A kind of unburned masonry block based on surface layer reinforcement and preparation method thereof

By using surface layer enhancement technology in the fire-free products of residue residue and high-strength cement-based materials and wire mesh layers, the problems of complexity and low performance of residue residue residue are solved, and the efficiency of residue residue residue is achieved Resource utilization and performance improvement.

CN118582008BActive Publication Date: 2024-11-29GUANGZHOU METRO DESIGN & RES INST CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411066715.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-29
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The existing waste residue sludge-free fired products have complex processing, low performance, low utilization rate, and low cost advantages, making it difficult to absorb large amounts of construction waste and be used in engineering applications.

Method used

Using a surface layer reinforcement method, cement blocks are made using residue mud, cement and water as raw materials, and the outer layer is covered with cement-based high-strength materials, including ordinary concrete, high-strength concrete or fiber-reinforced ultra-high performance concrete, combined with steel wire The mesh layer reduces the amount of cement and improves the resource utilization of residue residue.

Benefits of technology

Improve the compressive strength and durability of the burn-free masonry block of residue residue sludge, reduce costs, realize the resource utilization of residue residue sludge with a high proportion, solve the problems of residue residue sludge and pollution, and improve the materials physical performance and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118582008B_ABST
    Figure CN118582008B_ABST
Patent Text Reader

Abstract

This invention discloses a surface-reinforced, non-fired masonry block and its preparation method. The surface-reinforced, non-fired masonry block comprises a cement-soil block and a cement-based reinforcing layer. The raw materials for the cement-soil block include waste soil, cement, and water. Waste soil, a small amount of cement, and water are mixed to obtain a mixture, which is then placed in a mold, pressed under pressure, and naturally cured to obtain the cement-soil block. A cement-based reinforcing layer of a certain thickness is applied to the outer layer of the cement-soil block. The non-fired masonry block prepared by this invention possesses excellent physical properties, high strength, good durability, low cost, low carbon emissions, and high utilization rate of waste soil and mud. The cement-soil block in this invention serves as the internal filling material, with low requirements for strength and performance, achieving efficient resource utilization of solid waste; the outer cement and reinforcing layer significantly improve the strength, wear resistance, impact resistance, and impermeability of the masonry block, enhancing its usability and durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of environmentally friendly building materials, and in particular to a surface layer-reinforced unfired masonry block and a preparation method thereof. Background Art

[0002] Sludge refers to the excess soil generated during various construction projects, and is one of the main wastes of urban infrastructure projects. At present, the transfer, stacking or landfill of sludge generated by most projects will not only occupy a large amount of space and land resources, but also cause a lot of pollution to the environment. The stacking of sludge in the collection site also has certain safety hazards. Therefore, recycling sludge as building materials can not only solve the disposal problem of large-scale sludge and other construction solid wastes, but also save a lot of natural resources and reduce construction costs.

[0003] At present, many scholars have also conducted research on the reuse of slag mud. Chinese patent document CN116535154A "A high-strength tunnel slag mud brick and its preparation method" discloses that high-strength slag mud bricks are prepared by one-time pressing and molding using tunnel slag mud, cement, water and fiber as raw materials. However, in the process of research and analysis on the recycling of slag mud, most of the products formed by slag mud itself as raw materials have the following problems: (1) The material processing and preparation process is complicated, the preparation and maintenance have high requirements for equipment, and the production efficiency is low; (2) The performance of slag unburned products is relatively low, and the scope of use and application scenarios are limited; (3) The utilization rate of slag mud is low, and it is difficult to dispose of large amounts of slag mud and other construction waste; (4) In the process of making slag unburned products, it is necessary to add coarse and fine aggregates, cementitious materials and composite additives with appropriate grading, and the cost advantage is not obvious. The above problems make the current slag unburned products unable to absorb a large amount of slag mud, and difficult to use in engineering practice and promotion and application. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention aims to provide a surface-reinforced unfired masonry block and a preparation method thereof, wherein a cement-soil block is made from slag mud, cement and water as raw materials, and a certain thickness of cement-based high-strength material is covered on the outer layer. There is no need to add too much cement and admixtures, thereby reducing costs, achieving a high proportion of resource utilization of slag mud, and improving the physical properties of slag mud unfired products.

[0005] To achieve the above object, the present invention adopts the following technical solution:

[0006] A surface-reinforced unfired masonry block comprises a cement soil block and a cement-based reinforcement layer, wherein the raw materials of the cement soil block comprise waste soil, cement and water, the cement-based reinforcement layer is coated on the outer surface of the cement soil block, the material of the cement-based reinforcement layer comprises ordinary concrete, high-strength concrete, fiber-reinforced ultra-high performance concrete or engineering cement-based composite materials, and a wire mesh layer is provided between the cement-based reinforcement layer and the cement soil block.

