A kind of adhesive for polymer coating diaphragm and its preparation method and application
By introducing specific structural unit A and modification reagent into the adhesive for polymer-coated diaphragm, the cohesion and flexibility of the adhesive are improved, and the performance of polymer-coated diaphragm adhesive in the prior art is solved. The problem is that the heat resistance and bonding performance of the diaphragm are improved and the overall performance of the secondary battery is improved.
Patent Information
- Application Number
- CN202411045445.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-01
AI Technical Summary
In the prior art, the cohesiveness and flexibility of the adhesive for polymer-coated diaphragm are insufficient, resulting in poor heat resistance and bonding properties of the diaphragm.
Using a binder containing a polymer, the molecular chain structure of the polymer contains a specific structural unit A, through a combination of a water-soluble polyhydroxy polymer, a graft-modified monomer and an acetal modification reagent, Heat treatment and pH adjustment were performed to prepare adhesives with suitable cohesion and flexibility.
The coating peel strength and heat resistance of polymer-coated separators are improved, the bonding performance is enhanced, and the electrochemical performance and safety performance of secondary batteries are improved.
Smart Images

Figure CN118580813B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of bonding materials, and in particular to an adhesive for polymer-coated diaphragms, and a preparation method and application thereof. Background Art
[0002] The diaphragm is a key component of secondary batteries, including coated diaphragms and uncoated diaphragms. The traditional coated diaphragm is to use an adhesive to apply powdered ceramic to the surface of a polyolefin diaphragm to form a ceramic coating. This ceramic coating can effectively improve the safety-related properties of the diaphragm, such as heat resistance and puncture resistance, but the function of the ceramic coating is relatively single and the weight is heavy, which is not conducive to the lightweight of the battery. Due to its different functions and light weight, polymer powders have been increasingly widely used in the field of secondary battery diaphragm coatings in recent years. However, due to the performance differences between polymer powders and ceramic powders, especially the surface performance differences, the adhesive used for ceramic powder coating is difficult to apply to polymer powder coating. For example, when trying to use an adhesive for ceramic powder coating to coat polymer powder, the adhesive has poor dispersion and wettability on the powder, which makes it difficult for the powder to be effectively dispersed in the coating slurry, resulting in poor coating uniformity and poor adhesion. On the other hand, water-soluble polyhydroxy polymers represented by polyvinyl alcohol and sodium carboxymethyl cellulose are also commonly used adhesives. Although these substances can disperse and wet polymer powders well, they have defects such as insufficient cohesion or flexibility, so the bonding force is still insufficient and needs to be effectively modified before use.
[0003] Therefore, in order to meet the development needs of polymer powder coated diaphragms, it is urgent to develop an adhesive that is compatible with polymer powder coated diaphragms.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] One object of the present invention is to provide a polymer-coated membrane adhesive to solve the technical problem that the polymer-coated membrane adhesive in the prior art has insufficient cohesion and flexibility, resulting in poor heat resistance and bonding performance of the membrane. The polymer-coated membrane adhesive of the present invention has better cohesion and flexibility, good coating effect, good bonding performance, and is conducive to improving the coating peel strength and heat resistance of the membrane.
[0006] Another object of the present invention is to provide a method for preparing the adhesive for polymer-coated diaphragms. The method is simple and easy to implement. Through the coordination of various steps, an adhesive with suitable cohesion and flexibility, good coating effect and high bonding strength can be obtained.
[0007] Another object of the present invention is to provide a polymer-coated separator.
[0008] Another object of the present invention is to provide a secondary battery.
[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0010] An adhesive for a polymer-coated separator, the adhesive comprising a high molecular polymer, the molecular chain structure of the high molecular polymer comprising the following structural unit A;
[0011] ;
[0012] Wherein, p is a positive integer; R0 is a hydrogen atom or a methyl group; R1 includes a hydrogen atom, or includes a saturated hydrocarbon group with 1 to 4 carbon atoms, and the saturated hydrocarbon group also contains at least one of a carboxyl group, a hydroxyl group and an amino group; R5 includes X and an optional Y, X is a residue formed after X1 participates in a grafting reaction, wherein X1 is mainly prepared from a water-soluble polyhydroxy polymer and an acetalization modification agent, Y is a residue formed after a water-soluble polyhydroxy polymer participates in a grafting reaction, and Y contains a hydroxyl group.
[0013] In some embodiments, the following structure in the structural unit A can be partially or completely replaced by a structural unit of a polymer containing a cyclic amide group; the structural unit of the polymer containing a cyclic amide group includes a structural unit of polyvinyl pyrrolidone and / or a structural unit of polyacryloylmorpholine;
[0014] .
[0015] In some embodiments, the X comprises the following structure:
[0016] .
[0017] Wherein, q is 1 or 2; n is a positive integer; R2 includes a hydrogen atom, or a saturated hydrocarbon group with 1 to 2 carbon atoms, or a composite group consisting of a saturated hydrocarbon group with 2 to 5 carbon atoms and at least one hydroxyl group; * represents the connection site between R5 and -CH- in the structural unit A;
[0018] R4 includes a hydrogen atom or a structure of the following formula (I):
[0019] (I).
[0020] ** in formula (I) represents the connection site between R4 and X.
[0021] In some embodiments, the R4 may also include a structural unit of a polymer containing a cyclic amide group.
