An intelligent method for recovering cobalt from cobalt slag with cobalt removal agent
Through intelligent recovery methods, combined with purification, flotation and pickling steps, using zinc powder and flotation reagents, the problem of poor nickel removal effect from cobalt slag is solved, efficient recovery of cobalt and optimal utilization of indium resources are achieved, improving improve recovery efficiency and purity.
Patent Information
- Application Number
- CN202411089650.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-08-09
AI Technical Summary
In the existing cobalt slag recovery technology, there is a lack of effective methods to avoid the impact of cobalt removal agents and pickling decomposition products of cobalt removal agent slag on indium extraction, and the removal effect of nickel is poor, resulting in low cobalt recovery efficiency.
Using intelligent recovery methods, through purification, flotation and pickling steps, using zinc powder, activator and flotation reagents, combined with real-time monitoring and image analysis technology, the cobalt slag is separated and purified to ensure the effective removal of nickel and efficient recovery of cobalt. .
It achieves effective removal of nickel from cobalt slag, improves cobalt recovery efficiency and purity, ensures efficient utilization of indium resources, and optimizes the stability and efficiency of the recovery process through real-time monitoring and data analysis technology.
Smart Images

Figure CN118594759B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cobalt removal agent cobalt slag recovery, and in particular to an intelligent recovery method of cobalt in cobalt removal agent cobalt slag. Background Art
[0002] The indium element is distributed in small and dispersed amounts. It is usually dispersed as an associated element in sulfide minerals composed of other elements. 80% of indium comes from sphalerite, which contains 1000g / t-1500g / t of indium. The physical and chemical properties of metallic indium are special. It is widely used in optoelectronics, military and modern information industries. It is increasingly important for the development of the national economy and has become one of the most important supporting materials in the modern electronics industry. Therefore, in the process of removing cobalt from organic reagents in hydrometallurgical zinc smelting, how to avoid the influence of the decomposition products of the cobalt removal agent and the cobalt removal agent slag pickling on the indium extraction, and to ensure the effective removal of the impurity element nickel, so as to achieve the comprehensive recovery of cobalt and improve the recovery rate of indium resources, has become a research hotspot for relevant researchers.
[0003] Patent document with publication number CN113265548B discloses a method for enriching and recovering cobalt in cobalt slag containing a cobalt remover, the method comprising the following steps: (1) mixing the cobalt slag containing the cobalt remover with a 160-200 g / L sulfuric acid solution at a liquid-to-solid ratio of 5:1; (2) filtering after reacting for 4-5 hours, detecting and analyzing the obtained supernatant, and filtering the obtained filter residue to obtain tailings for later use; (3) micro-leaching the obtained tailings again in a sulfuric acid solution with an acidity of 25-30 g / L, filtering to obtain water-washed slag, and sampling the water-washed slag for detection and analysis. It can be seen that the existing technology for recovering cobalt from cobalt slag lacks a process that considers whether the cobalt remover and the acid washing decomposition products of the cobalt remover slag have an impact on indium extraction, and if there is no impact, effectively removes nickel from the cobalt slag to recover cobalt. Summary of the invention
[0004] To this end, the present invention provides an intelligent method for recovering cobalt from cobalt slag with a cobalt removal agent, so as to overcome the problems in the prior art of poor nickel removal effect in the cobalt slag due to the lack of direct comprehensive recovery of the impurity element nickel, and the lack of real-time monitoring of the purification process of the cobalt slag, resulting in low cobalt recovery efficiency.
[0005] To achieve the above object, the present invention provides an intelligent method for recovering cobalt from cobalt slag with a cobalt removal agent, comprising:
[0006] A first stage of purification, obtaining a mixed slag leaching solution, determining an initial cadmium content in the mixed slag leaching solution, and calculating a preset addition mass according to the initial cadmium content;
[0007] Adding zinc powder to the mixed slag leachate with a preset added mass, stirring and reacting for 30 minutes under a first water bath temperature condition, filtering, obtaining a primary filtrate, and determining a first actual content of zinc, cadmium, cobalt, nickel, and iron in the primary filtrate;
[0008] Second stage purification, obtaining the primary filtrate, adding an activator under the second water bath temperature condition, stirring and reacting for 10 minutes, calculating the amount of cobalt removal agent added according to the first actual content, adding the cobalt removal agent to the filtrate with the amount of cobalt removal agent added, continuing to stir and react for 90 minutes, and then filtering to obtain a secondary filtrate as a cobalt removal liquid, and a filter residue as a cobalt removal agent residue;
[0009] Three-stage purification, adding sulfuric acid solution to the cobalt removal agent slag under preset pickling conditions for pickling, keeping the water bath at a constant temperature of 75-80° C., stirring and reacting for 60 minutes, and then filtering the liquid to obtain a pickling solution and cobalt slag;
[0010] Purifying the cobalt slag, collecting the cobalt slag for flotation to obtain pure cobalt slag, determining the contents of nickel and cobalt in the pure cobalt slag, and obtaining the average nickel content of the supernatant and the cobalt recovery rate;
[0011] The flotation process is monitored by obtaining a continuous bubble image on the surface of the slurry to be processed, and the real-time bubble generation rate is calculated according to the continuous bubble image. When the real-time bubble generation rate is greater than the standard bubble generation rate, a continuous flotation sedimentation image is obtained to calculate the real-time bubble generation rate, and when the real-time sedimentation rate is greater than the standard sedimentation rate, a flotation sedimentation curve is drawn. When it is determined that a peak appears in the flotation sedimentation curve, the addition of flotation reagents is stopped to obtain flotation foam, thereby obtaining pure cobalt slag.