[0007] Furthermore, the waste soil includes slag mud, waste slag, furnace slag, brick slag, garbage incineration bottom ash or construction waste.

[0008] Furthermore, the raw material components of the cement soil block are set as follows:

[0009] In terms of mass, the waste soil is 25-60 parts, the cement is 1-5 parts, and the water is 3-15 parts.

[0010] Furthermore, the outer surface of the cement soil block is a rough surface with uneven surfaces, and is closely fitted with the inner surface of the cement-based reinforcement layer.

[0011] Furthermore, a grouting material layer is added to the surface of the cement soil block, and the cement-based reinforcement layer includes a cement-based reinforcement layer permanent mold wrapping the side and bottom surfaces of the cement soil block and a mortar layer covering the top surface of the cement soil block.

[0012] Furthermore, the thickness ratio of the cement-based reinforcing layer to the cement soil block in the height direction is 0.08-0.2; the thickness ratio of the cement-based reinforcing layer to the cement soil block in the length and width directions of the rectangular unfired masonry block is 0.1-0.3; the thickness ratio of the cement-based reinforcing layer to the cement soil block in the diameter direction of the cylindrical unfired masonry block is 0.12-0.3.

[0013] Further, the following steps are included:

[0014] S1: drying the waste soil, crushing the dried waste soil, sieving it through a sieve to obtain waste soil with a particle size of less than 5 mm, stirring and mixing cement and water, and then mixing the cement with the sieved waste soil to obtain a mixture;

[0015] S2: pressing the mixture into a shape at a pressure greater than 10 MPa, and then subjecting the mixture to natural curing to obtain a cement soil block;

[0016] S3: Laying wire mesh on the surface of cement soil block;

[0017] S4: applying a cement-based reinforcement layer of a certain thickness on the outer layer of the cement soil block.

[0018] Furthermore, when the thickness of the cement-based reinforcement layer is greater than 6 cm, the method for applying the cement-based reinforcement layer is as follows:

[0019] S301: Positioning and placing the formwork and the cement soil block: installing the mold to form a mold groove consisting of a side mold and a bottom mold, first placing a cushion block with the same thickness as the cement-based reinforcement layer into the mold groove, and then placing the cement soil block into the mold groove, using the cushion block to position the cement soil block, ensuring that the gap between the cement soil block and the mold groove template is not less than the thickness requirement of the cement-based reinforcement layer;

[0020] S302: pouring the cement-based reinforcement layer: mixing the concrete material for forming the cement-based reinforcement layer evenly and pouring it into the gap between the cement block and the mold groove, and vibrating it with a vibrating rod so that the concrete material fully fills the gap and the cement-based reinforcement layer on the upper surface of the cement block reaches a set thickness;

[0021] S303: watering, covering and naturally curing the poured cement-based reinforcement layer;

[0022] S304: after reaching the curing age, removing the mold to obtain the fire-free masonry block based on surface layer reinforcement;

[0023] When the thickness of the cement-based reinforcement layer is 3 cm to 6 cm, the construction method of the cement-based reinforcement layer is as follows:

[0024] S311: supporting the mold and setting the cushion block: installing the mold to form the mold groove composed of the side mold and the bottom mold, and placing the cushion block into the mold groove;

[0025] S312: Adding self-compacting concrete material: pouring self-compacting concrete having the same volume as the cement-based reinforcement layer into the mold groove;

[0026] S313: Placing and pressing the cement soil block: placing the cement soil block in the center of the mold groove and pressing the self-compacting concrete into the mold groove, the self-compacting concrete is forced to fill the gap between the cement soil block and the mold groove and cover the surface of the cement soil block, forming the cement-based reinforcement layer wrapped around the surface of the cement soil block;

[0027] S314: watering, coating and naturally curing the cement-based reinforcement layer;

[0028] S315: after reaching the curing age, removing the formwork to obtain the fire-free masonry blocks based on surface layer reinforcement;

[0029] When the thickness of the cement-based reinforcement layer is less than 3 cm, the construction method of the cement-based reinforcement layer is as follows:

[0030] S321: supporting formwork and setting cushion blocks, setting grouting holes: installing the mold to form the mold groove consisting of a side mold and a bottom mold, placing the cushion blocks into the mold groove, and setting the grouting holes at the bottom of the side of the mold groove;

[0031] S322: placing the cement soil block, placing the cement soil block into the mold groove and positioning the cement soil block, ensuring that the gap between the cement soil block and the template of the mold groove is not less than the thickness requirement of the cement-based reinforcement layer;

[0032] S323: Grouting the cement-based reinforcement layer: preparing the cement-based reinforcement layer material into a grouting liquid, injecting the grouting liquid from the grouting hole, so that the grouting liquid fills the gap between the mold groove and the cement soil block and covers the surface of the cement soil block to form the cement-based reinforcement layer, and the cement-based reinforcement layer reaches a set thickness;

[0033] S324: watering, covering and naturally curing the cement-based reinforcement layer;

[0034] S325: After the curing age is reached, the mold is removed to obtain the fire-free masonry blocks based on the surface layer reinforcement.