[0022] In some embodiments, the binder for polymer-coated separators further comprises water.
[0023] In some embodiments, the solid content of the binder for polymer-coated separator is 10% to 15%.
[0024] In some embodiments, the pH of the binder for polymer-coated separators is 2-5 or 7-10.
[0025] The method for preparing the adhesive for polymer-coated diaphragms as described above comprises the following steps:
[0026] A mixture of a water-soluble polyhydroxy polymer, a graft-modified monomer, an initiator and water is heat-treated.
[0027] In some embodiments, the water-soluble polyhydroxy polymer includes at least one of polyvinyl alcohol, natural polysaccharides, and modified natural polysaccharides.
[0028] In some embodiments, in the water-soluble polyhydroxy polymer, the natural polysaccharide and the modified natural polysaccharide include at least one of sodium carboxymethyl cellulose, hydroxyethyl cellulose, cyclodextrin, sodium alginate, xanthan gum, guar gum and gum arabic.
[0029] In some embodiments, the graft modification monomer includes methacrylic acid and / or water-soluble methacrylates, and the ester group of the methacrylate includes a saturated hydrocarbon group with 1 to 4 carbon atoms, and the saturated hydrocarbon group contains at least one of a carboxyl group, a hydroxyl group and an amino group.
[0030] In some embodiments, the graft-modified monomer further comprises an olefinic substance containing a cyclic amide group, and the olefinic substance containing a cyclic amide group comprises N-vinyl pyrrolidone and / or acryloylmorpholine.
[0031] In some embodiments, the molar amount of the graft modification monomer is equivalent to 0.1% to 100% of the molar amount of the repeating unit of the water-soluble polyhydroxy polymer.
[0032] In some embodiments, the synthetic raw materials of the adhesive further include an acetalization modification agent; the acetalization modification agent is added to the mixture. The preparation method of the adhesive for polymer-coated diaphragms specifically includes: adjusting the pH of the water-soluble polyhydroxy polymer aqueous solution to less than 2, keeping stirring, adding the acetalization modification agent, heating to 50-90°C, and keeping the temperature for reaction for 1-6 hours; then adjusting the pH of the aqueous solution to 6.5-7.5, adjusting the temperature to 60-70°C, adding the grafting modification monomer and initiator in sequence, and keeping the temperature for reaction for 4-16 hours.
[0033] In some embodiments, the initiator is a persulfate-based soluble initiator.
[0034] In some embodiments, the synthetic raw materials of the adhesive further include a pH regulator, and the pH of the mixed system obtained after the heat treatment is adjusted by the pH regulator to 2-5 or 7-10.
[0035] In some embodiments, the heat treatment temperature is 50-90°C.
[0036] In some embodiments, the heat treatment is carried out for a holding time of 4 to 16 hours.
[0037] In some embodiments, the water-soluble polyhydroxy polymer is at least one of cyclodextrin, xanthan gum and guar gum, and polyvinyl alcohol, and the mass fraction of the polyvinyl alcohol is greater than or equal to 95%.
[0038] In some embodiments, the graft-modified monomer is a composite of the methacrylate and the olefinic substance containing a cyclic amide group, and the mass fraction of the methacrylate in the composite is greater than or equal to 50%.
[0039] In some embodiments, the molar amount of the acetalization modification agent is equivalent to 10% to 50% of the molar amount of the hydroxyl group of the water-soluble polyhydroxy polymer.
[0040] A polymer coated diaphragm comprises a base film and a polymer layer located on the surface of the base film; the polymer layer is obtained by coating a coating slurry on the surface of the base film and drying; the coating slurry contains polymer powder, a wetting agent, deionized water and the above-mentioned adhesive or an adhesive obtained by the above-mentioned method.
[0041] A secondary battery comprises a negative electrode sheet, a positive electrode sheet, an electrolyte and the above-mentioned polymer-coated diaphragm.
[0042] Compared with the prior art, the present invention has the following beneficial effects:
[0043] (1) The adhesive of the present invention is a modified substance based on a polyhydroxy polymer, which has suitable cohesion and / or flexibility, good coating effect, good bonding performance, good heat resistance, and can improve the coating peel strength and heat resistance of the polymer coated diaphragm.
[0044] (2) The method of the present invention is based on the modification of water-soluble polyhydroxy polymers, and the obtained adhesive has suitable cohesion and flexibility, good coating effect, and good bonding performance. It can well improve the bonding performance of the coating of the polymer-coated diaphragm and improve its heat resistance.
[0045] (3) The polymer-coated separator of the present invention has high peel strength of the coating layer and good heat resistance. Furthermore, the obtained secondary battery has excellent electrochemical performance and high safety performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0047] Figure 1 is an infrared spectrum of the adhesive of Example 18 of the present invention;
[0048] Figure 2 is a differential scanning calorimetry curve diagram of the adhesive of Example 18 of the present invention;
[0049] Figure 3 is a thermogravimetric analysis curve of the adhesive of Example 18 of the present invention;
[0050] Figure 4 This is a cyclic voltammetry curve of a battery prepared with the adhesive of Example 18 of the present invention. DETAILED DESCRIPTION
[0051] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0052] According to one aspect of the present invention, the present invention relates to an adhesive for a polymer-coated diaphragm, the adhesive comprising a high molecular polymer, the molecular chain structure of the high molecular polymer comprising the following structural unit A;
[0053] ;
[0054] Wherein, p is a positive integer; R0 is a hydrogen atom or a methyl group; R1 includes a hydrogen atom, or includes a saturated hydrocarbon group with 1 to 4 carbon atoms, and the saturated hydrocarbon group also contains at least one of a carboxyl group, a hydroxyl group and an amino group; R5 includes X and optionally Y, X is a residue formed after X1 participates in a grafting reaction, wherein X1 is mainly prepared from a water-soluble polyhydroxy polymer and an acetalization modification agent, and Y is a residue formed after a water-soluble polyhydroxy polymer participates in a grafting reaction.
