A biodegradable polyurethane controlled-release fertilizer coating material and fertilizer molding process
By using polyurethane controlled-release fertilizer coating materials made of degradable polyether and isocyanate components, the soil pollution problem caused by non-degradable coating materials is solved, and the effect of reducing pollution risks and improving fertilizer utilization is achieved. And the process is simple and easy to follow.
Patent Information
- Application Number
- CN202411045151.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-01
AI Technical Summary
Most of the existing polyurethane coating materials are non-degradable, resulting in soil pollution. The degradable polyurethane is high in the industry and has high technical thresholds, so there are few cases that can be truly realized.
Use degradable polyether and isocyanate components to make polyurethane-type controlled-release fertilizer coating materials, control the fertilizer nutrient release rate through the polycarbonate section, increase the degradability and toughness of the material, and perform fertilizer molding through specific process steps. , reduce the risk of soil and water pollution.
It has achieved the reduction of soil and water pollution risks, extended the shelf life of fertilizers, maintained the quality and nutrient content of fertilizers, improved nutrient utilization, and low production costs and simple processes.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of agricultural fertilizers, and in particular relates to a biodegradable polyurethane controlled-release fertilizer coating material introduced with carbon dioxide and a fertilizer molding process. Background Art
[0002] Polyurethane has always been one of the mainstream directions of slow-release coating materials. Polyurethane fertilizer coatings achieve slow-release effects by wrapping fertilizer particles, delaying the release rate of nutrients, improving nutrient utilization, reducing nutrient loss and waste, and helping to stabilize crop growth and increase yields. Polyurethane coatings can also effectively protect fertilizers from external environmental influences, extend shelf life, maintain fertilizer quality and nutrient content, improve fertilizer stability and storability, and reduce environmental pollution risks.
[0003] However, most of the current polyurethane coating materials are non-degradable, and will cause secondary pollution to the soil when actually used. Currently, degradable polyurethane is restricted by cost and technical barriers in the industry, and there are few cases where the technology is truly realized. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a degradable polyurethane controlled-release fertilizer coating material and a fertilizer molding process with low preparation cost and simple production process.
[0005] The technical solution adopted by the present invention to solve the technical problem is: a degradable polyurethane controlled-release fertilizer coating material comprises two components A and B, wherein the component A is a polyether and the component B is an isocyanate, and is characterized in that the polyether is a polyether diol or a polyether polyol, the molecular chain of the polyether contains random or block polycarbonate segments, the polycarbonate segments are copolymerized by an epoxy compound and carbon dioxide, and the molar ratio of the polycarbonate segments in molecular weight is 5% to 95%.
[0006] The degradable polyurethane controlled-release fertilizer coating material of the present invention is made of degradable polyether and isocyanate components, which is beneficial to reducing the impact on the environment and reducing the risk of soil and water pollution. The content of the polycarbonate segment is used to control the release rate of fertilizer nutrients, improve nutrient utilization, and help reduce nutrient loss and waste; this material can effectively wrap fertilizer particles, provide good protection, extend the shelf life of fertilizers, maintain the quality and nutrient content of fertilizers, and increase the stability of fertilizers. Preferably, the molar ratio of the polycarbonate segment in molecular weight is 50% to 95%.
[0007] Preferably, in the above-mentioned degradable polyurethane controlled-release fertilizer coating material, the number average molecular weight of the polyether is between 300 and 5000.
[0008] The preferred number average molecular weight can maintain better degradability and is easy to coat. The polyether with a number average molecular weight within this range has a better controlled release effect, and the length of the molecular chain is moderate, which is conducive to achieving an appropriate nutrient release rate, thereby improving nutrient utilization. More preferably, the number average molecular weight of the polyether is between 1300 and 1700.
[0009] Preferably, in the above-mentioned degradable polyurethane controlled-release fertilizer coating material, the polyether molecular chain contains random or block polyether segments, the molar ratio of the polyether segments in molecular weight is 1% to 40%, and the polyether segments are self-polymerized segments of epoxy compounds. The appropriate amount of polyether segment content adjusts the coating material to have good elasticity, so that the coating material has appropriate ductility and toughness, thereby improving the material's wrapping effect on fertilizer particles, providing better protection, and reducing fertilizer loss and waste.
[0010] Preferably, in the above-mentioned degradable polyurethane controlled-release fertilizer coating material, the epoxy compound is ethylene oxide or / and propylene oxide. Ethylene oxide or / and propylene oxide can polymerize with carbon dioxide to form PEC and PPC segments, and the prepared coating has better fluidity and biodegradability during processing, thereby enhancing the adhesion and biocompatibility of the degradable polyurethane controlled-release fertilizer coating material.
[0011] The structural formula of the PEC segment is:
[0012] .
