Organic solar cell and method for preparing the same

By spin-coating the donor layer and the photosensitive hybrid layer on the conductive substrate of the organic solar cell, combined with the surface energy driving force, the problem of difficulty in controlling the thickness of the hole transport layer and the preparation of the hole transport layer is solved, achieving low-cost, large-scale preparation and performance improvement .

CN118591243BActive Publication Date: 2024-11-05SHENZHEN TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411074964.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-05
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The manufacturing cost of existing organic solar cells is high and difficult to prepare on a large scale, especially the thickness of the hole transport layer in the photosensitive mixing layer is difficult to regulate and prepare, and solvent orthogonality needs to be considered.

Method used

Provided is a method for preparing an organic solar cell by spin-coating a donor layer on a conductive substrate, preparing a photosensitive hybrid layer with an interpenetrating network structure, and spin-coating an electron transport layer thereon, and finally forming a metal electrode, which is driven by surface energy. Strive to simplify the process, reduce costs, and avoid solvent orthogonal problems.

Benefits of technology

The preparation process of organic solar cells is simplified, the manufacturing cost is reduced, and the thickness regulation of the photosensitive hybrid layer is realized. It is suitable for large-scale preparation and improves the photovoltaic performance and stability of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118591243B_ABST
    Figure CN118591243B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing an organic solar cell and an organic solar cell, and relates to the technical field of solar cells. The method comprises: providing a conductive substrate, and spin-coating a donor solution on the conductive substrate to form a donor layer on the surface of the conductive substrate; preparing an acceptor mixed solution, wherein the acceptor mixed solution is a solution formed by mixing a phosphonic acid-based material and an acceptor material; spin-coating the acceptor mixed solution on the surface of the donor layer so that the acceptor mixed solution swells into the donor layer to simultaneously form a photosensitive mixed layer with an interpenetrating network structure; preparing a transport layer material solution, and spin-coating the transport layer material solution on the photosensitive mixed layer to form an electron transport layer on the surface of the photosensitive mixed layer; and forming a metal electrode on the surface of the electron transport layer. The present application aims to solve the problems of high manufacturing cost, complicated preparation process, and inconvenience for large-area preparation of organic solar cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and in particular to a method for preparing an organic solar cell and an organic solar cell. Background Art

[0002] The hole transport layer of organic solar cells usually needs to be prepared using high vacuum conditions or solution methods, and then the photosensitive layer is prepared on the hole transport layer. However, high vacuum conditions will greatly increase the manufacturing cost of organic solar cells. Although the solution method has great cost advantages, it is difficult to control the thickness of the prepared layer. At the same time, it is also necessary to consider issues such as solvent orthogonality, which is not conducive to large-scale preparation. Summary of the invention

[0003] The present invention provides a method for preparing an organic solar cell and an organic solar cell, aiming to solve the problem that the manufacturing cost of the organic solar cell is high and it is not conducive to large-area preparation.

[0004] In a first aspect, the present invention provides a method for preparing an organic solar cell, the method comprising:

[0005] Providing a conductive substrate, and spin-coating a donor solution on the conductive substrate to form a donor layer on the surface of the conductive substrate;

[0006] preparing a receptor mixed solution, wherein the receptor mixed solution is a solution formed by mixing a phosphonic acid-based material and a receptor material;

[0007] Spin coating the acceptor mixed solution on the surface of the donor layer, so that the acceptor mixed solution swells into the donor layer to form a photosensitive mixed layer with an interpenetrating network structure;

[0008] preparing a transport layer material solution, and spin coating the transport layer material solution on the photosensitive mixed layer to form an electron transport layer on the surface of the photosensitive mixed layer;

[0009] A metal electrode is formed on the surface of the electron transport layer.

[0010] In a second aspect, the present invention provides an organic solar cell, wherein the organic solar cell is prepared by using the above-mentioned method for preparing an organic solar cell.