[0055] The adhesive of the present invention is a modified substance based on a polyhydroxy polymer, which has suitable cohesion and / or flexibility, good coating effect, good bonding performance, good heat resistance, and can improve the coating peeling strength and heat resistance of the polymer coated diaphragm.
[0056] It should be noted that, for any specific form of structural unit A, R1 may represent any single structure among the structures described above, or may represent two or more structures, which is related to the number of types of raw materials for synthesizing the grafted polymer. For example, when the raw materials for synthesizing the grafted polymer only include acrylic acid, R1 only represents a hydrogen atom; when the raw materials for synthesizing the grafted polymer include acrylic acid and hydroxyethyl acrylate, R1 simultaneously represents: (1) a hydrogen atom; (2) a composite group consisting of a saturated hydrocarbon group consisting of 2 carbon atoms and 1 hydroxyl group.
[0057] In some embodiments, the following structure in the structural unit A can be partially or completely replaced by a structural unit of a polymer containing a cyclic amide group; the structural unit of the polymer containing a cyclic amide group includes a structural unit of polyvinyl pyrrolidone and / or a structural unit of polyacryloylmorpholine;
[0058] .
[0059] In some embodiments, the X comprises the following structure, which is obtained by acetalization modification of a water-soluble polyhydroxy polymer.
[0060] ;
[0061] Wherein, q is 1 or 2; n is a positive integer; R2 includes a hydrogen atom, or a saturated hydrocarbon group with 1 to 2 carbon atoms, or a composite group consisting of a saturated hydrocarbon group with 2 to 5 carbon atoms and at least one hydroxyl group. The * in the X structure indicates the connection site between R5 and -CH- in the structural unit A.
[0062] R4 includes a hydrogen atom or a structure of the following formula (I);
[0063] (I).
[0064] In formula (I), p is a positive integer; R0 is a hydrogen atom or a methyl group; R1 includes a hydrogen atom, or includes a saturated hydrocarbon group with 1 to 4 carbon atoms, and the saturated hydrocarbon group also contains at least one of a carboxyl group, a hydroxyl group and an amino group. ** in formula (I) represents the connection site between R4 and the X structure.
[0065] In some embodiments, the R4 may further include a structural unit of a polymer containing a cyclic amide group. The structural unit of the polymer containing a cyclic amide group is a structural unit of polyvinyl pyrrolidone and / or a structural unit of polyacryloylmorpholine.
[0066] In some embodiments, the polymer-coated membrane adhesive further comprises water. The adhesive of the present invention is a modified substance based on a water-soluble polyhydroxy polymer, including modification by graft polymerization, and optionally acetalization modification. The product obtained after modification is a water-soluble polymer. The adhesive is prepared, stored and used in the form of an aqueous solution. The solid content of the polymer-coated membrane adhesive is 10% to 15%, for example, 10%, 11%, 12%, 13%, 15%, etc., or any range value between the two.
[0067] In some embodiments, the pH of the polymer-coated separator binder is 2-5 or 7-10, such as 2, 3, 4, 5, 7, 8, 9, 10, etc.
[0068] According to another aspect of the present invention, the present invention also relates to a method for preparing the adhesive for polymer-coated diaphragms as described above, comprising the following steps:
[0069] A mixture of a water-soluble polyhydroxy polymer, a graft-modified monomer, an initiator and water is heat-treated.
[0070] The present invention dissolves the grafted modified monomer, the initiator and the water-soluble polyhydroxy polymer in an aqueous solution, initiates polymerization and obtains a product in the form of an aqueous solution; the adhesive obtained by the method has suitable cohesion and flexibility, good coating effect and good bonding performance, can well improve the bonding performance of the coating of the polymer-coated diaphragm and improve its heat resistance.
[0071] In some embodiments, the water-soluble polyhydroxy polymer includes at least one of polyvinyl alcohol, natural polysaccharides and modified natural polysaccharides. Among the water-soluble polyhydroxy polymers, natural polysaccharides and modified natural polysaccharides include at least one of sodium carboxymethyl cellulose, hydroxyethyl cellulose, cyclodextrin, sodium alginate, xanthan gum, guar gum and gum arabic. The water-soluble polyhydroxy polymer of the present invention can be any one of the above, or a combination of multiple. Preferably, the water-soluble polyhydroxy polymer is at least one of cyclodextrin, xanthan gum and guar gum, and polyvinyl alcohol, and the mass fraction of the polyvinyl alcohol is ≥95%, such as 95%, 96%, 97%, 98%, 99% or 100%, etc. The water-soluble polyhydroxy polymer containing at least 95% polyvinyl alcohol is more conducive to improving the cohesion and / or flexibility of the adhesive.