[0035] Furthermore, the construction method of the cement-based reinforcement layer is:

[0036] S331: Formwork: using the cement-based reinforcement layer material to make an integral shell with a certain thickness as a permanent mold for the cement-based reinforcement layer, and setting grouting holes at the bottom of the permanent mold for the cement-based reinforcement layer;

[0037] S332: placing the cement soil block: placing the prepared cement soil block into the permanent mold of the cement-based reinforcement layer, positioning it with a pad consistent with the material of the cement-based reinforcement layer, and ensuring that the gap between the cement soil block and each part of the permanent mold of the cement-based reinforcement layer is not less than the thickness requirement of the cement-based reinforcement layer;

[0038] S333: grouting of the connection layer: the cement-based reinforcement surface material is made into a grouting liquid, and the grouting liquid is injected from the grouting hole so that the grouting liquid fills the gap between the permanent mold of the cement-based reinforcement layer and the cement soil block;

[0039] S334: The upper surface layer of the cement soil block is filled and smoothed with a mortar layer material, wherein the mortar layer material includes high-strength mortar, concrete or high-ductility cement-based composite material;

[0040] S335: After reaching the curing age, the fire-free masonry blocks based on surface layer reinforcement are obtained.

[0041] The beneficial effects of the present invention are:

[0042] (1) The present invention makes full use of the excellent strength and durability of the outer cement-based reinforcing material to closely wrap and constrain the slag mud cement blocks with relatively poor internal mechanical properties, greatly improving the compressive strength and durability of the entire slag mud unfired masonry block, and providing a new way for the resource utilization of slag mud. The outer layer of concrete can effectively isolate the adverse effects of the external environment on the cement blocks, prevent the cement blocks from absorbing water and softening, and improve the physical properties of the slag mud unfired masonry blocks, so that they can be reused as building materials.

[0043] (2) The present invention has a high utilization rate of slag, can quickly consume slag, has a high utilization rate of slag mud, recycles slag mud, improves the problem of slag land storage and pollution, and realizes sustainable utilization of resources.

[0044] (3) The internal blocks in the fire-free masonry blocks of the present invention do not have high requirements on strength and performance, and can achieve efficient resource utilization of solid waste. It has strong versatility and can be prepared from solid waste such as waste slag, furnace slag, brick slag, garbage incineration bottom ash, and construction waste.

[0045] (4) The process and formula of the present invention are simple, the material processing and preparation process are simple, the preparation and maintenance have low equipment requirements, the production efficiency is high, and the operability is high.

[0046] (5) In the process of making the unburned soil masonry blocks, the present invention does not need to add materials such as coarse and fine aggregates with appropriate grading, cementitious materials and composite additives, so the amount of cement used in the unburned soil masonry blocks is small and the cost is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0048] Figure 1 It is a schematic diagram of the steps of realizing the external reinforcement layer by using the formwork cast-in-place method of the present invention;

[0049] Figure 2 It is a schematic diagram of the steps of realizing the external reinforcement layer by adopting the self-compacting method of formwork in the present invention;

[0050] Figure 3 It is a schematic diagram of the steps of implementing the external reinforcement layer by formwork grouting in the present invention;

[0051] Figure 4 It is a schematic diagram of the steps of realizing the external reinforcement layer by using the permanent formwork grouting method of the present invention;

[0052] Figure 5It is a schematic diagram of the structure of the fire-free masonry block composed of a cement-based reinforcement layer and cement soil blocks of the present invention;

[0053] Figure 6 It is a schematic diagram of the structure of the fire-free masonry block composed of a cement-based reinforcement layer, a steel wire mesh, and a cement soil block of the present invention;

[0054] Figure 7 It is a schematic diagram of the structure of the unfired masonry block composed of a cement-based reinforcement layer permanent mold (shell), a mortar layer, a filling layer, and cement soil blocks of the present invention;

[0055] Figure 8 It is a schematic diagram of the structure of the fire-free masonry block composed of a cement-based reinforcement layer mortar layer permanent template (shell), a mortar layer, a steel wire mesh, a filling layer, and cement soil blocks;