[0012] Further, the cobalt slag is collected for flotation to obtain pure cobalt slag including:
[0013] Pre-treating the cobalt slag to obtain cobalt slag sample particles for later use;
[0014] Mixing the cobalt slag sample particles with water to form a slurry to be processed;
[0015] Control the valve to open so as to add flotation reagents to the slurry to be processed in a stirring state, and introduce air into the slurry to be processed at a preset air flow rate, and monitor the adding process in real time to obtain flotation froth;
[0016] Controlling the scraper to collect the flotation foam to obtain a foam product, and drying the foam product to obtain pure cobalt slag;
[0017] The flotation reagent is composed of xanthate, lignin and rosin acid, and the mass ratio of each component is 1:1:1.
[0018] Further, the addition process is monitored in real time to obtain flotation foam including:
[0019] Taking a continuous bubble image of the surface of the slurry to be processed, and analyzing the bubbles in the continuous bubble image to determine whether to adjust the preset air flow rate;
[0020] Taking initial pulp images and continuous flotation sedimentation images from the side of the pulp to be processed;
[0021] Calculating the initial color value of the initial pulp image and the average color value corresponding to each continuous flotation sedimentation image;
[0022] Calculate the percentage of the average color value corresponding to any continuous flotation sedimentation image to the initial color value to obtain the real-time sedimentation rate;
[0023] Whether to control the valve to be closed is determined according to the real-time sedimentation rate, thereby forming flotation foam.
[0024] Further, analyzing the bubbles in the continuous bubble image includes:
[0025] The real-time bubble generation rate is calculated based on the continuous bubble image, and the real-time bubble generation rate is determined based on the standard bubble generation rate.
[0026] If the real-time bubble generation rate is less than or equal to the standard bubble generation rate, the preset air flow rate is increased to the corrected air flow rate;
[0027] If the real-time bubble generation rate is greater than the standard bubble generation rate, continuous flotation sedimentation images are taken on the side of the slurry to be processed, and the real-time sedimentation rate is obtained according to the flotation sedimentation images.
[0028] Further, when the real-time bubble generation rate is greater than the standard bubble generation rate, the real-time sedimentation rate is compared with the standard sedimentation rate.
[0029] If the real-time sedimentation rate is less than or equal to the standard sedimentation rate, the valve is controlled to close;
[0030] If the real-time sedimentation rate is greater than the standard sedimentation rate, a flotation sedimentation curve is drawn according to the continuous flotation sedimentation image, and whether to control the valve to be closed is determined according to the flotation sedimentation curve.
[0031] Further, determining whether to control the valve to be closed according to the flotation sedimentation curve includes:
[0032] Obtaining the average gray value corresponding to each continuous flotation sedimentation image;
[0033] The average gray value is plotted over time according to the preset acquisition time, and a linear fit is performed to obtain the average gray value fitting curve;
[0034] The maximum slope of the average grayscale fitting curve is taken as the image grayscale change rate;
[0035] Obtaining the grayscale change rate of each image in each preset acquisition period, and drawing a curve of the grayscale change rate of each image over time as the flotation sedimentation curve;
[0036] The change trend of the flotation sedimentation curve is determined, and when a peak value appears in the flotation sedimentation curve, the valve is controlled to be closed, and it is determined that the bubbles on the surface of the ore pulp to be processed form flotation foam;
[0037] When no peak appears in the flotation sedimentation curve, the valve is not controlled to be closed.
[0038] Further, calculating the real-time bubble generation rate based on the continuous bubble image includes,
[0039] Obtain an arbitrary bubble image and a next adjacent bubble image to perform bubble recognition and contour marking respectively;
[0040] The sum of the newly added bubble positions and the newly added inner contour areas in the adjacent bubble images is obtained to obtain the real-time bubble generation rate.
[0041] Furthermore, pre-treating the cobalt slag includes:
[0042] The cobalt slag is dried and crushed within a preset crushing particle size range to obtain the cobalt slag sample particles whose actual crushing particle size is within the preset crushing particle size range, and the preset crushing particle size range is 0.1 mm-1 mm.
[0043] Furthermore, the preset added mass is 0.9 times of the initial cadmium content, and the first water bath temperature condition is a constant water bath temperature of 45-50°C.
[0044] Furthermore, the amount of the cobalt removal agent added is 5-10 times the sum of the masses of cobalt and nickel, or 4-8 times the sum of the masses of cadmium and iron, the amount of the activator added is one tenth of the amount of the cobalt removal agent added, and the cobalt removal agent is sodium dimethyldithiocarbamate.