[0011] The present application provides a method for preparing an organic solar cell and an organic solar cell, the method comprising providing a conductive substrate, and spin-coating a donor solution on the conductive substrate to form a donor layer on the surface of the conductive substrate; preparing an acceptor mixed solution; spin-coating the acceptor mixed solution on the surface of the donor layer so that the acceptor mixed solution swells into the donor layer to form a photosensitive mixed layer with an interpenetrating network structure; preparing a transport layer material solution, and spin-coating the transport layer material solution on the photosensitive mixed layer to form an electron transport layer on the surface of the photosensitive mixed layer; and forming a metal electrode on the surface of the electron transport layer. This can greatly simplify the process of preparing organic solar cells by sequential deposition. By using surface energy as a driving force, the problems of the difficulty in controlling the thickness of the hole transport layer in the photosensitive mixed layer and the difficulty in preparing the hole transport layer can be solved, so that the photosensitive mixed layer can be prepared using low-cost coating technology, thereby reducing the manufacturing cost. At the same time, there is no need to consider problems such as solvent orthogonality, so it is conducive to large-scale preparation and has a good application prospect. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying any creative work.

[0013] Figure 1 An embodiment of the present invention provides a schematic flow chart of a method for preparing an organic solar cell;

[0014] Figure 2 An embodiment of the present invention provides a schematic diagram of the molecular structure of PM6;

[0015] Figure 3 An embodiment of the present invention provides a schematic diagram of preparing a donor layer on a conductive substrate;

[0016] Figure 4 The embodiment of the present invention provides a schematic diagram of the molecular structure of 4PADCB and 2PACZ;

[0017] Figure 5 An embodiment of the present invention provides a schematic diagram of the molecular structure of BTP-eC9;

[0018] Figure 6 An embodiment of the present invention provides a schematic diagram of preparing a photosensitive mixed layer;

[0019] Figure 7 An embodiment of the present invention provides a schematic diagram of preparing an electron transport layer on a photosensitive mixed layer;

[0020] Figure 8 An embodiment of the present invention provides a schematic structural diagram of an organic solar cell;

[0021] Fig. 9 It is a schematic diagram of the photovoltaic performance effect of organic solar cells prepared by different hole transport materials proposed in the examples of the present application. DETAILED DESCRIPTION

[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] It should be understood that when used in this specification and the appended claims, the terms "include" and "comprises" indicate the presence of described features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or combinations thereof.

[0024] It should also be understood that the terms used in this specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. As used in the specification of the present invention and the appended claims, unless the context clearly indicates otherwise, the singular forms "a", "an" and "the" are intended to include plural forms.

[0025] It should be further understood that the term "and / or" used in the present description and the appended claims refers to and includes any and all possible combinations of one or more of the associated listed items.

[0026] In conjunction with the accompanying drawings, some embodiments of the present application are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0027] High-efficiency organic solar cells require good ohmic contact between the photosensitive layer and the electrode to achieve effective charge transfer and extraction, thereby reducing interfacial recombination. Therefore, the introduction of a hole / electron transport layer between the photosensitive layer and the electrode plays a vital role in the performance of organic photovoltaic devices. In the related art, the preparation methods of the hole / electron transport layer generally include vacuum deposition and solution methods, but these methods retain some difficult-to-solve problems. For example, vacuum deposition technology requires high vacuum conditions, which greatly increases the manufacturing cost; although the solution method has great cost advantages, it is difficult to control the thickness of the hole / electron transport layer, and the problem of solvent orthogonality needs to be considered, and its application to large-area device preparation is extremely limited. Therefore, developing an organic solar cell preparation strategy that simultaneously improves device efficiency and simplifies processing is urgent for future industrial production.

[0028] The present application provides a method for preparing an organic solar cell and an organic solar cell, which can greatly simplify the process of preparing an organic solar cell by a sequential deposition method. By utilizing surface energy as a driving force, the problems of difficulty in controlling the thickness of a hole transport layer in a photosensitive mixing layer and difficulty in preparing the layer can be solved. Thus, a low-cost coating technology can be used to prepare the photosensitive mixing layer, thereby reducing the manufacturing cost. At the same time, there is no need to consider problems such as solvent orthogonality, which is conducive to large-scale preparation and has a good application prospect.