[0072] In some embodiments, the graft modification monomer includes methacrylic acid and / or water-soluble methacrylates; the ester group of the methacrylate includes a saturated hydrocarbon group with a carbon number of 1 to 4, and the saturated hydrocarbon group contains at least one of a carboxyl group, a hydroxyl group and an amino group. In some embodiments, the water-soluble methacrylates include: hydroxyethyl (meth)acrylate, hydroxypropyl ester or hydroxybutyl ester, the hydrocarbon group has 2, 3 or 4 carbon atoms, and also includes a hydroxyl group. In some embodiments, the water-soluble methacrylates include: carboxyethyl (meth)acrylate, carboxypropyl ester or carboxybutyl ester, the hydrocarbon group has 2, 3 or 4 carbon atoms, and also includes a carboxyl group. In some embodiments, the water-soluble methacrylates include: dimethylaminomethyl (meth)acrylate or dimethylaminoethyl ester, the hydrocarbon group has 1 or 2 carbon atoms, and also includes an amino group (or a monomethyl / dimethyl substituted amino group).
[0073] In some embodiments, the molar amount of the graft-modified monomer is equivalent to 0.1% to 100% of the molar amount of the repeating unit of the water-soluble polyhydroxy polymer (base resin), for example, 0.1%, 1%, 5%, 10%, 15%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90% or 100%, or any range between two values, preferably 1% to 20%, more preferably 5% to 15%.
[0074] An example (not limiting, only for readers to better understand the calculation of the amount of graft modification monomer): Assume that the base resin is polyvinyl alcohol, the molecular weight of its repeating unit is 44g / mol; the graft modification monomer is acrylic acid, the molecular weight is 72g / mol. If the amount of polyvinyl alcohol is 44g, that is, the molar amount of the repeating unit is 1mol, then at least 0.001mol of acrylic acid should be added, that is, 0.072g; at most 1mol of acrylic acid should be added, that is, 72g.
[0075] In some embodiments, the graft-modified monomer further comprises an olefinic substance containing a cyclic amide group, and the olefinic substance containing a cyclic amide group comprises N-vinyl pyrrolidone and / or acryloylmorpholine. In some embodiments, the graft-modified monomer is a composite of the methacrylate and the olefinic substance containing a cyclic amide group, and the mass fraction of the methacrylate in the composite is greater than or equal to 50%, including but not limited to 50%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, etc., or any range value between the two. The above-mentioned olefinic substance containing a cyclic amide group can introduce a rigid cyclic amide group into the graft-modified polymer, and thus is beneficial to improve the heat resistance of the product, that is, the ability of the coated diaphragm to resist shrinkage when heated.
[0076] In some embodiments, the synthetic raw materials of the adhesive further include an acetalization modifying agent; the acetalization modifying agent is added to the mixture. The acetalization modifying agent is a water-soluble monoaldehyde, including an aldehyde group, with a carbon number of 1 to 3, such as formaldehyde, acetaldehyde, propionaldehyde; it can also be a water-soluble aldose with a carbon number of 3 to 6, such as propionose, butyrose, pentose, and hexose. The introduction of the acetalization modifying agent can form a rigid ring structure on the main chain, thereby improving the cohesion of the product, and thus can improve at least one of the adhesion and heat resistance of the product. Since the acetalization reaction is a reaction of an aldehyde group with two hydroxyl groups, the amount of the acetalization modifying agent is determined by the number of hydroxyl groups of the water-soluble polyhydroxy polymer. Specifically, the amount (molar amount) of the acetal modification agent is equivalent to 10% to 50% of the molar amount of the hydroxyl group of the water-soluble polyhydroxy polymer, such as 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45% or 50%, etc. The use of an appropriate amount of the acetal modification agent in the present invention is more conducive to improving the adhesion and heat resistance of the adhesive.
[0077] An example is given (not limiting, only to help readers better understand the calculation of the amount of acetal modification agent): Assume that the base resin is polyvinyl alcohol, the molecular weight of its repeating unit is 44g / mol, and each repeating unit contains 1 hydroxyl group; the acetal modification agent is a commercially available formaldehyde solution with a concentration of 37% and a formaldehyde molecular weight of 30g / mol. If the amount of polyvinyl alcohol used is 44g, the molar amount of hydroxyl groups is 1mol, so the amount of formaldehyde used is at least 0.1mol, equivalent to a solution mass of about 8.11g; at most 0.5mol, equivalent to a solution mass of about 40.54g.
[0078] In some embodiments, the initiator includes but is not limited to ammonium persulfate, and the weight of the initiator is 0.5% to 1% of the total weight of the graft-modified monomer, for example, 0.5%, 0.6%, 0.7%, 0.8%, 1%, etc.
[0079] In some embodiments, the synthetic raw materials of the adhesive further include a pH regulator, including an acidity regulator and an alkalinity regulator. The pH value of the adhesive can be adjusted within the range of 2 to 5 or 7 to 10 as required. Generally, the pH value of the adhesive is related to the type of grafted modified monomer. If the grafted modified monomer is acidic or neutral, the pH value of the product is generally adjusted to 2 to 5; if the grafted modified monomer is alkaline, the pH value of the product is generally adjusted to 7 to 10.
