then adding a coupling agent solution dropwise while stirring, continuing to stir the reaction after the addition is complete, cooling the reaction product after the reaction is complete, then centrifuging, and drying the precipitate to obtain modified graphene; Wherein, the anti-corrosion monomer is prepared by the following steps: Step b1: 3,5-di(trifluoromethyl)nitrobenzene, 1,3-dibromo-5,5-dimethylhydantoin and anhydrous acetic acid are stirred for reaction. After the reaction, the reaction product is poured into ice water, and then allowed to stand for precipitation. After that, vacuum filtration is performed, and the filter cake is dried to obtain intermediate 1; Step b2: Stir and react magnesium powder, methyltriethoxysilane, iodine particles and anhydrous tetrahydrofuran, then add intermediate 1 and continue stirring and reacting, after the reaction is completed, cool the reaction product, then vacuum filter, and rotary evaporate the filtrate to obtain intermediate 2; Step b3: reacting the intermediate 2, 10% palladium carbon and anhydrous ethanol with stirring under the condition of passing hydrogen gas, cooling the reaction product after the reaction, and then vacuum filtering, and rotary evaporating the filtrate to obtain the intermediate 3; Step b4: Stir the intermediate 3, cesium carbonate and dimethyl sulfoxide for reaction, then add acryloyl chloride dropwise while stirring, continue stirring for reaction after the addition is complete, cool the reaction product after the reaction is complete, then add it into distilled water, extract it, wash and dry the extract, then vacuum filter it, and rotary evaporate the filtrate to obtain an anti-corrosion monomer; Wherein, component B is polysiloxane resin; The polysiloxane resin is a polysiloxane resin with a model number of SH-1151.
2. The underwater ceramic coating according to claim 1, characterized in that: The amount ratio of the graphite powder, sodium nitrate, concentrated sulfuric acid, potassium permanganate and deionized water in step a1 is 2g:0.8-1g:40-45mL:6-8g:40-45mL; the mass fraction of the concentrated sulfuric acid is 97-98%, and the mass fraction of the hydrogen peroxide solution is 21-25%.
3. The underwater ceramic coating according to claim 1, characterized in that: The amount ratio of the graphene oxide, anhydrous toluene and coupling agent solution in step a2 is 3g:30-35mL:10-15mL; the coupling agent solution is a solution in which the coupling agent, anhydrous ethanol and deionized water are mixed according to 0.8-2.4g:20-25mL:2-5mL; the coupling agent is one of silane coupling agent KH-580 and silane coupling agent KH-590.
4. The underwater ceramic coating according to claim 1, characterized in that: The usage ratio of the 3,5-bis(trifluoromethyl)nitrobenzene, 1,3-dibromo-5,5-dimethylhydantoin and anhydrous acetic acid in step b1 is 10 mmol: 5-6 mmol: 50-55 mL.
5. The underwater ceramic coating according to claim 1, characterized in that: The dosage ratio of the magnesium powder, methyltriethoxysilane, iodine particles, anhydrous tetrahydrofuran and intermediate 1 in step b2 is 0.45-0.55 g: 13-15 mmol: 0.1-0.12 g: 50-55 mL: 10 mmol.
6. The underwater ceramic coating according to claim 1, characterized in that: The usage ratio of the intermediate 2, 10% palladium carbon and anhydrous ethanol in step b3 is 10 mmol: 0.12-0.16 g: 50-55 mL.
7. The underwater ceramic coating according to claim 1, characterized in that: The usage ratio of the intermediate 3, cesium carbonate, dimethyl sulfoxide and acryloyl chloride in step b4 is 10 mmol: 13-15 mmol: 70-80 mL: 11-13 mmol.
8. The underwater ceramic coating according to claim 1, characterized in that: The mass ratio of the methyl methacrylate, butyl acrylate, acrylamide and anti-corrosion monomer is 2.2-3.2:6.8-9.8:1.4-3.6:0.5-5.5; the ultraviolet absorber is ultraviolet absorber uv329; the antioxidant is antioxidant 1010; the dispersant is dispersant NNO; and the defoamer is defoamer BYK-024.
9. A method for preparing underwater ceramic coating according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step 1: Weigh 40-50 parts of mixed resin monomer, 55-65 parts of xylene, 22-30 parts of trimethylolpropane triacrylate, 2-6 parts of azobisisobutyronitrile, 2.5-8.5 parts of modified graphene, 3-6 parts of sodium silicate, 2.2-4.4 parts of boron nitride, 1.3-2.5 parts of silicon carbide, 3-7 parts of titanium dioxide, 11-19 parts of cobalt blue pigment, 2-4 parts of ultraviolet absorber, 2-4 parts of antioxidant, 3-7 parts of dispersant and 0.8-1.6 parts of defoaming agent according to weight parts, and set aside; wherein the mixed resin monomer includes methyl methacrylate, butyl acrylate, acrylamide and anti-corrosion monomer; Step 2: Add the mixed resin monomer, xylene, trimethylolpropane triacrylate and azobisisobutyronitrile into a mixer, and then stir and react for 4-5 hours at a temperature of 70-90° C. and a stirring rate of 300-400 r / min to obtain an anti-corrosion emulsion; Step 3: Add modified graphene, sodium silicate, boron nitride, silicon carbide, titanium dioxide and cobalt blue pigment to the anti-corrosion emulsion in turn and continue to stir and react for 20-30 minutes, then add ultraviolet absorber, antioxidant, dispersant and defoaming agent in turn and continue to stir and react for 1-1.5 hours to obtain component A, and mix component A and component B in a mass ratio of 4:1 to obtain underwater ceramic coating; wherein component B is polysiloxane resin; the polysiloxane resin is a polysiloxane resin with model SH-1151.