[0045] Compared with the prior art, the beneficial effect of the present invention lies in that nickel is removed while removing cobalt by means of a wet treatment method for comprehensive recovery, cobalt is effectively separated from cobalt slag by means of a flotation method utilizing the hydrophobicity difference of minerals, so as to achieve the separation of large particles and impurities, thereby extracting relatively pure cobalt slag, and further providing a basis for subsequent cobalt recovery, real-time monitoring of the addition process, control of valve opening and scraper collection of foam, ensuring stable operation process, improving recovery efficiency, obtaining pure cobalt slag through an intelligent recovery method, and effectively recovering cobalt from the cobalt slag, and combining real-time monitoring and data analysis technology to achieve sustainable recovery of cobalt.
[0046] Furthermore, during the flotation process, bubbles will gradually form a foam layer, which is rich in cobalt minerals. Finally, the foam layer formed on the surface of the slurry is clearly stratified from the sediment at the bottom, which is easy to separate. The bubble generation rate and sedimentation rate are monitored to improve the flotation efficiency and obtain a stable foam layer. By analyzing the effect of the addition of flotation agents on the bubble generation rate and sedimentation rate, the addition amount of flotation agents is controlled in time to ensure sufficient flotation agents to stabilize the foam. At the same time, the negative impact of excessive addition of flotation agents on the flotation efficiency is avoided. The flotation process is optimized through dynamic monitoring and intelligent adjustment strategies to improve the flotation efficiency and the recovery rate and purity of cobalt.
[0047] Furthermore, the color change of the cobalt slag slurry is analyzed through image recognition technology to effectively monitor the sedimentation process. The speed of color change is analyzed to analyze the sedimentation efficiency. If the real-time sedimentation rate is determined to be less than or equal to the standard sedimentation rate, it means that the flotation efficiency is not high. This is caused by excessive addition of reagents. In this case, the valve is closed in time to stop adding flotation reagents to avoid the influence of excessive reagents on the flotation effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 It is a schematic flow chart of the intelligent recovery method of cobalt in cobalt slag with a cobalt removal agent according to an embodiment of the present invention;
[0049] Figure 2 This is a schematic diagram of the process of cobalt slag purification according to an embodiment of the present invention;
[0050] Figure 3 A logic decision diagram for adjusting a preset air flow rate according to an embodiment of the present invention;
[0051] Figure 4 This is a logic decision diagram for controlling valve closing according to an embodiment of the present invention. DETAILED DESCRIPTION
[0052] In order to make the objects and advantages of the present invention more clearly understood, the present invention is further described below in conjunction with embodiments; it should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0053] The preferred embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.
[0054] It should be noted that, in the description of the present invention, terms such as "up", "down", "left", "right", "inside" and "outside" indicating directions or positional relationships are based on the directions or positional relationships shown in the drawings. This is merely for the convenience of description and does not indicate or imply that the device or element must have a specific orientation, be constructed and operated in a specific orientation. Therefore, it cannot be understood as a limitation on the present invention.
[0055] In addition, it should be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0056] See also Figure 1 and Figure 2 As shown, Figure 1 This is a schematic flow chart of an intelligent method for recovering cobalt from cobalt slag using a cobalt removal agent according to an embodiment of the present invention. Figure 2 The present invention is a schematic diagram of the process of purifying cobalt slag in an embodiment of the present invention. The present invention provides an intelligent method for recovering cobalt from cobalt slag with a cobalt removal agent, comprising:
[0057] Step S1, a first stage of purification, obtaining a mixed slag leaching solution, determining an initial cadmium content in the mixed slag leaching solution, and calculating a preset added mass according to the initial cadmium content;
[0058] Step S2, adding zinc powder to the mixed slag leachate with a preset addition mass, stirring the reaction for 30 minutes under a first water bath temperature condition, filtering, obtaining a primary filtrate, and determining a first actual content of zinc, cadmium, cobalt, nickel, and iron in the primary filtrate;
[0059] The preset added mass is 0.9 times the cadmium content, and the first water bath temperature condition is a constant water bath temperature of 45-50°C;
[0060] Step S3, second-stage purification, obtaining the primary filtrate, adding an activator under the second water bath temperature condition, stirring and reacting for 10 minutes, calculating the amount of cobalt removal agent added according to the first actual content, adding the cobalt removal agent to the filtrate with the amount of cobalt removal agent added, continuing to stir and react for 90 minutes, and then filtering to obtain a secondary filtrate as a cobalt removal liquid, and a filter residue as a cobalt removal agent residue;
[0061] The amount of the activator added is one tenth of the mass of the cobalt removal agent added, and the cobalt removal agent is sodium dimethyldithiocarbamate;
[0062] Step S4, three-stage purification, adding sulfuric acid solution to the cobalt removal agent slag for pickling under preset pickling conditions, keeping the water bath at a constant temperature of 75-80° C., stirring and reacting for 60 minutes, and then filtering the liquid to obtain a pickling solution and cobalt slag;
[0063] Among them, the preset pickling conditions are the initial acid sulfuric acid concentration and liquid-to-solid ratio, the initial acid sulfuric acid concentration is between 100g / L-200g / L, and the liquid-to-solid ratio is 5:1;
[0064] Step S5, cobalt slag purification, collecting the cobalt slag for flotation to obtain pure cobalt slag, determining the contents of nickel and cobalt in the pure cobalt slag, and obtaining the average nickel content of the supernatant and the cobalt recovery rate.