[0080] In some embodiments, the temperature of the heat treatment is 50-90°C, such as 50°C, 55°C, 60°C, 70°C, 80°C, 90°C, etc. In some embodiments, the heat treatment holding time is 4-16h, such as 4h, 5h, 6h, 9h, 10h, 12h, 15h or 16h, etc., or any range between the two. The suitable heat treatment temperature and holding time of the present invention are conducive to the reaction to ensure the bonding performance of the adhesive, etc.
[0081] In some embodiments, the method for preparing the adhesive for polymer-coated separators comprises the following steps:
[0082] (a) Prepare the measured water, water-soluble polyhydroxy polymer, grafted modified monomer, initiator, and pH adjuster. The amount of each substance should ensure that the solid content of the final product is 10%~15%. (b) In the reaction device, prepare an aqueous solution of water-soluble polyhydroxy polymer, then add the above-mentioned grafted modified monomer into the reaction device, stir it thoroughly to completely dissolve it; keep stirring and raise the temperature to 60~70℃. (c) Add initiator into the reaction device, then keep the temperature for 4~16h. (d) Add pH adjuster as needed to make the pH value of the product 3~5 or 7~10, then cool and collect the material.
[0083] In some embodiments, the method for preparing the adhesive for polymer-coated separators comprises the following steps:
[0084] (a) Prepare measured water, water-soluble polyhydroxy polymer, acetalization modification agent, grafting modification monomer, initiator, and pH regulator. The amount of each substance should ensure that the solid content of the final product is 10%~15%. (b) In the reaction device, prepare an aqueous solution of water-soluble polyhydroxy polymer, and then add pH regulator to the reaction device to make the pH value of the aqueous solution less than 2. (c) Keep stirring, add acetalization modification agent, then raise the temperature to 50~90℃, and keep the temperature for reaction for 1~6h. (d) Add pH regulator to make the pH value of the aqueous solution 6.5~7.5, and then adjust the temperature to 60~70℃. (e) Add grafting modification monomer and stir it thoroughly to dissolve it completely. (f) Add initiator, and then keep the temperature for reaction for 4~16h; (g) Add pH regulator as needed to make the pH value of the product 3~5 or 7~10, and then cool and collect the material.
[0085] According to one aspect of the present invention, the present invention also relates to a diaphragm including a base film and a polymer layer located on the surface of the base film; the polymer layer is obtained by coating a coating slurry on the surface of the base film and drying; the coating slurry contains polymer powder, a wetting agent, deionized water and an adhesive, and the adhesive is the above-mentioned binder, or an adhesive obtained by the above-mentioned method.
[0086] The separator of the present invention has excellent bonding performance and heat resistance.
[0087] According to one aspect of the present invention, the present invention also relates to a secondary battery, comprising a negative electrode sheet, a positive electrode sheet, an electrolyte and the above-mentioned separator.
[0088] The battery of the present invention adopts the diaphragm prepared by the above-mentioned binder, and has more excellent electrochemical performance and good safety performance.
[0089] The following is further explained in conjunction with specific embodiments and comparative examples.
[0090] Example 1
[0091] A method for preparing an adhesive comprises the following steps:
[0092] (1) Prepare measured amounts of water, water-soluble polyol polymer (polyvinyl alcohol), grafting modification monomer (carboxybutyl acrylate), initiator (ammonium persulfate), and pH adjuster (lithium hydroxide monohydrate). The amount of carboxybutyl acrylate is equivalent to 100% of the molar amount of the repeating unit of the base resin. The amount of each substance should ensure that the solid content of the final product is 12%.
[0093] (2) In a reaction device, an aqueous solution of a water-soluble polyhydroxy polymer is prepared, and then carboxybutyl acrylate is added to the reaction device and stirred thoroughly to completely dissolve it;
[0094] (3) Keep stirring and raise the temperature to 65°C;
[0095] (4) adding ammonium persulfate to the reaction device, wherein the weight of the ammonium persulfate is 0.5% of the total weight of the grafted monomer, and then keeping the temperature to react for 8 hours;
[0096] (5) Add lithium hydroxide monohydrate as needed to make the pH value of the product reach 4, and then cool and collect the material.
[0097] Embodiments 2 to 8
[0098] The difference between Examples 2 to 8 and Example 1 is that the types of water-soluble polyhydroxy polymers are different.
[0099] The water-soluble polyhydroxy polymers of Examples 2 to 8 are specifically shown in Table 1.
[0100] Table 1 Water-soluble polyhydroxy polymers of Examples 2 to 8
[0101]
[0102] Embodiments 9 to 22
[0103] The difference between Examples 9 to 22 and Example 1 is that the amount of carboxybutyl acrylate used is different.
[0104] The amount of carboxybutyl acrylate used in Examples 9 to 22 is equivalent to the molar amount of the repeating unit of the base resin as shown in Table 2.
[0105] Table 2 Amount of carboxybutyl acrylate in Examples 9 to 22
[0106]
[0107] Embodiments 24 to 40
[0108] The difference between Examples 24 to 40 and Example 18 is that the types of graft-modified monomers are different.
[0109] The graft-modified monomers of Examples 24 to 40 are shown in Table 3.
[0110] Table 3 Graft-modified monomers of Examples 24 to 40
[0111]
[0112] Embodiment 41
[0113] The difference between Example 41 and Example 18 is that the water-soluble polyhydroxy polymer is a compound of polyvinyl alcohol and cyclodextrin, wherein the mass fraction of polyvinyl alcohol is 95%.