[0013] The structural formula of the PPC segment is:
[0014] .
[0015] Preferably, in the above-mentioned degradable polyurethane controlled-release fertilizer coating material, the mass ratio of the polyether to the isocyanate is 1:0.1-0.5. The mass ratio of the polyether to the isocyanate is controlled to optimize the structure of the coating material, ensure the degradability of the material, control the nutrient release rate, reduce the dissolution and loss of the fertilizer, and improve the nutrient utilization rate.
[0016] Preferably, in the above-mentioned degradable polyurethane controlled-release fertilizer coating material, the isocyanate is toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), diphenylmethane diisocyanate (MDI), dicyclohexylmethane diisocyanate (HMDI) or hexamethylene diisocyanate (HDI).
[0017] A fertilizer forming process comprises the following steps:
[0018] 1) removing water from the raw materials of the two components A and B of the above-mentioned biodegradable polyurethane controlled-release fertilizer coating material to make the moisture content less than 0.1%; and mixing the raw materials into the coating material;
[0019] 2) Add the coating material and fertilizer into the coating machine at a mass ratio of 1:30~60, control the temperature in the coating machine at 40℃~60℃ and rotate and stir to solidify the coating material on the surface of the fertilizer, and cool to obtain.
[0020] During the fertilizer molding process, biodegradable polyurethane controlled-release fertilizer coating materials are used to mold fertilizers to achieve controlled-release effects and improve nutrient utilization: first, the two components of the coating materials are dehydrated to avoid reducing the weather resistance of the coating materials due to moisture, reduce the formation of bubbles on the coating, and prevent uneven curing. A certain proportion of the coating material and fertilizer are added to the coating machine, and the temperature range is controlled to ensure that the coating material is evenly cured on the fertilizer surface.
[0021] Preferably, in the above fertilizer molding process, the coating material and the fertilizer described in step 2) are in a mass ratio of 1:40-50. The preferred ratio can better balance the ratio between the coating material and the fertilizer, ensure the uniformity and consistency of the coating layer, thereby improving the quality and stability of the coating, while ensuring the nutrient release effect and controlled release performance of the fertilizer.
[0022] Preferably, in the above fertilizer molding process, the temperature in the coating machine in step 2) is controlled at 45° C. to 55° C. At the preferred coating temperature, the curing and wrapping process of the coating material is more favorable, which is beneficial to the quality and stability of the coating.
[0023] Compared with the prior art, the degradable polyurethane controlled-release fertilizer coating material and fertilizer molding process of the present invention have the following beneficial effects: the present invention utilizes the content of the polycarbonate segment to control the fertilizer nutrient release rate. The polyether segment content is utilized to make the coating material have appropriate ductility and toughness, thereby improving the material's coating effect on fertilizer particles. Carbon dioxide is introduced into the present material to synthesize polyether, and the production cost is lower. The main components of the coating material are normally in a liquid state, and are directly mixed and used when coating fertilizer particles, and the production process is simple and easy to use. After coating the fertilizer particles, the shelf life of the fertilizer can be extended, the dissolution and loss of the fertilizer before use can be reduced, and the quality and nutrient content of the fertilizer can be maintained. After use, the coating can be gradually degraded by organisms after a certain period of time, and the fertilizer release rate can be controlled to improve nutrient utilization. The present invention uses degradable polyether and isocyanate components to make controlled-release fertilizer coating materials, thereby reducing the risk of soil and water pollution. DETAILED DESCRIPTION
[0024] The present invention is described in detail below through examples. Unless otherwise specified, the raw materials used are commercially available. The examples of the present invention are only partial performance comparisons of the basic components of the coating material. In actual use, conventional additives such as color paste, chain extender, viscosity reducer, leveling agent, etc. can be further added to the formula to facilitate use or further improve performance, which will not be shown in detail here. In addition, other existing polyether polyols and polyester polyols can also be optionally used according to the use requirements to adjust the viscosity and reactivity of the coating material.
[0025] Example 1
[0026] Preparation of polyether:
[0027] Ethylene glycol, ethylene oxide, phthalic anhydride and catalyst were added to the reactor in a molar ratio of 5:100:10:0.05, wherein the catalyst was a composite catalyst of triethyl boron and tetra-n-butyl ammonium bromide in a molar ratio of 1:1.5, carbon dioxide was charged to 2.0MPa, and the temperature was raised to 45°C for copolymerization for 3.5h. The molar ratio of carbon dioxide consumption to the amount of ethylene oxide or / and propylene oxide input was 70:100. After terminating the reaction, the material was discharged to obtain polyether. The number average molecular weight of the obtained polyether was detected to be 1700. The molar ratio of the polycarbonate segment on the molecular chain of the polyether was 70%, the molar ratio of the polyester segment was 10%, and the molar ratio of the polyether segment was 20%.