[0056] Fig. 9 is a preparation flow chart of an embodiment of the present invention, wherein (a) is a cement soil block, (b) is an externally poured cement-based reinforcement layer, and (c) is a fire-free masonry block containing a cement-based reinforcement layer;

[0057] Fig.10 is the pressure-resistance displacement curve of the cement-soil block after the cement-based reinforcement layer is poured externally in the embodiment of the present invention;

[0058] Fig.11 is a compression displacement curve of a cement soil block without a cement-based reinforcement layer according to an embodiment of the present invention;

[0059] Fig.12 is a comparison diagram of the pressure-displacement curves of cement-soil blocks with and without cement-based reinforcement layers according to an embodiment of the present invention;

[0060] Fig.13 It represents the thickness ratio of the cement-based reinforcement layer and the cement soil block in the height direction of the fire-free masonry block of the embodiment of the present invention;

[0061] Fig.14 It represents the thickness ratio of the cement-based reinforcement layer and the cement soil block in the length direction and the width direction of the rectangular unfired masonry block of the embodiment of the present invention;

[0062] Fig.15 It represents the thickness ratio of the cement-based reinforcement layer and the cement soil block in the diameter direction of the cylindrical unfired masonry block of the embodiment of the present invention.

[0063] Reference numerals

[0064] 1. Cement soil block; 2. Cement-based reinforcement layer; 21. Permanent mold for cement-based reinforcement layer; 3. Wire mesh layer; 4. Grouting material layer; 5. Mortar layer; 6. Grouting hole. DETAILED DESCRIPTION

[0065] Below in conjunction with accompanying drawing, preferred embodiment of the present invention is described.It should be understood that the preferred embodiment described herein is only used to illustrate and explain the present invention, and is not intended to limit the present invention.The reagents, methods and equipment described in the following examples are all adopted existing reagents, methods and equipment unless otherwise specified.

[0066] The invention discloses a non-fired masonry block based on surface layer reinforcement and a preparation method thereof. The non-fired masonry block based on surface layer reinforcement includes a cement soil block and a cement-based reinforcement layer. The raw materials of the cement soil block include waste soil, cement and water. The waste soil, a small amount of cement, hydration and stirring are used to obtain a mixture, which is loaded into a mold, pressed and formed by pressure, and then naturally cured to obtain a cement soil block. A cement-based reinforcement layer of a certain thickness is applied to the outer layer of the cement soil block. The non-fired masonry block prepared by the present invention has excellent physical properties, high strength, good durability, low cost, low carbon emissions, and a large utilization rate of slag and residual mud. The cement soil block in the non-fired masonry block of the present invention is used as an internal filling material, and the strength and performance requirements are not high, so that efficient resource utilization of solid waste is realized; the outer cement and the reinforcement layer can significantly improve the strength, wear resistance, impact resistance and penetration resistance of the masonry block and its durability.

[0067] 1. The composition of the fire-free masonry block of the present invention is as follows:

[0068] The slag mud unburned masonry block based on surface layer reinforcement includes a cement soil block 1 and a cement-based reinforcement layer 2.

[0069] The raw materials of cement soil block 1 include slag mud, cement and water. Take 25 parts of slag mud, 1 part of cement and 3-4 parts of water.

[0070] The slag mud can be replaced by waste slag, furnace slag, brick slag, garbage incineration bottom slag, construction waste and other solid waste preparation

[0071] The particle size of the slag and residual mud is 2~5mm.

[0072] The cement-based reinforcement layer 2 material can be high-performance cement-based materials such as ordinary concrete, high-strength concrete, fiber-reinforced ultra-high performance concrete (UHPC) and engineered cement-based composite materials (ECC).

[0073] 2. The specific preparation method of the fire-free masonry block of the present invention is as follows:

[0074] Step 1: Take 25 parts of slag mud, 1 part of cement, and 3-4 parts of water, air-dry the slag mud naturally, then dry it, sieve the dried slag mud through a drying net to obtain slag mud with a particle size of less than 5 mm, stir and mix the cement and water, and then mix them with the sieved slag mud to obtain a mixture;

[0075] Step 2: The mixture is pressed into shape and then naturally cured to obtain a cement soil block 1; the mixture can be pressed into shape by hydraulic pressure, and the molding pressure is not less than 10MPa; it can also be formed by static pressure, the mixture is placed in a steel mold, covered with a cover and pressure is applied, and the molding pressure is not less than 10MPa.

[0076] A rough and concave surface is constructed on the surface of the cement soil block 1 to improve the connection surface and bite force between the cement soil block 1 and the cement-based reinforcement layer 2.

[0077] Step 3: Apply a cement-based reinforcement layer 2 of a certain thickness on the outer layer of the cement soil block 1.