[0114] Embodiment 42
[0115] The difference between Example 42 and Example 18 is that the water-soluble polyhydroxy polymer is a compound of polyvinyl alcohol and xanthan gum, wherein the mass fraction of polyvinyl alcohol is 95%.
[0116] Embodiment 43
[0117] The difference between Example 43 and Example 18 is that the water-soluble polyhydroxy polymer is a compound of polyvinyl alcohol and guar gum, wherein the mass fraction of polyvinyl alcohol is 95%.
[0118] Embodiment 44
[0119] The difference between Example 44 and Example 43 is that in the composite of polyvinyl alcohol and guar gum, the mass fraction of polyvinyl alcohol is 96%.
[0120] Embodiment 45
[0121] The difference between Example 45 and Example 43 is that in the composite of polyvinyl alcohol and guar gum, the mass fraction of polyvinyl alcohol is 97%.
[0122] Embodiment 46
[0123] The difference between Example 46 and Example 43 is that in the composite of polyvinyl alcohol and guar gum, the mass fraction of polyvinyl alcohol is 98%.
[0124] Embodiment 47
[0125] The difference between Example 47 and Example 43 is that in the composite of polyvinyl alcohol and guar gum, the mass fraction of polyvinyl alcohol is 99%.
[0126] Embodiment 48
[0127] The difference between Example 48 and Example 18 is that the graft-modified monomer is a compound of carboxybutyl acrylate and N-vinyl pyrrolidone, wherein the mass fraction of carboxybutyl acrylate in the compound is 50%.
[0128] Embodiment 49
[0129] The difference between Example 49 and Example 18 is that the graft-modified monomer is a compound of carboxybutyl acrylate and acryloylmorpholine, wherein the mass fraction of carboxybutyl acrylate in the compound is 50%.
[0130] Embodiment 50
[0131] The difference between Example 50 and Example 49 is that the mass fraction of carboxybutyl acrylate in the compound is 60%.
[0132] Embodiment 51
[0133] The difference between Example 51 and Example 49 is that the mass fraction of carboxybutyl acrylate in the compound is 70%.
[0134] Embodiment 52
[0135] The difference between Example 52 and Example 49 is that the mass fraction of carboxybutyl acrylate in the compound is 80%.
[0136] Embodiment 53
[0137] The difference between Example 53 and Example 49 is that the mass fraction of carboxybutyl acrylate in the compound is 90%.
[0138] Embodiment 54
[0139] The preparation method of the adhesive of this embodiment introduces an acetal modification agent based on Example 18, and the amount used is equivalent to 10% of the molar amount of the hydroxyl group of the water-soluble polyhydroxy polymer. Specifically, it includes the following steps:
[0140] (1) Prepare the measured water, water-soluble polyhydroxy polymer (polyvinyl alcohol), acetal modification agent, graft modification monomer (carboxybutyl acrylate), initiator, and pH adjuster. The amount of each substance should ensure that the solid content of the final product is 12%;
[0141] (2) preparing an aqueous solution of a water-soluble polyhydroxy polymer in a reaction device, and then adding a pH adjuster into the reaction device to adjust the pH value of the aqueous solution to less than 2;
[0142] (3) Keep stirring and add acetal modification reagent, then raise the temperature to 70°C and keep the temperature for reaction for 3 hours;
[0143] (4) Adding a pH adjuster to adjust the pH value of the aqueous solution to 7.2, and then adjusting the temperature to 65°C;
[0144] (5) Add the grafted modified monomer and stir thoroughly to make it completely dissolved;
[0145] (6) Add initiator and then keep warm for 8 hours;
[0146] (7) Add pH adjuster as needed to adjust the pH value of the product to 4.6, and then cool and collect the material.
[0147] Embodiments 55 to 63
[0148] The difference between Examples 55 to 63 and Example 54 is that the types of acetalization modification reagents are different, as shown in Table 4.
[0149] Table 4 Acetalization modification reagents of Examples 55 to 63
[0150]
[0151] Embodiment 64
[0152] The difference between Example 64 and Example 61 is that the amount of glucose used is equivalent to 20% of the molar amount of hydroxyl groups of the water-soluble polyhydroxy polymer.
[0153] Embodiment 65
[0154] The difference between Example 65 and Example 61 is that the amount of glucose used is equivalent to 30% of the molar amount of hydroxyl groups of the water-soluble polyhydroxy polymer.
[0155] Embodiment 66
[0156] The difference between Example 66 and Example 61 is that the amount of glucose used is equivalent to 40% of the molar amount of hydroxyl groups of the water-soluble polyhydroxy polymer.
[0157] Embodiment 67
[0158] The difference between Example 67 and Example 61 is that the amount of glucose used is equivalent to 50% of the molar amount of hydroxyl groups of the water-soluble polyhydroxy polymer.
[0159] Comparative Example 1
[0160] A binder is a commercially available product of the water-soluble polyhydroxy polymer (polyvinyl alcohol) in Example 1.
[0161] Comparative Example 2
[0162] A binder is a commercially available product of the water-soluble polyhydroxy polymer (sodium carboxymethyl cellulose) in Example 2.
[0163] Comparative Example 3
[0164] A binder is a commercially available water-soluble polyhydroxy polymer (hydroxyethyl cellulose) in Example 3.