[0028] Fertilizer Forming:
[0029] 1) Dehydrate the obtained polyether and TDI to make the moisture content less than 0.1%; prepare the materials in a mass ratio of 1:0.3 and mix them to form a coating material;
[0030] 2) Add the coating material and fertilizer into the coating machine at a mass ratio of 1:45, control the temperature in the coating machine at 50°C and rotate and stir to solidify the coating material on the surface of the fertilizer, and cool to obtain.
[0031] Example 2
[0032] Preparation of polyether: Ethylene glycol, propylene oxide, phthalic anhydride and catalyst are added to the reactor in a molar ratio of 5:100:10:0.05, wherein the catalyst is a composite catalyst of triethyl boron and tetra-n-butyl ammonium bromide in a molar ratio of 1:1.7, carbon dioxide is charged to 2.0MPa, and the temperature is raised to 50°C for copolymerization for 4h. The molar ratio of carbon dioxide consumption to propylene oxide input is 50:100. After terminating the reaction, the material is discharged to obtain polyether. The number average molecular weight of the obtained polyether is detected to be 1500. By nuclear magnetic resonance detection, the molar ratio of the polycarbonate segment on the molecular chain of the polyether is 50%, the molar ratio of the polyester segment is 10%, and the molar ratio of the polyether segment is 40%.
[0033] The fertilizer forming process is the same as that in Example 1.
[0034] Example 3
[0035] Preparation of polyether: Ethylene glycol / glycerol, propylene oxide and catalyst are added to the reactor in a molar ratio of 5:100:0.03, wherein the catalyst is a compound catalyst of tributyl boron and tetra-n-butyl ammonium chloride in a molar ratio of 1:1.3, carbon dioxide is charged to 3.5MPa, and the temperature is raised to 40°C for copolymerization for 3.5h. The molar ratio of carbon dioxide consumption to the total amount of ethylene oxide and propylene oxide input is 95:100. After terminating the reaction, the material is discharged to obtain polyether. The number average molecular weight of the obtained polyether is detected to be 1300. The molar ratio of the polycarbonate segment on the molecular chain of the polyether is detected by nuclear magnetic resonance to be 95%, and the molar ratio of the polyether segment is 5%.
[0036] The fertilizer forming process is the same as that in Example 1.
[0037] Example 4
[0038] Fertilizer molding: 1) dehydrating the polyether and IPDI obtained in Example 1 to reduce the moisture content to less than 0.1%; preparing the materials in a mass ratio of 1:0.5 and mixing them to form a coating material;
[0039] 2) Add the coating material and fertilizer into the coating machine at a mass ratio of 1:40, control the temperature in the coating machine at 45°C and rotate and stir to solidify the coating material on the surface of the fertilizer, and cool to obtain.
[0040] Example 5
[0041] Fertilizer molding: 1) dehydrating the polyether and MDI obtained in Example 1 to reduce the moisture content to less than 0.1%; preparing the materials in a mass ratio of 1:0.1 and mixing them to form a coating material;
[0042] 2) Add the coating material and fertilizer into the coating machine at a mass ratio of 1:50, control the temperature in the coating machine at 45°C and rotate and stir to solidify the coating material on the surface of the fertilizer, and cool to obtain.
[0043] Example 6
[0044] Preparation of polyether: glycerol, propylene oxide, phthalic anhydride and catalyst are added to the reactor in a molar ratio of 12:100:20:0.05, wherein the catalyst is a composite catalyst of triethyl boron and tetra-n-butyl ammonium bromide in a molar ratio of 1:1.5, carbon dioxide is charged to 2.0MPa, the temperature is raised to 40°C for copolymerization for 4h, and the molar ratio of carbon dioxide consumption to propylene oxide input is 60:100. After terminating the reaction, the material is discharged to obtain polyether. The number average molecular weight of the obtained polyether is detected to be 300. The molar ratio of the polycarbonate segment on the molecular chain of the polyether is 60%, the molar ratio of the polyester segment is 20%, and the molar ratio of the polyether segment is 20%.
[0045] The fertilizer forming process is the same as that in Example 1.
[0046] Example 7
[0047] Preparation of polyether: glycerol, ethylene oxide, phthalic anhydride and catalyst are added to the reactor in a molar ratio of 2:100:30:0.05, wherein the catalyst is a composite catalyst of triethyl boron and tetra-n-butyl ammonium bromide in a molar ratio of 1:1.5, carbon dioxide is charged to 0.15MPa, the temperature is raised to 65°C for copolymerization for 4h, and the molar ratio of carbon dioxide consumption to propylene oxide input is 5:100. After terminating the reaction, the material is discharged to obtain polyether. The number average molecular weight of the obtained polyether is detected to be 5000. By nuclear magnetic resonance detection, the molar ratio of the polycarbonate segment on the molecular chain of the polyether is 5%, the molar ratio of the polyester segment is 30%, and the molar ratio of the polyether segment is 65%.