[0078] The cement-based reinforcement layer 2 can be implemented by cast-in-place method, self-compacting method, grouting method or permanent formwork grouting method, and a steel mesh can be added on the surface of the cement block 1 or the grouting material layer 4 to further improve the crack resistance and strength of the cement-based reinforcement layer 2. The specific application method is as follows:

[0079] Method 1: If Figure 1 As shown, when the thickness of the cement-based reinforcement layer 2 is greater than 6 cm, the implementation method of the cement-based reinforcement layer 2 can adopt a formwork cast-in-place method, and the steps are as follows:

[0080] S301: Formwork and cement soil block 1 are placed in position. The prepared cement soil block 1 is placed in a mold, preferably a reusable metal mold, and positioned using a pad made of the same material as the cement-based reinforcement layer 2 to ensure that the thickness of the cement-based reinforcement layer 2 meets the requirements. The volume of the positioning pad is as small as possible and the surface is rough, so that it has a high connection strength with the cement-based reinforcement layer 2 (the interface between the new and old materials).

[0081] S302: Casting of cement-based reinforcement layer 2. The concrete of cement-based reinforcement layer 2 is evenly mixed and poured into the gap between cement soil block 1 and steel mold, and vibrated with a vibrating rod to make the concrete fully fill the gap and the cement-based reinforcement layer 2 reaches a set thickness.

[0082] S303: watering, covering and naturally curing the cement-based reinforcement layer 2;

[0083] S304: After reaching the curing age, the mold is removed to obtain the unfired masonry blocks.

[0084] Method 2: If Figure 2 As shown, when the thickness of the cement-based reinforcement layer 2 is between 3 cm and 6 cm, the implementation method of the cement-based reinforcement layer 2 can be implemented in a solid manner, and the steps are as follows:

[0085] S311: Support the mold and set the positioning blocks. Install the mold and place the positioning blocks.

[0086] S312: Adding self-compacting concrete material: Pour a certain volume (the volume of the cement-based reinforcement layer 2) of self-compacting concrete into the mold.

[0087] S313: Place and press in the cement soil block 1 (solid waste) block. The cement soil block 1 (solid waste) block is placed in the center of the mold and pressed into the self-compacting concrete, and the self-compacting concrete rises to fill the gaps and the surface layer to form an outer sheath.

[0088] S314: watering, covering and naturally curing the poured cement-based reinforcement layer 2;

[0089] S315: After reaching the curing age, the mold is removed to obtain the unfired masonry blocks.

[0090] Method 3: When the thickness of the cement-based reinforcement layer 2 is less than 3 cm, the implementation method of the cement-based reinforcement layer 2 can adopt the method of formwork grouting, and the steps are as follows:

[0091] S321: Support the formwork and set the positioning blocks. Install the formwork, place the positioning blocks, and set the grouting holes at the bottom of the formwork.

[0092] S322: Putting in cement soil block 1. Putting the cement soil block 1 (solid waste) into the mold and positioning it to ensure that the gaps between the parts meet the requirements of the thickness of the reinforcement layer;

[0093] S323: Grouting of the reinforcement layer. Add an appropriate amount of water to the grouting mixture and stir to form a grouting liquid, and inject the grouting liquid from the grouting hole 6 at the bottom of the mold so that the grouting material fills the gaps and covers the surface of the cement soil block 1 to reach a set thickness;

[0094] S324: watering, covering and naturally curing the poured cement-based reinforcement layer 2;

[0095] S325: After reaching the curing age, the mold is removed to obtain the unfired masonry blocks.

[0096] The fire-free masonry block structure obtained by the above scheme is as follows Figure 5 shown.

[0097] As a preferred embodiment of the present invention, the above-mentioned method 1, method 2, and method 3 can add a steel wire mesh between the cement-based reinforcement layer and the cement soil block to further improve the crack resistance and strength of the external cement-based reinforcement material layer. Figure 6 shown.

[0098] Method 4: The implementation method of the cement-based reinforcement layer 2 can be implemented by grouting the cement-based reinforcement layer permanent mold 21, and the steps are as follows:

[0099] S331: Formwork. A cement-based reinforced layer permanent mold 21 made of cement-based reinforced layer 2 material, or an integral shell with a certain thickness made of cement-based reinforced layer 2 material is used as a mold, and a grouting hole 6 is set at the bottom of the mold;

[0100] S332: Put in cement soil block 1. Put the prepared cement soil block 1 (solid waste) into the mold, and use the pads that are consistent with the material of the cement-based reinforcement layer 2 to position it, so as to ensure that the thickness of the cast cement-based reinforcement layer 2 reaches the requirement. The volume of the positioning pad is as small as possible, and the surface is rough, so that it has a high connection strength with the cement-based reinforcement layer 2 (the interface between the new and old materials).