[0165] Comparative Example 4
[0166] A binder using a commercially available water-soluble polyhydroxy polymer (cyclodextrin) in Example 4.
[0167] Comparative Example 5
[0168] A binder using a commercially available water-soluble polyhydroxy polymer (sodium alginate) in Example 5.
[0169] Comparative Example 6
[0170] A binder using a commercially available water-soluble polyhydroxy polymer (xanthan gum) in Example 6.
[0171] Comparative Example 7
[0172] A binder is a commercially available water-soluble polyhydroxy polymer (guar gum) as described in Example 7.
[0173] Comparative Example 8
[0174] A commercially available water-soluble polyhydroxy polymer (gum arabic) in Example 8 was used as an adhesive.
[0175] Comparative Example 9
[0176] The invention discloses an adhesive, which adopts a certain brand of commercially available water-based acrylic emulsion ceramic diaphragm adhesive.
[0177] Experimental Example 1
[0178] The adhesive of Example 18 was subjected to infrared spectroscopy test, differential scanning calorimetry test, thermogravimetric analysis and cyclic voltammetry test. The infrared spectrum (FT-IR curve) of the adhesive is as follows: Figure 1The differential scanning calorimetry curve (DSC curve) of the adhesive is shown in Figure 2 The thermogravimetric analysis curve (TGA curve) of the adhesive is shown in Figure 3 The cyclic voltammetry curve (CV curve) of the battery obtained by the adhesive is shown as Figure 4 As shown, compared with the blank sample, the battery obtained by the adhesive in Example 18 of the present invention has no abnormal redox reaction in the range of 0~4.6V.
[0179] Experimental Example 2
[0180] Application Examples 1-67 and Application Comparative Examples 1-9: The adhesives of Examples 1-67 and Comparative Examples 1-9 are respectively prepared to obtain polymer powder coating slurries, and the specific methods are as follows:
[0181] In a pulping device, deionized water, adhesive and wetting agent are mixed and stirred until uniformly dispersed; polymer powder is added and stirred at a speed of 1500 rpm for 60-90 minutes to obtain polymer powder coating slurry. Among them, the mass fraction of the adhesive in the slurry formula is 1% (based on total non-volatile matter); the wetting agent is lauryl alcohol polyoxyethylene ether; and the polymer powder is modified polyacrylate powder.
[0182] The obtained slurry is applied to the surface of the secondary battery separator made of polyolefin, with a coating amount of 1.0~1.1g / m 2 , a secondary battery separator coated with polymer powder is obtained.
[0183] Application Example 68: The difference from Application Example 18 is that the polymer powder is polyvinylidene fluoride powder.
[0184] Application Example 69: The difference from Application Example 18 is that the polymer powder is polyimide powder.
[0185] Application Example 70: The difference from Application Example 18 is that the polymer powder is polyaniline powder.
[0186] Experimental Example 3
[0187] The coated separators of application examples 1 to 67 and application comparative examples 1 to 9 in Experimental Example 2 were respectively subjected to peel strength test and heat resistance test.
[0188] 1. Separator coating peel strength test: Take the coated separators of application examples 1 to 67 and application comparative examples 1 to 9, cut them into test strips with a length of about 10 cm and a width of about 2.5 cm. Stick the coated surface of the strips onto 3M double-sided tape, press them with a roller, and then use an electronic tensile tester to test their 180° peel strength.
[0189] 2. Diaphragm heat resistance test: Take the coated diaphragms described in Application Examples 1 to 67 and Application Comparative Examples 1 to 9, and cut them into test samples with a length and width of about 10 cm. Sandwich the sample between two A4 printing papers, and then place it flat in an electric hot air drying oven at 130°C. Take it out after 1 hour, measure and calculate the transverse and longitudinal heat shrinkage rates of the sample. Take another uncoated diaphragm and test it in the same way as a blank sample. The test results are shown in Table 5.
[0190] Table 5 Test results of membrane coating peel strength and membrane heat resistance
[0191]
[0192]
[0193]
[0194]
[0195]
[0196] It can be seen from the test results of Table 5 that compared with the blank sample and application comparative examples 1 to 9, application examples 1 to 67 have better performance in the coating peel strength and heat resistance of the diaphragm than application comparative examples 1 to 9. It can be seen from application examples 48 to 53 that the introduction of cyclic amide groups is beneficial to improving the heat resistance of the product. It can be seen from application examples 54 to 67 that the introduction of acetalization modification is beneficial to improving the peel strength and / or heat resistance of the product. It can be seen from application examples 68 to 70 that the adhesive of the present invention can be applied to the coating of various polymer powders.