[0029] See also Figure 1 , Figure 1 The present invention provides a schematic flow chart of a method for preparing an organic solar cell. The method for preparing an organic solar cell can greatly simplify the process of preparing an organic solar cell by a sequential deposition method. By using surface energy as a driving force, it can solve the problems of difficulty in controlling the thickness of the hole transport layer in the photosensitive mixed layer and difficulty in preparation. Therefore, the photosensitive mixed layer can be prepared by low-cost coating technology, thereby reducing the manufacturing cost. At the same time, there is no need to consider the problem of solvent orthogonality, so it is conducive to large-scale preparation and has a good application prospect.

[0030] like Figure 1 As shown, the method for preparing the organic solar cell includes: step S101 to step S105.

[0031] S101, providing a conductive substrate, and spin-coating a donor solution on the conductive substrate to form a donor layer on the surface of the conductive substrate.

[0032] The conductive substrate 10 may be any substrate that can be used for support and conduct electricity, such as transparent conductive glass, indium tin oxide, etc. The donor solution may be a solution prepared by a donor material, used to prepare the donor layer 20, and the prepared donor layer 20 is stacked with the conductive substrate 10.

[0033] In some embodiments, after providing the conductive substrate 10, the conductive substrate 10 is ultrasonically cleaned; the conductive substrate 10 after the ultrasonic cleaning is dried at a constant temperature; the conductive substrate 10 after the constant temperature drying is plasma-ozone cleaned to obtain a cleaned conductive substrate 10. In this way, dust and oil attached to the surface of the conductive substrate 10 can be cleaned to avoid affecting the quality of the prepared solar cell.

[0034] Specifically, the dirt on the surface of the conductive substrate 10 can be wiped off with a cotton swab soaked in anhydrous ethanol, and then the conductive substrate 10 is ultrasonically cleaned in cleaning solution, deionized water, acetone, deionized water, and isopropyl alcohol in sequence for 10-30 minutes, and then the cleaned conductive substrate 10 is placed in a constant temperature box at a temperature of 70-90° C. for drying, and finally the dried conductive substrate 10 is subjected to plasma ozone cleaning for about 2-10 minutes.

[0035] For example, since the commercially purchased conductive substrate 10 will inevitably be attached with dust and oil during transportation, the impurities visible to the naked eye on the surface of the conductive substrate 10 can be removed with a cotton swab soaked in ethanol. Subsequently, the pretreated conductive substrate 10 is ultrasonically cleaned in detergent water, deionized water, acetone, deionized water, and isopropanol in sequence, with each step cleaning for 15 minutes. The cleaned conductive substrate 10 is then transferred to a constant temperature drying oven for treatment for 4 hours. Finally, the dried conductive substrate 10 is plasma ozone cleaned for 6 minutes to enhance the hydrophilicity of the surface of the conductive substrate 10, so that the surface of the conductive substrate 10 can be fully cleaned to facilitate the subsequent preparation of the organic solar cell 100.

[0036] In some embodiments, before spin coating the donor solution on the conductive substrate 10 to form the donor layer 20 on the surface of the conductive substrate 10, the donor material is added to the halogen-free solvent to dissolve the donor material in the halogen-free solvent; the halogen-free solvent is heated and stirred to obtain a donor solution, wherein the concentration of the donor solution is 5-10 mg / ml. In this way, a donor solution of a corresponding concentration can be prepared.

[0037] like Figure 2 As shown, the donor material may be a polymer donor material (PBDB-TF, PM6), and the halogen-free solvent may include toluene or other solvents for dissolving the polymer donor material.

[0038] Specifically, the donor material PM6 can be dissolved in a halogen-free solvent to form a donor layer solution, and the concentration of the donor layer solution is controlled to be 5-10 mg / ml.

[0039] For example, the polymer donor material PM6 can be heated and stirred to dissolve in the halogen-free solvent toluene for 1 hour, thereby preparing a PM6 solution with a concentration of 8 mg / ml.

[0040] It should be noted that the concentration of the donor layer solution can be determined according to the required thickness of the donor layer 20 and is not specifically limited here.

[0041] like Figure 3 As shown, in some embodiments, the first working parameter of the coating machine is determined according to the concentration of the donor solution, the first working parameter includes a first rotation speed and a first coating time, the first rotation speed is 3000 rpm, and the first coating time is 30 seconds; the coating machine is controlled to spin-coat the donor solution on the conductive substrate 10 based on the first working parameter to form a donor layer 20 on the surface of the conductive substrate 10. In this way, a donor layer 20 with a specific thickness can be prepared on the surface of the conductive substrate 10.