[0048] The fertilizer forming process is the same as that in Example 1.
[0049] Example 8
[0050] Fertilizer molding: 1) dehydrating the polyether and IPDI obtained in Example 1 to reduce the moisture content to less than 0.1%; preparing the materials in a mass ratio of 1:0.3 and mixing them to form a coating material;
[0051] 2) Add the coating material and fertilizer into the coating machine at a mass ratio of 1:30, control the temperature in the coating machine at 40°C and rotate and stir to solidify the coating material on the surface of the fertilizer, and cool to obtain.
[0052] Example 9
[0053] Fertilizer molding: 1) dehydrating the polyether and MDI obtained in Example 1 to reduce the moisture content to less than 0.1%; preparing the materials in a mass ratio of 1:0.3 and mixing them to form a coating material;
[0054] 2) Add the coating material and fertilizer into the coating machine at a mass ratio of 1:60, control the temperature in the coating machine at 60°C and rotate and stir to solidify the coating material on the surface of the fertilizer, and cool to obtain.
[0055] The results of the performance tests on the controlled-release fertilizers obtained in each embodiment are shown in Table 1, where:
[0056] The puncture strength refers to the puncture strength of the composite fertilizer coating material of each embodiment cast into a film with a thickness of 0.1 mm and tested according to GB / T21302.
[0057] The 24h release rate refers to the cumulative release rate of nutrients in the fertilizer in 24 hours in red soil at 25°C and 25% humidity.
[0058] The 28d release rate refers to the cumulative release rate of nutrients in the fertilizer in red soil at 25°C and 25% humidity after 28 days.
[0059] The 120d release rate refers to the cumulative release rate of nutrients in the fertilizer in red soil at 25°C and 25% humidity after 120 days.
[0060] The sterilization release rate refers to the fertilizer nutrient release rate in sterilized water kept at 38°C for one week.
[0061] The 90-degree peel strength refers to the peel strength value of the coating material obtained in step 1) of the fertilizer molding in each embodiment applied on the stainless steel test plate of the 90-degree peel strength tester, and obtained an adhesion film with a thickness of 0.5 mm after curing.
[0062] Table 1 Performance test results
[0063] .
[0064] It can be seen from Table 1 that the degradable polyurethane coating material prepared in the present invention has good puncture resistance, peeling resistance and controlled release ability.
[0065] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.
Claims
1. A degradable polyurethane controlled-release fertilizer coating material, comprising two components A and B, wherein the component A is polyether and the component B is isocyanate, characterized in that: The polyether is a polyether diol or a polyether polyol, and the molecular chain of the polyether contains random or block polycarbonate segments, the polycarbonate segments are copolymerized by epoxy compounds and carbon dioxide, and the molar ratio of the polycarbonate segments in the molecular chain is 50% to 95%; the number average molecular weight of the polyether is 1300 to 1700; The molecular chain of the polyether contains random or block polyether segments, the molar ratio of the polyether segments in molecular weight is 1% to 40%, and the polyether segments are self-polymerized segments of epoxy compounds; the epoxy compounds are ethylene oxide and / or propylene oxide.
2. A degradable polyurethane controlled-release fertilizer coating material according to claim 1, characterized in that: The mass ratio of the polyether to the isocyanate is 1:0.1-0.
5.
3. A degradable polyurethane controlled-release fertilizer coating material according to claim 1, characterized in that: The isocyanate is TDI, IPDI, MDI, HMDI or HDI.
4. A fertilizer forming process, characterized in that: The following steps are involved: 1) removing water from the raw materials of the two components A and B of the degradable polyurethane controlled-release fertilizer coating material according to any one of claims 1 to 3 to make the moisture content less than 0.1%; and mixing the raw materials into the coating material; 2) Add the coating material and fertilizer into the coating machine at a mass ratio of 1:30~60, control the temperature in the coating machine at 40℃~60℃ and rotate and stir to solidify the coating material on the surface of the fertilizer, and cool to obtain.
5. A fertilizer forming process according to claim 4, characterized in that: The coating material and fertilizer described in step 2) are in a mass ratio of 1:40~50.
6. A fertilizer forming process according to claim 4, characterized in that: The temperature in the coating machine described in step 2) is controlled at 45°C to 55°C.
Citation Information
Patent Citations
Preparation method of fertilizer coated by carbon dioxide-based degradable polymer and product of preparation method
CN110698307A
Carbon dioxide-based polyester polycarbonate diol and preparation method thereof
CN116003759A