[0065] In step S1, the mixed slag leaching liquid, i.e., the cadmium-rich liquid, is obtained, and the actual amount of zinc powder added is accurately calculated according to the cadmium content. The liquid after the reaction is filtered, and the filtrate is a cadmium-depleted liquid, and the filter residue is sponge cadmium. In step S4, after the liquid is filtered, the filtrate is a pickling liquid, and the filter residue is a cobalt slag.
[0066] In the hydrometallurgical zinc smelting, nickel is enriched in the system for a long time, resulting in an increase in the nickel content in the middle and upper supernatant, which affects the production of the subsequent process. The main method of open-circuit nickel at present is to regularly send a batch of two-clean slag to the Austrian furnace for smelting and treatment to achieve the purpose of open-circuit nickel, but the current coal price is high, the processing cost is large, and the Austrian furnace needs to process other materials such as leached slag, and the processing of two-clean slag will occupy the Austrian furnace time. Therefore, the comprehensive recovery method is used to remove nickel while removing cobalt. Under the conditions of stable nickel content in zinc concentrate and stable leaching rate, the nickel content in the middle and upper supernatant is reduced to below 20 mg / L, and the flotation method is used to effectively separate cobalt from cobalt slag by utilizing the hydrophobicity difference of minerals to achieve the separation of large particles and impurities, thereby extracting relatively pure cobalt slag, and then providing a basis for subsequent cobalt recovery, real-time monitoring of the addition process, control of valve opening and scraper collection of foam, ensuring stable operation process, improving recovery efficiency, and obtaining pure cobalt slag through intelligent recovery methods to effectively recover cobalt from cobalt slag. It combines real-time monitoring and data analysis technology to achieve sustainable recovery of cobalt.
[0067] Specifically, in step S5, it includes:
[0068] Step S501, pre-treating the cobalt slag to obtain cobalt slag sample particles for later use;
[0069] The pretreatment includes drying and crushing, crushing the cobalt slag within a preset crushing particle size range to obtain the cobalt slag sample particles whose actual crushing particle size is within the preset crushing particle size range, and the preset crushing particle size range is 0.1 mm-1 mm;
[0070] Step S502, slurry preparation, mixing the cobalt slag sample particles with water to form slurry;
[0071] Step S503, controlling the valve to open, so as to add flotation reagents to the slurry to be processed in a stirring state, and introducing air into the slurry to be processed at a preset air flow rate, and monitoring the adding process in real time to obtain flotation froth;
[0072] Step S504, controlling the scraper to collect the flotation foam to obtain a foam product, and drying the foam product to obtain pure cobalt slag;
[0073] The flotation reagent is composed of xanthate, lignin and rosin acid, and the mass ratio of each component is 1:1:1.
[0074] In this embodiment, the concentration of the slurry is between 10% and 30%, and is selected and adjusted according to the flotation equipment and the properties of the mineral. It is only necessary to ensure that the cobalt slag sample particles are completely dissolved. By fully stirring the slurry, the reagent is evenly distributed and reacts with the mineral surface, thereby promoting the hydrophobicity of the cobalt mineral.
[0075] During the flotation process, bubbles will gradually form a foam layer, which is rich in cobalt minerals. Finally, the foam layer formed on the surface of the pulp is clearly separated from the sediment at the bottom, which is easy to separate. The bubble generation rate and sedimentation rate are monitored to improve the flotation efficiency and obtain a stable foam layer. By analyzing the effect of the addition of flotation reagents on the bubble generation rate and sedimentation rate, the addition amount of flotation reagents is controlled in time to ensure sufficient flotation reagents to stabilize the foam. At the same time, the negative impact of excessive addition of flotation reagents on flotation efficiency is avoided. The addition process is monitored in real time, the valve opening and scraper collection of foam are controlled to ensure stable operation and improve recovery efficiency. The flotation process is optimized through dynamic monitoring and adjustment strategies to improve flotation efficiency and the recovery rate and purity of cobalt.
[0076] Specifically, real-time monitoring of the addition process to obtain flotation foam includes:
[0077] Taking a continuous bubble image of the surface of the slurry to be processed, and analyzing the bubbles in the continuous bubble image to determine whether to adjust the preset air flow rate;
[0078] Taking initial pulp images and continuous flotation sedimentation images from the side of the pulp to be processed;
[0079] Calculating the initial color value of the initial pulp image and the average color value corresponding to each continuous flotation sedimentation image;
[0080] Calculate the percentage of the average color value corresponding to any continuous flotation sedimentation image to the initial color value to obtain the real-time sedimentation rate;
[0081] Whether to control the valve to be closed is determined according to the real-time sedimentation rate, thereby forming flotation foam.
[0082] Since the color of the impurity particles is darker, the color of the slurry becomes lighter after sedimentation. Therefore, in this embodiment, the sedimentation rate is characterized by calculating the percentage change of the slurry color relative to the initial color. The standard sedimentation rate is set to 20%, which means that when the percentage change of the slurry color relative to the initial color reaches 20%, the slurry color has become lighter. At this time, the sedimentation process is progressing well. The initial color value is R=120, G=100, and B=80. The RGB component of each pixel is analyzed to calculate the average color value of the slurry. When it is determined that the real-time sedimentation rate is greater than the standard sedimentation rate, it means that the average color value reaches or exceeds the set threshold, that is, R≥140, G≥120, and B≥100. The color change is monitored in real time to analyze the sedimentation process, and the changes in the sedimentation process are discovered in time. By monitoring the color change rate, the operating parameters are adjusted in time, the flotation process is optimized, and the flotation recovery efficiency is improved.