[0042] The first working parameter includes a first rotation speed and a first glue-spinning time.

[0043] Specifically, the first rotation speed and the first coating time of the coating machine are determined according to the thickness of the donor layer 20 to be prepared and the concentration of the donor solution, and then the coating machine is controlled to spin-coat the donor solution on the conductive substrate 10 at the first rotation speed and continue to spin-coat for the first coating time, thereby forming a donor layer 20 with a target thickness on the surface of the conductive substrate 10.

[0044] For example, the first rotation speed and the first coating time of the coating machine can be determined to be 3000 rpm and 30 s respectively according to the thickness of the donor layer 20 to be prepared and the concentration of the donor solution, and then the coating machine is controlled to spin-coat the donor solution on the conductive substrate 10 at a rotation speed of 3000 rpm so as to form a donor layer 20 with a target thickness on the surface of the conductive substrate 10 for 30 s.

[0045] S102, preparing a receptor mixed solution, wherein the receptor mixed solution is a solution formed by mixing a phosphonic acid-based material and a receptor material.

[0046] like Figure 4 and Figure 5 As shown, the acceptor mixed solution is a solution formed by mixing a phosphonic acid-based material and an acceptor material. The phosphonic acid-based material may include a self-assembled monomolecular material 4-(7H-dibenzo[c,g]carbazole-7-yl)butyl)phosphonic acid (4PADCB) or 2-(9H-carbazole-9-acyl)ethyl)phosphonic acid (2PACZ). The acceptor material may include an organic photovoltaic OPV material BTP-eC9.

[0047] In some embodiments, a phosphonic acid-based material is added to an organic solvent so that the phosphonic acid-based material is dissolved in the organic solvent to obtain a phosphonic acid-based solution, and the concentration of the phosphonic acid-based solution is 0.3-5 mg / ml; an acceptor material is added to a halogen-free solvent so that the acceptor material is dissolved in the halogen-free solvent to obtain an acceptor solution, and the concentration of the acceptor solution is 6-12 mg / ml; the phosphonic acid-based solution is added to the acceptor solution and mixed to obtain an acceptor mixed solution. Since the phosphate oxygen of the phosphonic acid-based solution can coordinate with the metal Lewis acid, it is anchored on the surface of the ITO electrode, so that a suitable energy orientation is provided on the photosensitive mixed layer 30, and the work function of the electrode is effectively adjusted, thereby reducing the non-radiative recombination of the organic solar cell 100 and improving the device stability and photoelectric conversion efficiency.

[0048] Specifically, the self-assembled single molecule 4PADCB or 2PACZ is dissolved in an organic solvent at a concentration of 0.3-5 mg / ml to form a high-concentration phosphonic acid solution; the receptor material BTP-eC9 is then dissolved in a halogen-free solvent at a concentration of 6-12 mg / ml to form a receptor solution; finally, the phosphonic acid solution is added to the receptor solution, the volume ratio is controlled between 1:100-5:100, and stirred evenly to form a uniformly mixed receptor mixed solution.

[0049] In the related art, when preparing the hole transport layer and the photosensitive layer, it is also necessary to consider whether the photosensitive layer solution will dissolve the hole transport layer, that is, there is a problem of solvent orthogonality. The present application prepares a mixed solution of the hole transport layer material and the acceptor material, thereby achieving the simultaneous preparation of the photosensitive layer and the hole transport layer through the mixed solution, that is, the photosensitive mixed layer 30 provided in the present application, and the process is simpler.

[0050] Exemplarily, the self-assembled single molecule material 4PADCB or 2PACZ can be dissolved by stirring at room temperature using methanol solvent at a concentration of 4 mg / ml to form a uniform self-assembled single molecule 4PADCB solution or 2PACZ solution; the acceptor material BTP-eC9 is heated and stirred to dissolve for 1 hour using halogen-free solvent toluene at a concentration of 8 mg / ml to form a uniform acceptor BTP-eC9 solution; then, the self-assembled single molecule 4PADCB solution or 2PACZ solution is added to the acceptor BTP-eC9 solution and stirred for 0.5 hours, with the addition volume ratio of 5:100 to form a uniform acceptor mixed solution.