[0197] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A polymer-coated diaphragm adhesive, characterized in that: The adhesive comprises a high molecular polymer, and the molecular chain structure of the high molecular polymer comprises the following structural unit A; ; Wherein, p is a positive integer; R0 includes a hydrogen atom or a methyl group; R1 includes a hydrogen atom, or a saturated hydrocarbon group having 1 to 4 carbon atoms replaced by at least one of a carboxyl group, a hydroxyl group and an amino group; R5 includes X and optionally Y, X is a residue formed by X1 participating in a grafting reaction, wherein X1 is mainly prepared from a water-soluble polyhydroxy polymer and an acetal modification agent, and Y is a residue formed by a water-soluble polyhydroxy polymer participating in a grafting reaction; The water-soluble polyhydroxy polymer includes at least one of polyvinyl alcohol, natural polysaccharides and modified natural polysaccharides; among the water-soluble polyhydroxy polymers, the natural polysaccharides and modified natural polysaccharides include at least one of sodium carboxymethyl cellulose, hydroxyethyl cellulose, cyclodextrin, sodium alginate, xanthan gum, guar gum and gum arabic; The following structure in the structural unit A is partially or completely replaced by a structural unit of a polymer containing a cyclic amide group; the structural unit of the polymer containing a cyclic amide group includes a structural unit of polyvinyl pyrrolidone and / or a structural unit of polyacryloylmorpholine; 。 2. The adhesive for polymer-coated separators according to claim 1, characterized in that The X comprises the following structure; ; Wherein, q is 1 or 2; n is a positive integer; R2 includes a hydrogen atom, or a saturated hydrocarbon group with 1 to 2 carbon atoms, or a composite group consisting of a saturated hydrocarbon group with 2 to 5 carbon atoms and at least one hydroxyl group; * represents the connection site between R5 and -CH- in the structural unit A; R4 includes a hydrogen atom or a structure of the following formula (I); (I); ** in formula (I) represents the connection site between R4 and X.
3. The adhesive for polymer-coated separators according to claim 2, characterized in that: The R4 further comprises a structural unit of a polymer containing a cyclic amide group.
4. The adhesive for polymer-coated separators according to claim 1, characterized in that: Contains at least one of the following features (1) to (3): (1) The polymer-coated separator adhesive further comprises water; (2) The solid content of the adhesive for the polymer-coated diaphragm is 10% to 15%; (3) The pH of the polymer-coated separator binder is 2 to 5 or 7 to 10.
5. The method for preparing the adhesive for polymer-coated separators according to claim 1, characterized in that: The following steps are involved: Heat-treating a mixture of a water-soluble polyhydroxy polymer, a grafting modification monomer, an initiator and water; the synthetic raw materials of the adhesive also include an acetalization modification agent; The acetalization modifying agent is added to the mixture.
6. The method for preparing the adhesive for polymer-coated separator according to claim 5, characterized in that: Contains at least one of the following features (1) to (9): (1) The water-soluble polyhydroxy polymer comprises at least one of polyvinyl alcohol, natural polysaccharides and modified natural polysaccharides; (2) In the water-soluble polyhydroxy polymer, the natural polysaccharide and the modified natural polysaccharide include at least one of sodium carboxymethyl cellulose, hydroxyethyl cellulose, cyclodextrin, sodium alginate, xanthan gum, guar gum and gum arabic; (3) The graft modification monomer includes methacrylic acid and / or water-soluble methacrylic acid esters, and the ester group of the methacrylic acid ester includes a group formed by replacing the hydrogen atom of a saturated hydrocarbon group having 1 to 4 carbon atoms with at least one of a carboxyl group, a hydroxyl group and an amino group; (4) The graft-modified monomer further comprises an olefinic substance containing a cyclic amide group, wherein the olefinic substance containing a cyclic amide group comprises N-vinyl pyrrolidone and / or acryloylmorpholine; (5) The molar amount of the graft-modified monomer is equivalent to 0.1% to 100% of the molar amount of the repeating unit of the water-soluble polyhydroxy polymer; (6) The preparation method of the polymer-coated diaphragm adhesive comprises: adjusting the pH of the water-soluble polyhydroxy polymer aqueous solution to less than 2, maintaining stirring, adding the acetalization modification reagent, heating to 50-90°C, and keeping the temperature for reaction for 1-6 hours; then adjusting the pH of the aqueous solution to 6.5-7.5, adjusting the temperature to 60-70°C, adding the graft modification monomer and the initiator in sequence, and keeping the temperature for reaction for 4-16 hours; (7) The synthetic raw materials of the adhesive further include a pH adjuster, and the pH of the mixed system obtained after the heat treatment is adjusted by the pH adjuster to 2-5 or 7-10; (8) The temperature of the heat treatment is 50-90°C; (9) The heat treatment holding time is 4 to 16 hours.
7. The method for preparing the adhesive for polymer-coated separator according to claim 6, characterized in that: Contains at least one of the following features (1) to (3): (1) The water-soluble polyhydroxy polymer is at least one of cyclodextrin, xanthan gum and guar gum, and polyvinyl alcohol, and the mass fraction of the polyvinyl alcohol is ≥95%; (2) The graft modification monomer is a composite of the methacrylate and the olefinic substance containing a cyclic amide group, and the mass fraction of the methacrylate in the composite is greater than or equal to 50%; (3) The molar amount of the acetalization modification agent is equivalent to 10% to 50% of the molar amount of the hydroxyl group of the water-soluble polyhydroxy polymer.
8. A polymer-coated diaphragm, characterized in that: It comprises a base film and a polymer layer located on the surface of the base film; the polymer layer is obtained by coating a coating slurry on the surface of the base film and drying; the coating slurry contains polymer powder, a wetting agent, deionized water and an adhesive, and the adhesive is the adhesive for polymer-coated diaphragms according to any one of claims 1 to 4, or the adhesive obtained by the preparation method of the adhesive for polymer-coated diaphragms according to any one of claims 5 to 7.
9. A secondary battery, characterized in that: It comprises a negative electrode sheet, a positive electrode sheet, an electrolyte and the polymer-coated separator according to claim 8.