[0083] By analyzing the data during the recycling process, the process parameters are optimized to improve the recovery rate and purity of cobalt.
[0084] See also Figure 3 As shown, it is a logic determination diagram for adjusting the preset air flow rate according to an embodiment of the present invention;
[0085] Specifically, the analysis of bubbles in the continuous bubble image includes:
[0086] Obtain any bubble image and the next adjacent bubble image for bubble recognition and contour marking respectively, obtain the sum of the newly added bubble position and the newly added contour area in the adjacent bubble image, obtain the real-time bubble generation rate, and determine the real-time bubble generation rate according to the standard bubble generation rate.
[0087] If the real-time bubble generation rate is less than or equal to the standard bubble generation rate, the preset air flow rate is increased to the corrected air flow rate;
[0088] If the real-time bubble generation rate is greater than the standard bubble generation rate, a continuous flotation sedimentation image is taken on the side of the slurry to be processed, and the real-time sedimentation rate is obtained according to the flotation sedimentation image;
[0089] Wherein, Qc'=min{Qc×[1+(Vb-Vs) / Vb], Qmax}, Qc' is the corrected air flow, Qc is the preset air flow, Vs is the calculated real-time bubble generation rate, Vb is the set standard bubble generation rate, and Qmax is the maximum air flow of the device;
[0090] The standard bubble generation rate in this embodiment represents the volume change of bubbles. Generally, the standard bubble generation rate is set to generate 1000 square pixels per minute to 10000 square pixels of bubbles per minute. It is adjusted according to the resolution of the image, the specifications of the flotation equipment and the actual needs. The maximum air flow rate is 3dm 3 / s, and adjust according to the actual device specifications.
[0091] When it is determined that the real-time bubble generation rate is greater than the standard bubble generation rate, the associated sedimentation process is analyzed to control the valve closure in time and stop adding the flotation agent to avoid excessive addition of flotation agent, which will cause excessive bubble generation and make the bubbles too viscous, thereby reducing the flotation efficiency.
[0092] See also Figure 4 As shown, it is a logic determination diagram for controlling valve closing according to an embodiment of the present invention;
[0093] Specifically, when the real-time bubble generation rate is greater than the standard bubble generation rate, the real-time sedimentation rate is compared with the standard sedimentation rate.
[0094] If the real-time sedimentation rate is less than or equal to the standard sedimentation rate, the valve is controlled to close;
[0095] If the real-time sedimentation rate is greater than the standard sedimentation rate, a flotation sedimentation curve is drawn according to the continuous flotation sedimentation image, and whether to control the valve to be closed is determined according to the flotation sedimentation curve.
[0096] Image recognition technology is used to analyze the color changes of cobalt slag slurry, effectively monitor the sedimentation process, and analyze the speed of color change to analyze the sedimentation efficiency. If the real-time sedimentation rate is determined to be less than or equal to the standard sedimentation rate, it means that the flotation efficiency is not high. This is caused by excessive addition of reagents. In this case, the valve should be closed in time to stop adding flotation reagents to avoid the influence of excessive reagents on the flotation effect.
[0097] Specifically, determining whether to control the valve to be closed according to the flotation sedimentation curve includes:
[0098] Obtaining the average gray value corresponding to each continuous flotation sedimentation image;
[0099] The average gray value is plotted over time according to the preset acquisition time, and a linear fit is performed to obtain the average gray value fitting curve;
[0100] The maximum slope of the average grayscale fitting curve is taken as the image grayscale change rate;
[0101] Obtaining the grayscale change rate of each image in each preset acquisition period, and drawing a curve of the grayscale change rate of each image over time as the flotation sedimentation curve;
[0102] The change trend of the flotation sedimentation curve is determined, and when a peak value appears in the flotation sedimentation curve, the valve is controlled to be closed, and it is determined that the bubbles on the surface of the ore pulp to be processed form flotation foam;
[0103] When no peak appears in the flotation sedimentation curve, the valve is not controlled to be closed.
[0104] In this embodiment, the preset acquisition duration is set to 5 seconds; the preset acquisition interval is 1 second;
[0105] In this embodiment, the mean filtering method is used to filter the continuous sedimentation process images. The grayscale values of all pixels on any image are added and then divided by the total number of pixels to obtain the average grayscale value of the corresponding sedimentation process image. A linear fit of "average grayscale value-time" is performed every five frames of images, and the fitting curve with a correlation coefficient greater than 0.9 is taken, and the maximum slope is taken as the image grayscale change rate.
[0106] The flotation sedimentation process is monitored by joint image recognition technology. During the flotation process of cobalt slag slurry, the impurity particles with strong hydrophilicity will not adhere to the bubbles, but will settle to the bottom. As the solid particles suspended in the slurry settle to the bottom, the concentration of suspended matter is reduced and the slurry transmittance will increase. Therefore, the image grayscale change rate represents the sedimentation rate.
[0107] Specifically, the experimental process to explore the effect of cobalt removal agent on indium extraction is as follows:
[0108] Experiment 1: Take 200 mL of the filtrate, keep it in a water bath at a constant temperature of 30°C, add it to a separatory funnel, then add 100 mL of the extractant, and oscillate and extract for 2 minutes. After the organic phase and the aqueous solution are separated, the In content of the liquid before and after the extraction is determined, and the extraction rate is calculated.