[0051] S103 , spin-coating the acceptor mixed solution on the surface of the donor layer 20 , so that the acceptor mixed solution swells into the donor layer 20 to form a photosensitive mixed layer 30 having an interpenetrating network structure.

[0052] The photosensitive mixed layer 30 is formed by mutual diffusion of donors and acceptors, and has a bicontinuous interpenetrating network structure.

[0053] like Figure 6 As shown, in some embodiments, the second working parameter of the coating machine is determined according to the concentration of the acceptor mixed solution, and the second working parameter includes a second rotation speed and a second coating time, the second rotation speed is 3500rpm, and the second coating time is 30s; the coating machine is controlled based on the second working parameter to spin-coat the acceptor mixed solution on the donor layer 20, so that the acceptor mixed solution swells into the donor layer 20 to form a photosensitive mixed layer 30 with an interpenetrating network structure, and the thickness of the photosensitive mixed layer 30 is 40-300nm. In this way, a photosensitive mixed layer 30 with a specific thickness can be prepared on the donor layer 20.

[0054] The second working parameter includes a second rotation speed and a second glue-spinning time.

[0055] Specifically, the second rotation speed and the second coating time of the coating machine are determined according to the thickness of the photosensitive mixed layer 30 to be prepared and the concentration of the acceptor mixed solution, and then the coating machine is controlled to spin-coat the acceptor mixed solution on the donor layer 20 at the second rotation speed and continue to spin-coat for the second coating time. During the spin-coating process, the acceptor mixed solution will quickly swell the lower donor PM6 layer. On the one hand, the acceptor BTP-eC9 will diffuse and penetrate into the donor, thereby forming a photosensitive layer of a double continuous interpenetrating network; on the other hand, driven by the surface energy, the self-assembled single molecule 4PADCB or 2PACZ will also pass through the donor PM6 layer and be deposited near the conductive substrate 10, thereby forming a 4PADCB monolayer or a 2PACZ monolayer; the above two processes are carried out simultaneously, and the mixture is left to dry for 4-6 minutes to finally form a photosensitive mixed layer 30, and the thickness of the photosensitive mixed layer 30 can be controlled within the range of 40-300nm, thereby reducing the non-radiative recombination of the prepared solar cell, thereby improving the stability and photoelectric conversion efficiency of the solar cell.

[0056] Since the hole transport layer in the related art can be prepared by 4PADCB solution or 2PACZ solution, and the photosensitive layer solution can be prepared by PM6 solution and BTP-eC9 solution. The present application prepares a mixed solution of 4PADCB solution or 2PACZ solution and BTP-eC9 solution to obtain a mixed acceptor solution. The present application can achieve the simultaneous preparation of the photosensitive layer and the hole transport layer by preparing the mixed solution, that is, the photosensitive mixed layer 30 provided by the present application, the process is simpler, and can solve the problems of the difficulty in controlling the thickness of the hole transport layer and the difficulty in preparation, so that the photosensitive mixed layer 30 can be prepared by low-cost coating technology, thereby reducing the manufacturing cost, and there is no need to consider problems such as solvent orthogonality, so it is conducive to large-scale preparation and has a good application prospect.

[0057] Exemplarily, the second rotation speed and the second coating time of the coating machine can be determined to be 3500 rpm and 30 s respectively according to the thickness of the photosensitive mixed layer 30 to be prepared and the concentration of the acceptor mixed solution, and the acceptor mixed solution is spin-coated onto the donor PM6 layer at a rotation speed of 3500 rpm for 30 s and allowed to stand for 5 minutes; during this process, the acceptor mixed solution will rapidly swell the lower donor PM6 layer. On the one hand, the acceptor BTP-eC9 will diffuse and penetrate into the donor to form a photosensitive layer of a double continuous interpenetrating network; on the other hand, driven by the surface energy, the self-assembled single molecule 4PADCB or 2PACZ will also pass through the donor PM6 layer and be deposited near the transparent conductive glass to form a self-assembled monolayer 4PADCB or 2PACZ; the above two processes are carried out simultaneously, and the mixture is allowed to stand and dry for 4-6 minutes to finally form a photosensitive mixed layer 30.