[0101] S333: Grouting of the connection layer. Add an appropriate amount of water to the grouting mixture and stir to form a grouting liquid, and inject the grouting liquid from the grouting hole 6 at the bottom of the mold so that the grouting material fills the gap between the template and the cement soil block 1;

[0102] Before the implementation of the cement-based reinforcement layer 2, the pad used to support and position the cement soil block 1 in the mold is made of the same material as the cement-based reinforcement layer 2 or a material with performance not lower than that of the cement-based reinforcement layer 2, and is prepared into a smaller pad with a rough surface, so that the connection between the pad and the post-cast cement-based reinforcement layer 2 or the grouting material is tight and reliable.

[0103] S334: The upper surface layer of the cement soil block 1 is filled and smoothed with high-strength cement-based materials (high-strength mortar, concrete, UHPC, ECC, etc.).

[0104] S335: After reaching the curing age, the mold is removed to obtain the unfired masonry block product, and its product structure is as follows Figure 7 shown.

[0105] As a preferred embodiment of the present invention, the fourth method can add a steel mesh to the grouting material layer to further improve the crack resistance and strength of the cement-based reinforcement layer 2. Figure 8 shown.

[0106] 3. Performance test of the present invention on slag unburned bricks:

[0107] (1) Compressive strength

[0108] Testing equipment: microcomputer electro-hydraulic servo universal testing machine, hydraulic testing machine

[0109] Test method: The compressive strength R of the cylindrical sample is tested in accordance with GB / T2810-2016 "Test Methods for Ceramic Tiles" using a universal electronic press. The compressive strength test method for unfired masonry blocks is tested in accordance with the compressive strength test method specified in GB / T2542-2012 "Test Methods for Wall Bricks". The two halves of the brick formed after the middle fracture are stacked together with the fracture facing outwards, and the specimen is placed on the pressure plate of the testing machine so that the central axis of the specimen coincides with the pressure center of the pressure plate of the testing machine. Then, the load is slowly applied at a speed of 10kN / s-30kN / s until the specimen is destroyed. The maximum failure load P is recorded. The compressive strength of each specimen is calculated according to formula (1) with an accuracy of 0.1MPa.

[0110] Formula (1)

[0111] Where: R is the compressive strength of the specimen, MPa;

[0112] P-failure load, N;

[0113] L is the length of the pressure surface, mm;

[0114] B is the width of the pressure surface, mm.

[0115] IV. Related instructions

[0116] The unfired masonry blocks provided by the present invention are mainly used in application scenarios under compression, such as wall bricks and blocks, pavement bricks, curbstones, retaining slope masonry blocks, etc. Their shape, volume, inner layer material, reinforcement layer material and specific requirements are shown in the following table.

[0117] (1) The shape and volume of the unfired masonry blocks of the present invention are listed in Table 1:

[0118] Table 1 Shape and volume of unfired masonry blocks

[0119]

[0120] (2) The composition, moisture content and molding pressure of the internal block material of the present invention are listed in Table 2:

[0121] Table 2 Material composition, moisture content and molding pressure of cement soil blocks

[0122]

[0123] (3) The thickness comparison between the cement-based reinforcement layer of the unfired masonry block and the cement-soil block is shown in Table 3:

[0124] Table 3 Thickness comparison of cement-based reinforcement layer and cement soil block ( Figure 13-Figure 15 )

[0125]

[0126] The thickness ratio of the cement-based reinforcing layer of the unfired masonry block to the cement-soil block in the height direction is 0.08-0.2; the thickness ratio of the cement-based reinforcing layer of the rectangular unfired masonry block to the cement-soil block in the length and width directions is 0.1-0.3; the thickness ratio of the cement-based reinforcing layer of the cylindrical unfired masonry block to the cement-soil block in the diameter direction is 0.12-0.3.

[0127] 5. Experimental setup:

[0128] Embodiment 1:

[0129] like Fig. 9 As shown, this embodiment provides a non-fired masonry block based on surface layer reinforcement, which is made of slag mud, cement and water as raw materials to form a cement soil block, and a cement-based reinforcement layer 2 of a certain thickness is covered on its outer layer. The cement content in the cement soil block 1 is 5% and the water content is 13%. The material of the cement-based reinforcement layer 2 is ordinary C30 concrete. The non-fired masonry block in this experimental example is a standard solid brick, and the thickness of the cement-based reinforcement layer 2 is 25mm.