[0109] Experiment 2: Take 1000mL of the filtrate, add 5g of cobalt removal agent and 0.5g of activator, keep the temperature in a water bath at 85℃, stir and react for 2 hours, filter the liquid, cool the filtrate and keep the temperature in a water bath at 30℃, take 200mL of the filtrate and add it to the separatory funnel, add 100mL of the extractant, oscillate and extract for 2 minutes, separate the organic phase and the aqueous solution after they are separated, determine the In content of the liquid before and after the extraction, and calculate the extraction rate.
[0110] Experiment 3: Take 1000mL of the filtrate, add 15g of cobalt removal agent and 1.5g of activator, keep the temperature in a water bath at 85℃, stir and react for 2 hours, filter the liquid, cool the filtrate and keep the temperature in a water bath at 30℃, take 200mL of the filtrate and add it to the separatory funnel, add 100mL of the extractant, oscillate and extract for 2 minutes, separate the organic phase and the aqueous solution after they are separated, determine the In content of the liquid before and after the extraction, and calculate the extraction rate.
[0111] Experiment 4: Take 1000mL of the filtrate, add 5g of cobalt removal agent, 0.5g of activator, keep the temperature in a water bath at 85℃, stir and react for 2 hours, filter the liquid, add 5g of activated carbon to the filtrate and stir and react for 20 minutes, filter the liquid, cool the filtrate and keep the temperature in a water bath at 30℃, take 200mL of the filtrate and add it to the separatory funnel, add 100mL of the extractant, oscillate and extract for 2 minutes, separate the organic phase and the aqueous solution after they are separated, determine the In content of the liquid before and after the extraction, and calculate the extraction rate.
[0112] Experiment 5: Take 1000mL of the filtrate, add 15g of cobalt removal agent and 1.5g of activator, keep the temperature in a water bath at 85℃, stir and react for 2 hours, filter the liquid, add 5g of activated carbon to the filtrate and stir and react for 20 minutes, filter the liquid, cool the filtrate and keep the temperature in a water bath at 30℃, take 200mL of the filtrate and add it to the separatory funnel, add 100mL of the extractant, oscillate and extract for 2 minutes, separate the organic phase and the aqueous solution after they are separated, determine the In content of the liquid before and after extraction, and calculate the extraction rate.
[0113] The experimental results are shown in Table 1.
[0114] Table 1
[0115]
[0116] According to Table 1, the cobalt removal agent has no effect on indium extraction.
[0117] Specifically, the effect of cobalt removal agent slag pickling solution on indium extraction was investigated and verified by the following experiments:
[0118] Experiment 1: Pre-extraction liquid: Take 1000mL of the first filtrate, add distilled water and concentrated sulfuric acid (98%), make the volume to 2000mL, make the liquid contain H2SO4 to reach 170g / L, take a sample and test the indium content of the pre-extraction liquid.
[0119] Experiment 2: Pre-extraction liquid: Take 1000mL of cobalt slag pickling liquid, add clean filtrate and concentrated sulfuric acid (98%), make the volume to 2000mL, make the liquid contain H2SO4 to reach 170g / L, take a sample and test the indium content of the pre-extraction liquid.
[0120] Preparation of cobalt slag pickling solution in Experiment 2: Take 4000mL of cadmium-rich solution (i.e., mixed slag leaching solution) from the comprehensive recovery workshop, add 50g of zinc powder, keep the water bath at a constant temperature of 65-70℃, stir and react for 40 minutes, filter, and test the filtrate for cadmium and cobalt. Add 50g of zinc powder again, keep the water bath at a constant temperature of 65-70℃, stir and react for 30 minutes, filter, and test the filtrate to find out if the cadmium content is less than 50mg. Add a cobalt removal agent at 20 times the cobalt content in the filtrate, keep the water bath at a constant temperature of 80℃, stir and react for 2 hours, filter, and obtain the cobalt removal agent slag. Mix the obtained slag with 1000mL of electrolytic waste liquid, add an appropriate amount of sulfuric acid (1:1) to make the liquid contain 180g / L of H2SO4, bath at 80℃, stir and react for 2 hours, filter to obtain the cobalt slag pickling solution, and test the H2SO4 content in the cobalt slag pickling solution.
[0121] The experiment recycled the organic phase according to the process of extraction - sulfuric acid washing - hydrochloric acid stripping - oxalic acid washing. The specific operations of each process are as follows:
[0122] (1) Extraction: Take 100 mL of lean organic phase and 200 mL of pre-extraction solution and add them into a 1000 mL separatory funnel. Oscillate and extract for 2 minutes. Let the layers stand and release the aqueous phase, which is the raffinate. The raffinate is tested for indium content.
[0123] (2) Sulfuric acid washing: Take 100 mL of 100 g / L sulfuric acid solution and add it to the separatory funnel in (1), mix it with the loaded organic phase, extract it by oscillation for 2 minutes, let it stand and separate the layers, and discard the aqueous phase.