[0058] S104 , preparing a transport layer material solution, and spin-coating the transport layer material solution on the photosensitive mixed layer 30 to form an electron transport layer on the surface of the photosensitive mixed layer.

[0059] The electron transport layer 40 is prepared by spin coating a transport layer material solution on the surface of the photosensitive mixed layer 30 , and is stacked with the photosensitive mixed layer 30 .

[0060] In some embodiments, the electron transport layer 40 material is added to an organic solvent to dissolve the electron transport layer 40 material in the organic solvent; the organic solvent is stirred to obtain a transport layer material solution, and the concentration of the transport layer material solution is 0.3-2 mg / ml. In this way, a transport layer material solution of corresponding concentration can be prepared.

[0061] The material of the electron transport layer 40 may include a material capable of forming the electron transport layer 40 , such as a PNDIT-F3N material of the electron transport layer 40 .

[0062] Specifically, the electron transport layer 40PNDIT-F3N material is dissolved in an organic solvent, and then stirred to form a transport layer material solution with a concentration of about 0.3-2 mg / ml.

[0063] For example, a mixed solvent of methanol and acetic acid may be used to dissolve the electron transport layer 40 material PNDIT-F3N, and the ratio of methanol to acetic acid may be 1000:5, thereby stirring to form a transport layer material solution, and the concentration of the transport layer material solution is 0.5 mg / ml.

[0064] like Figure 7As shown, in some embodiments, the third working parameter of the coating machine is determined according to the concentration of the transport layer material solution, and the third working parameter includes a third rotation speed and a third coating time, the third rotation speed is 2000rpm, and the third coating time is 30s; the coating machine is controlled based on the third working parameter to spin-coat the transport layer material solution on the photosensitive mixed layer 30 to form an electron transport layer 40 on the surface of the photosensitive mixed layer 30, and the thickness of the electron transport layer 40 is 4-50nm. In this way, an electron transport layer 40 with a specific thickness can be prepared on the photosensitive mixed layer 30.

[0065] The third working parameter includes a third rotation speed and a third glue-spinning time.

[0066] Specifically, the transport layer material solution is spin-coated on the prepared photosensitive mixed layer 30 and left to dry for 7-10 minutes, and the thickness of the electron transport layer 40 can be controlled within the range of 40-300 nm.

[0067] Exemplarily, a coating machine is used to spin-coat the transport layer material solution onto the prepared photosensitive mixed layer 30, the rotation speed is controlled at 2000 rpm, and the coating time is 30 s, thereby forming an electron transport layer 40 on the surface of the photosensitive mixed layer 30, and the thickness of the electron transport layer 40 is controlled at 15 nm.

[0068] S105, forming a metal electrode on the surface of the electron transport layer.

[0069] The metal electrode 50 may include a silver electrode, a gold electrode, an aluminum electrode, or the like.

[0070] like Figure 8 As shown, in some embodiments, a thermal evaporation device is used to dissolve metal; based on a preset vacuum condition, the dissolved metal is evaporated onto the electron transport layer 40 to form a metal electrode 50 on the surface of the electron transport layer 40, and the thickness of the metal electrode 50 is 30-300nm. Thus, a metal electrode 50 with a specific thickness can be prepared on the surface of the electron transport layer 40.

[0071] Specifically, metallic silver can be placed on a tungsten boat and placed under high vacuum conditions, and the metallic silver can be evaporated onto the electron transport layer 40 by thermal evaporation, thereby forming a silver electrode on the surface of the electron transport layer 40, and the thickness of the metal electrode 50 can be controlled within the range of 30-300nm.

[0072] For example, the silver metal is dissolved by thermal evaporation equipment under a vacuum degree of 5×10 -4 Under the condition of Pa, metallic silver will be liquefied, and the liquid silver will be vaporized onto the electron transport layer 40 to form a silver electrode, and the thickness of the silver electrode is 150 nm, thereby preparing the organic solar cell 100.