[0130] The specific preparation process is as follows:

[0131] Step 1: Calculate by mass, take 25 parts of slag mud, 1 part of cement, and 3-4 parts of water, air-dry the slag mud naturally, then dry it, sieve the dried slag mud through a drying net to obtain slag mud with a particle size of less than 5 mm, stir and mix the cement and water, and then mix them with the sieved slag mud to obtain a mixture;

[0132] Step 2: The mixture is pressed into shape and then naturally cured to obtain a cement soil block 1; the mixture is pressed into shape by hydraulic pressure, and the molding pressure is 10 MPa;

[0133] Step 3: Using method 1, a cement-based reinforcement layer 2 of a certain thickness is applied to the outer layer of the cement soil block 1.

[0134] The cement soil block 1 obtained in step 2 of Example 1 and the cement soil block after pouring the cement-based reinforcement layer obtained in step 3 of Example 1 were subjected to compression tests. The test results are as follows: Figure 10-12 .

[0135] Test conclusion: The compressive strength of cement-soil blocks with cement-based reinforcement layers is significantly stronger than that of cement-soil blocks without cement-based reinforcement layers.

[0136] Therefore, the unfired masonry blocks of the present invention use materials such as construction waste as raw materials, and do not need to be mixed with too much cement and admixtures, thereby reducing costs, realizing resource utilization of waste mud, and improving the tensile strength of the unfired masonry blocks.

[0137] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein with equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a fire-free masonry block based on surface layer reinforcement, characterized in that: The following steps are involved: S1: drying the waste soil, crushing the dried waste soil, and screening it through a sieve to obtain waste soil with a particle size of less than 5 mm, mixing cement and water, and then mixing the cement with the screened waste soil to obtain a mixture; S2: pressing the mixture into a shape at a pressure greater than 10 MPa, and then subjecting the mixture to natural curing to obtain a cement soil block (1); S3: Laying wire mesh on the surface of cement soil blocks; S4: applying a cement-based reinforcement layer (2) of a certain thickness on the outer layer of the cement soil block (1); When the thickness of the cement-based reinforcement layer (2) is greater than 6 cm, the method for applying the cement-based reinforcement layer (2) is as follows: S301: Positioning and placing the formwork and the cement soil block (1): Installing the mold to form a mold groove consisting of a side formwork and a bottom formwork, first placing a pad having the same thickness as the cement-based reinforcement layer (2) into the mold groove, then placing the cement soil block (1) into the mold groove, and using the pad to position the cement soil block (1), ensuring that the gap between the cement soil block (1) and the formwork of the mold groove is not less than the thickness requirement of the cement-based reinforcement layer (2); S302: pouring the cement-based reinforcement layer (2): mixing the concrete material for forming the cement-based reinforcement layer (2) evenly and pouring it into the gap between the cement block (1) and the mold groove, and vibrating it with a vibrating rod so that the concrete material fully fills the gap and the cement-based reinforcement layer (2) on the upper surface of the cement block (1) reaches a set thickness; S303: watering, covering and naturally curing the poured cement-based reinforcement layer (2); S304: After the curing age is reached, the formwork is removed to obtain the surface layer-reinforced, non-fired masonry blocks; When the thickness of the cement-based reinforcement layer (2) is 3 cm to 6 cm, the construction method of the cement-based reinforcement layer (2) is as follows: S311: Supporting the mold and setting the cushion block: Installing the mold to form the mold groove consisting of the side mold plate and the bottom mold plate, and placing the cushion block into the mold groove; S312: Adding self-compacting concrete material: pouring self-compacting concrete into the mold groove in an amount that is consistent with the volume of the cement-based reinforcement layer (2); S313: placing and pressing the cement soil block (1): placing the cement soil block (1) in the center of the mold groove and pressing the self-compacting concrete into it, so that the self-compacting concrete is forced to fill the gap between the cement soil block (1) and the mold groove and cover the surface of the cement soil block (1), forming the cement-based reinforcement layer (2) wrapped around the surface of the cement soil block (1); S314: watering, covering and naturally curing the cement-based reinforcement layer (2); S315: After the curing age is reached, the formwork is removed to obtain the surface layer-reinforced, fire-free masonry blocks; When the thickness of the cement-based reinforcement layer (2) is less than 3 cm, the construction method of the cement-based reinforcement layer (2) is as follows: S321: supporting the formwork and setting the pads, setting the grouting holes (6): installing the mold to form the mold groove consisting of the side mold and the bottom mold, placing the pads into the mold groove, and setting the grouting holes (6) on the bottom of the side of the mold groove; S322: placing the cement soil block (1), placing the cement soil block (1) into the mold groove and positioning the cement soil block (1), ensuring that the gap between the cement soil block (1) and the template of the mold groove is not less than the thickness requirement of the cement-based reinforcement layer (2); S323: Grouting the cement-based reinforcement layer (2): preparing the cement-based reinforcement layer (2) material into a grouting liquid, injecting the grouting liquid into the grouting hole (6), so that the grouting liquid fills the gap between the mold groove and the cement soil block (1) and covers the surface of the cement soil block (1) to form the cement-based reinforcement layer (2), and making the cement-based reinforcement layer (2) reach a set thickness; S324: watering, covering and naturally curing the cement-based reinforcement layer (2); S325: After reaching the curing age, the formwork is removed to obtain the fire-free masonry blocks based on the surface layer reinforcement.