[0124] (3) Hydrochloric acid stripping: Take 100 mL of 6 mol / L hydrochloric acid solution and add it to the separatory funnel in (2), mix it with the loaded organic phase, extract it by oscillation for 2 minutes, let it stand and separate the layers, and release the aqueous solution phase, which is the stripping solution. The stripping solution is tested for indium content.
[0125] (4) Oxalic acid washing: Take 100 mL of 7% oxalic acid solution and add it to the separatory funnel in (3), mix it with the lean organic phase, extract it by oscillation for 2 minutes, let it stand to separate the layers, discard the aqueous phase, and return the organic phase to (1) for recycling.
[0126] Specifically, the following experiments were conducted to investigate whether the cobalt removal agent would be enriched in the organic phase during use, resulting in a significant decrease in the extraction rate:
[0127] Experiment 3: Pre-extraction solution: Take 2000 mL of the clean filtrate as the pre-extraction solution and test the indium content.
[0128] Experiment 4: Pre-extraction liquid: Take 2000mL of clean filtrate, add 10g of cobalt removal agent and 1g of activator, keep the water bath at a constant temperature of 80℃, stir and react for 2 hours, filter the liquid, and the filtrate is the pre-extraction liquid, and test the indium content.
[0129] Experiment 5: Pre-extraction liquid: Take 2000mL of clean filtrate, add 10g of cobalt removal agent, 1g of activator, keep the water bath temperature at 80℃, stir and react for 2 hours, filter the liquid, add 10g of activated carbon to the filtrate, stir and adsorb for 30 minutes, filter, and the filtrate is the pre-extraction liquid, test the indium content.
[0130] The experiment recycled the organic phase according to the process of extraction-sulfuric acid washing-hydrochloric acid stripping-oxalic acid washing, and carried out 6 cycle experiments. The specific operation methods of each process were the same as those in the experiment to explore the effect of cobalt removal agent slag pickling solution on indium extraction.
[0131] The experimental results are shown in Table 2.
[0132] Table 2
[0133]
[0134] According to Table 2, the cobalt slag pickling solution has no effect on indium extraction.
[0135] Specifically, the nickel content and cobalt recovery rate of the supernatant measured at different times by the method of the embodiment of the present invention were compared with the nickel content and cobalt recovery rate of the supernatant measured by the conventional nickel removal method. The comparison results are shown in Table 3;
[0136] There are two comparison items, which are divided into comparative examples and examples. The comparative example represents the average nickel content and cobalt recovery rate of the supernatant measured in June by adopting a conventional nickel removal method, that is, regularly sending a batch of clean slag after the second stage purification to the Austrian furnace for smelting treatment. The example represents the average nickel content and cobalt recovery rate of the supernatant measured by adopting the method of the embodiment of the present invention, that is, removing nickel by a wet treatment method while removing cobalt. The example includes the test results in November and December.
[0137] Table 3 is a comparison and result of the average nickel content of the supernatant measured in the examples of the present invention and the comparative examples;
[0138] Table 3
[0139]
[0140] According to Table 3, the wet treatment method of this embodiment achieves the effect of removing nickel while removing cobalt. The average nickel content in the supernatant in November is 18 mg / L, which is 44 mg / L lower than that in June. The average nickel content in the supernatant in December is 21 mg / L, which is 41 mg / L lower than that in June. This shows that the method provided in this embodiment has certain feasibility and provides experimental data that can confirm that the above method can remove nickel while removing cobalt.
[0141] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.
[0142] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An intelligent method for recovering cobalt from cobalt slag with cobalt removal agent, It is characterized in that include, A first stage of purification, obtaining a mixed slag leaching solution, determining an initial cadmium content in the mixed slag leaching solution, and calculating a preset addition mass according to the initial cadmium content; Adding zinc powder to the mixed slag leachate with a preset added mass, stirring and reacting for 30 minutes under a first water bath temperature condition, filtering, obtaining a primary filtrate, and determining a first actual content of zinc, cadmium, cobalt, nickel, and iron in the primary filtrate; Second stage purification, obtaining the primary filtrate, adding an activator under the second water bath temperature condition, stirring and reacting for 10 minutes, calculating the amount of cobalt removal agent added according to the first actual content, adding the cobalt removal agent to the filtrate with the amount of cobalt removal agent added, continuing to stir and react for 90 minutes, and then filtering to obtain a secondary filtrate as a cobalt removal liquid, and a filter residue as a cobalt removal agent residue; Three-stage purification, adding sulfuric acid solution to the cobalt removal agent slag under preset pickling conditions for pickling, keeping the water bath at a constant temperature of 75-80° C., stirring and reacting for 60 minutes, and then filtering the liquid to obtain a pickling solution and cobalt slag; Purifying cobalt slag, collecting the cobalt slag for flotation to obtain pure cobalt slag, determining the contents of nickel and cobalt in the pure cobalt slag, and obtaining the average nickel content of the supernatant and the cobalt recovery rate; The flotation process is monitored by obtaining a continuous bubble image on the surface of the slurry to be processed, and the real-time bubble generation rate is calculated according to the continuous bubble image. When the real-time bubble generation rate is greater than the standard bubble generation rate, a continuous flotation sedimentation image is obtained to calculate the real-time bubble generation rate, and when the real-time sedimentation rate is greater than the standard sedimentation rate, a flotation sedimentation curve is drawn. When it is determined that a peak appears in the flotation sedimentation curve, the addition of flotation reagents is stopped to obtain flotation foam, thereby obtaining pure cobalt slag.