[0073] See also Fig. 9 , Fig. 9 Schematic diagram of the photovoltaic performance of an organic solar cell 100 prepared using different hole transport materials proposed in an embodiment of the present application. Fig. 9 The photovoltaic performance of a solar cell prepared by an acceptor solution formed by BTP-eC9 (Example 1), the photovoltaic performance of a solar cell prepared by an acceptor mixed solution formed by 4PADCB and BTP-eC9 (Example 2), and the photovoltaic performance of a solar cell prepared by an acceptor mixed solution formed by 2PACZ and BTP-eC9 (Example 3) are shown.

[0074] Depend on Fig. 9 The photovoltaic performances of Example 1, Example 2 and Example 3 can be obtained as shown in Table 1.

[0075] Table 1

[0076]

[0077] The photovoltaic performance of Example 1, Example 2 and Example 3 is under the AM 1.5G standard simulated sunlight light source, and the light intensity is controlled at 100mW / cm 2 It can be seen from Table 1 that after the acceptor BTP-eC9 solution is doped with phosphonic acid-based materials, the photovoltaic performance of the prepared solar cell is greatly improved; when the phosphonic acid-based material is 4PADCB, the open circuit voltage V OC , short circuit current density J SC and fill factor FF reached 0.869V and 28.10 mA / cm 2 and 78.20%, and the photoelectric conversion efficiency PCE increased significantly to 19.10%. When the phosphonic acid-based material is 2PACZ, the open circuit voltage V OC , short circuit current density J SC and fill factor FF reached 0.861V and 27.92 mA / cm 2 and 78.22%, and the photoelectric conversion efficiency PCE increased to 18.81%. It can be seen that the preparation method of the organic solar cell 100 proposed in the embodiment of the present application can significantly improve the photovoltaic performance of the organic solar cell 100, has good universality, and can greatly simplify the advanced sequential deposition process, has a good application prospect, and is very suitable for industrial-grade preparation and production.

[0078] The present application provides a method for preparing an organic solar cell 100, which comprises providing a conductive substrate 10, and spin-coating a donor solution on the conductive substrate 10 to form a donor layer 20 on the surface of the conductive substrate 10; preparing an acceptor mixed solution; spin-coating the acceptor mixed solution on the surface of the donor layer 20 so that the acceptor mixed solution swells into the donor layer 20 to form a photosensitive mixed layer 30 with an interpenetrating network structure; preparing a transport layer material solution, and spin-coating the transport layer material solution on the photosensitive mixed layer 30 to form an electron transport layer 40 on the surface of the photosensitive mixed layer 30; and forming a metal electrode 50 on the surface of the electron transport layer 40. Thus, the process of preparing the organic solar cell 100 by the sequential deposition method can be greatly simplified. By using surface energy as a driving force, the problems of the difficulty in controlling the thickness of the hole transport layer and the difficulty in preparing the hole transport layer can be solved, so that the photosensitive mixed layer 30 can be prepared by using a low-cost coating technology, thereby reducing the manufacturing cost. At the same time, there is no need to consider the problems of solvent orthogonality, so it is conducive to large-scale preparation and has a good application prospect.

[0079] The embodiment of the present application further provides an organic solar cell 100 , which is prepared by using the method for preparing a solar cell provided by any of the above embodiments.

[0080] The specific method of preparing the organic solar cell 100 can refer to the corresponding embodiment recorded in the specification of this application, and this embodiment will not be repeated here. The organic solar cell 100 provided in the embodiment of this application has high photovoltaic performance, low manufacturing cost, and can be prepared on a large scale, and has a good application prospect.

[0081] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed by the present invention, and these modifications or replacements should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A method for preparing an organic solar cell, characterized in that: The method comprises: Providing a conductive substrate, and spin-coating a donor solution on the conductive substrate to form a donor layer on the surface of the conductive substrate; Prepare a receptor mixed solution, wherein the receptor mixed solution is a solution formed by mixing a phosphonic acid-based material and a receptor material, wherein the phosphonic acid-based material includes a self-assembled monomolecular material 4-(7H-dibenzo[c,g]carbazole-7-yl)butyl)phosphonic acid or a self-assembled monomolecular material 2-(9H-carbazole-9-acyl)ethyl)phosphonic acid; Spin coating the acceptor mixed solution on the surface of the donor layer, so that the acceptor mixed solution swells into the donor layer to form a photosensitive mixed layer with an interpenetrating network structure; preparing a transport layer material solution, and spin coating the transport layer material solution on the photosensitive mixed layer to form an electron transport layer on the surface of the photosensitive mixed layer; A metal electrode is formed on the surface of the electron transport layer.