2. The method for preparing a surface-reinforced unburned masonry block according to claim 1, characterized in that: The construction method of the cement-based reinforcement layer (2) is: S331: Formwork: using the cement-based reinforcement layer (2) material to make an integral shell having a certain thickness as a cement-based reinforcement layer permanent mold (21), and providing a grouting hole (6) at the lower part of the cement-based reinforcement layer permanent mold (21); S332: placing the cement soil block (1): placing the prepared cement soil block (1) into the cement-based reinforcement layer permanent mold (21), positioning it with a spacer made of the same material as the cement-based reinforcement layer (2), ensuring that the gap between the cement soil block (1) and each part of the cement-based reinforcement layer permanent mold (21) is not less than the thickness requirement of the cement-based reinforcement layer (2); S333: grouting the connection layer: the material of the cement-based reinforcement layer (2) is made into a grouting liquid, and the grouting liquid is injected from the grouting hole (6) so that the grouting liquid fills the gap between the cement-based reinforcement layer permanent mold (21) and the cement soil block (1); S334: The upper surface layer of the cement soil block (1) is filled and smoothed with a mortar layer (5) material, wherein the mortar layer (5) material is one or more of high-strength mortar, concrete, or high-ductility cement-based composite materials; S335: After reaching the curing age, the fire-free masonry blocks based on surface layer reinforcement are obtained.

3. A surface-reinforced, fire-free masonry block according to any one of claims 1 or 2, characterized in that: The invention comprises a cement block (1) and a cement-based reinforcement layer (2), wherein the raw materials of the cement block (1) include waste soil, cement and water, the cement-based reinforcement layer (2) is coated on the outer surface of the cement block (1), and the material of the cement-based reinforcement layer (2) is one or more of ordinary concrete, high-strength concrete, fiber-reinforced ultra-high performance concrete or engineering cement-based composite materials; a grouting material layer (4) is added to the surface of the cement block (1), and the cement-based reinforcement layer (2) includes a cement-based reinforcement layer permanent mold (21) that wraps the side and bottom surfaces of the cement block (1) and a mortar layer (5) that covers the top surface of the cement block (1).

4. The surface-reinforced fire-free masonry block according to claim 3, characterized in that: The waste soil is one or more of slag mud, waste slag, furnace slag, brick slag, waste incineration bottom ash or construction waste.

5. The surface-reinforced unburned masonry block according to claim 4, characterized in that: The raw material components of the cement soil block (1) are as follows: by mass, the waste soil is 25-60 parts, the cement is 1-5 parts, and the water is 3-15 parts.

6. The surface-reinforced fire-free masonry block according to claim 3, characterized in that: The outer surface of the cement soil block (1) is a rough and concave surface, and is in close contact with the inner surface of the cement-based reinforcement layer (2).

7. The surface-reinforced fire-free masonry block according to claim 3, characterized in that: A steel mesh layer (3) is provided between the cement-based reinforcement layer (2) and the cement soil block (1).

8. The surface-reinforced fire-free masonry block according to claim 3, characterized in that: The thickness ratio of the cement-based reinforcing layer (2) of the unfired masonry block to the cement soil block (1) in the height direction is 0.08-0.2; when the unfired masonry block is in the shape of a rectangular parallelepiped, the thickness ratio of the cement-based reinforcing layer (2) to the cement soil block (1) in the length direction and the width direction is 0.1-0.3; when the unfired masonry block is in the shape of a cylinder, the thickness ratio of the cement-based reinforcing layer (2) to the cement soil block (1) in the diameter direction is 0.12-0.3.

Citation Information

Patent Citations

  • High-strength tunnel residue soil brick and preparation method thereof

    CN116535154A

  • Baking-free antique black brick and preparation method thereof

    CN108560806A

  • Composite thermal insulation wall containing high-ductility solid waste-based non-dismantling formwork and preparation method of composite thermal insulation wall

    CN113931352A

  • Cement soil building block coated with cement shell on outer surface and preparation method of cement soil building block

    CN117803125A

  • Sandwiched brick and manufacturing method thereof

    CN1804236A