2. The intelligent recovery method of cobalt in cobalt slag with cobalt removal agent according to claim 1, It is characterized in that The cobalt slag is collected for flotation to obtain pure cobalt slag including: Pre-treating the cobalt slag to obtain cobalt slag sample particles for later use; Mixing the cobalt slag sample particles with water to form a slurry to be processed; Control the valve to open so as to add the flotation reagent to the slurry to be processed in a stirring state, and introduce air into the slurry to be processed at a preset air flow rate, and monitor the adding process in real time to obtain flotation froth; Controlling the scraper to collect the flotation foam to obtain a foam product, and drying the foam product to obtain pure cobalt slag; The flotation reagent is composed of xanthate, lignin and rosin acid, and the mass ratio of each component is 1:1:
1.
3. The intelligent recovery method of cobalt in cobalt slag with cobalt removal agent according to claim 2, It is characterized in that Real-time monitoring of the addition process to obtain flotation foam including, photographing the continuous bubble image on the surface of the slurry to be processed, and analyzing the bubbles in the continuous bubble image to determine whether to adjust the preset air flow rate; Taking initial pulp images and continuous flotation sedimentation images from the side of the pulp to be processed; Calculating the initial color value of the initial pulp image and the average color value corresponding to each continuous flotation sedimentation image; Calculate the percentage of the average color value corresponding to any continuous flotation sedimentation image to the initial color value to obtain the real-time sedimentation rate; Whether to control the valve to be closed is determined according to the real-time sedimentation rate, thereby forming flotation foam.
4. The intelligent recovery method of cobalt in cobalt slag with cobalt removal agent according to claim 3, It is characterized in that Analysis of bubbles in continuous bubble images includes, The real-time bubble generation rate is calculated based on the continuous bubble image, and the real-time bubble generation rate is determined based on the standard bubble generation rate. If the real-time bubble generation rate is less than or equal to the standard bubble generation rate, the preset air flow rate is increased to the corrected air flow rate; If the real-time bubble generation rate is greater than the standard bubble generation rate, the continuous flotation sedimentation image is photographed on the side of the slurry to be processed, and the real-time sedimentation rate is obtained according to the flotation sedimentation image.
5. The intelligent recovery method of cobalt in cobalt slag with cobalt removal agent according to claim 4, It is characterized in that When the real-time bubble generation rate is greater than the standard bubble generation rate, the real-time sedimentation rate is compared with the standard sedimentation rate. If the real-time sedimentation rate is less than or equal to the standard sedimentation rate, the valve is controlled to close; If the real-time sedimentation rate is greater than the standard sedimentation rate, a flotation sedimentation curve is drawn according to the continuous flotation sedimentation image, and whether to control the valve to be closed is determined according to the flotation sedimentation curve.
6. The intelligent recovery method of cobalt in cobalt slag with cobalt removal agent according to claim 5, It is characterized in that Determining whether to control the valve to be closed according to the flotation sedimentation curve includes: Obtaining the average gray value corresponding to each continuous flotation sedimentation image; The average gray value is plotted over time according to the preset acquisition time, and a linear fit is performed to obtain the average gray value fitting curve; The maximum slope of the average grayscale fitting curve is taken as the image grayscale change rate; Obtaining the grayscale change rate of each image in each preset acquisition period, and drawing a curve of the grayscale change rate of each image over time as the flotation sedimentation curve; The change trend of the flotation sedimentation curve is determined, and when a peak value appears in the flotation sedimentation curve, the valve is controlled to be closed, and it is determined that the bubbles on the surface of the ore pulp to be processed form flotation foam; When no peak appears in the flotation sedimentation curve, the valve is not controlled to be closed.
7. The intelligent recovery method of cobalt in cobalt slag with cobalt removal agent according to claim 4, It is characterized in that Calculation of real-time bubble generation rate based on continuous bubble images includes, Obtain an arbitrary bubble image and a next adjacent bubble image to perform bubble recognition and contour marking respectively; The sum of the newly added bubble positions and the newly added inner contour areas in the adjacent bubble images is obtained to obtain the real-time bubble generation rate.
8. The intelligent recovery method of cobalt in cobalt slag with cobalt removal agent according to claim 2, It is characterized in that Pre-treating the cobalt slag comprises: The cobalt slag is dried and crushed within a preset crushing particle size range to obtain the cobalt slag sample particles whose actual crushing particle size is within the preset crushing particle size range, and the preset crushing particle size range is 0.1 mm-1 mm.
9. The intelligent recovery method of cobalt in cobalt slag with cobalt removal agent according to claim 1, It is characterized in that The preset added mass is 0.9 times of the initial cadmium content, and the first water bath temperature condition is a constant water bath temperature of 45-50°C.
10. The intelligent recovery method of cobalt in cobalt slag with cobalt removal agent according to claim 1, It is characterized in that The amount of the cobalt removal agent added is 5-10 times the sum of the mass of cobalt and nickel, or 4-8 times the sum of the mass of cadmium and iron. The amount of the activator added is one tenth of the amount of the cobalt removal agent added. The cobalt removal agent is sodium dimethyldithiocarbamate.