2. The method according to claim 1, characterized in that: The method of preparing the receptor mixed solution comprises: Adding the phosphonic acid-based material to an organic solvent so that the phosphonic acid-based material is dissolved in the organic solvent to obtain a phosphonic acid-based solution, wherein the concentration of the phosphonic acid-based solution is 0.3-5 mg / ml; Adding the receptor material to a halogen-free solvent so that the receptor material is dissolved in the halogen-free solvent to obtain a receptor solution, wherein the concentration of the receptor solution is 6-12 mg / ml; The phosphonic acid-based solution is added to the receptor solution and mixed to obtain a receptor mixed solution.

3. The method according to claim 1, characterized in that The method of spin coating the acceptor mixed solution on the surface of the donor layer so that the acceptor mixed solution swells into the donor layer to form a photosensitive mixed layer having an interpenetrating network structure comprises: Determining the second working parameter of the coating machine according to the concentration of the receptor mixed solution, the second working parameter includes a second rotation speed and a second coating time, the second rotation speed is 3500 rpm, and the second coating time is 30 s; The coating machine is controlled based on the second working parameter to spin-coat the acceptor mixed solution on the donor layer, so that the acceptor mixed solution swells into the donor layer to form a photosensitive mixed layer with an interpenetrating network structure, and the thickness of the photosensitive mixed layer is 40-300nm.

4. The method according to claim 1, characterized in that Before spin coating the donor solution on the conductive substrate to form a donor layer on the surface of the conductive substrate, the method further comprises: adding a donor material to a halogen-free solvent so that the donor material is dissolved in the halogen-free solvent; The halogen-free solvent is heated and stirred to obtain the donor solution, wherein the concentration of the donor solution is 5-10 mg / ml.

5. The method according to claim 1, characterized in that The step of spin coating the donor solution on the conductive substrate to form a donor layer on the surface of the conductive substrate comprises: Determining the first working parameter of the coating machine according to the concentration of the donor solution, the first working parameter includes a first rotation speed and a first coating time, the first rotation speed is 3000 rpm, and the first coating time is 30 s; The coating machine is controlled to spin-coat the donor solution on the conductive substrate based on the first working parameter to form a donor layer on the surface of the conductive substrate.

6. The method according to claim 1, characterized in that The method of preparing the transport layer material solution comprises: adding a transport layer material to an organic solvent so that the transport layer material is dissolved in the organic solvent; The organic solvent is stirred to obtain the transport layer material solution, wherein the concentration of the transport layer material solution is 0.3-2 mg / ml.

7. The method according to claim 1, characterized in that The step of spin coating the transport layer material solution on the photosensitive mixed layer to form an electron transport layer on the surface of the photosensitive mixed layer comprises: Determine the third working parameter of the coating machine according to the concentration of the transmission layer material solution, the third working parameter includes a third rotation speed and a third coating time, the third rotation speed is 2000 rpm, and the third coating time is 30 s; The coating machine is controlled to spin-coat the transport layer material solution on the photosensitive mixed layer based on the third working parameter to form an electron transport layer on the surface of the photosensitive mixed layer, and the thickness of the electron transport layer is 4-50 nm.

8. The method according to claim 1, characterized in that The step of forming a metal electrode on the surface of the electron transport layer comprises: Dissolving metals using thermal evaporation equipment; Based on the preset vacuum condition, the dissolved metal is evaporated onto the electron transport layer to form a metal electrode on the surface of the electron transport layer, and the thickness of the metal electrode is 30-300 nm.

9. The method according to claim 1, characterized in that: After providing the conductive substrate, the method further comprises: Performing ultrasonic cleaning on the conductive substrate; performing a constant temperature drying treatment on the conductive substrate after the ultrasonic cleaning treatment; The conductive substrate after the constant temperature drying treatment is cleaned by plasma ozone to obtain a cleaned conductive substrate.

10. An organic solar cell, characterized in that: The organic solar cell is prepared by using the method for preparing an organic solar cell according to any one of claims 1 to 9.