A sewage denitrification carrier and its preparation method and preparation system

By heating, melting and extruding the method during the transportation process, the complexity and energy consumption problems in the preparation process of the sulfur autotrophic denitrification carrier are solved, and the high yield and uniformity of the carrier are achieved, which is suitable for production of different scales. , and improve the denitrification effect.

CN118598358BActive Publication Date: 2024-10-25SCIMEE TECH & SCI CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411067367.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-25
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The existing preparation process of sulfur autotrophic denitrification carriers has problems such as complex procedures, high energy consumption, difficulty in temperature control, low yield, low particle strength and poor particle size heterogeneity. In addition, there is a lot of waste and it is difficult to achieve continuous production.

Method used

The method of heating, melting, mixing, and extrusion molding during the transportation process is adopted. The twin-screw melt extrusion device is used to propel the transportation, mixing, and heating and melting. The temperature is controlled in stages for heating and melting to ensure that the sulfur is melted to a viscous state and combined with calcium carbonate. And magnetic powder is used as auxiliary materials to control the particle size and shape to achieve carrier uniformity and high yield.

Benefits of technology

It achieves uniform mixing of carrier materials, high particle strength, high yield, and less waste. It is suitable for large, medium and small production scales, and improves production efficiency and denitrification effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118598358B_ABST
    Figure CN118598358B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of preparation of sewage denitrification carriers, and discloses a sewage denitrification carrier and a preparation method and a preparation system thereof, wherein the method comprises the following steps: S1, mixing crushed sulfur and auxiliary materials according to a formula, and obtaining a raw material mixture; S2, mixing and heating and melting the raw material mixture during transportation, wherein the heating and melting temperature is 145-190°C, and then extruding and molding; S3, cooling and cutting the extruded strip mixture to obtain a denitrification carrier. The method and system can directly produce the raw materials after mixing, and directly obtain the carrier by heating, melting, mixing, and extruding during transportation, without step-by-step addition of processed materials, and can realize continuous production. The obtained carrier has high mechanical compressive strength, uniform material mixing, good particle size uniformity, high yield rate, less waste, and convenient recycling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sewage denitrification carrier preparation, and in particular relates to a sewage denitrification carrier and a preparation method and a preparation system thereof. Background Art

[0002] At present, sulfur autotrophic denitrification technology is widely used and mature in sewage denitrification treatment. Sulfur autotrophic denitrification is an autotrophic denitrification technology that uses elemental sulfur as an electron donor to reduce nitrate and nitrite to nitrogen. However, the use of elemental sulfur has problems such as sulfur being fragile, difficult to backwash, and acidification of effluent. Therefore, composite sulfur autotrophic denitrification carriers containing sulfur and other materials are usually used on the market.

[0003] The existing preparation process of sulfur autotrophic denitrification carrier mostly adopts wet underwater granulation method: first, the raw materials are mixed and added to the melting tank for heating and melting, or the sulfur is melted first and then other auxiliary materials are added to the molten sulfur for stirring and mixing, and then flow into the distributor, and the material drips into the water cooling device below by its own gravity, forming spherical particles that sink to the bottom of the water, and finally drains the water and sieves to obtain the sulfur autotrophic composite carrier. However, this preparation process has problems such as complex procedures, high energy consumption, long melting time, difficult temperature control, low yield, low particle strength, etc., and the particle size uniformity of the obtained denitrification carrier is poor, and a lot of waste is generated. Summary of the invention

[0004] In view of the defects of the above-mentioned prior art, the present invention provides a wastewater denitrification carrier and a preparation method and system thereof. The method and system can directly produce after mixing the raw materials, and directly prepare the carrier by heating, melting, mixing and extrusion molding during the transportation process. There is no need to add and process materials in steps, and continuous production can be achieved. The prepared carrier materials are evenly mixed, have good particle size uniformity, high yield, less waste and are easy to recycle.

[0005] The technical solution adopted by the present invention is as follows:

[0006] A method for preparing a wastewater denitrification carrier comprises the following steps:

[0007] S1, mixing crushed sulfur and auxiliary materials according to a formula to obtain a raw material mixture;

[0008] S2, mixing and heating the raw material mixture during transportation, wherein the heating and melting temperature is 145-190° C., and then extruding and molding;

[0009] S3, cooling and cutting the extruded strip mixture into shapes to obtain a denitrification carrier.

[0010] In one embodiment of the present application, the sulfur is a sulfur sheet with a thickness of 0.5-1.0 mm and a diameter of 5-10 mm;

[0011] And / or, the auxiliary material is calcium carbonate powder, and the sieve particle size of the calcium carbonate powder is 3000-5000 mesh;

[0012] And / or, the auxiliary material includes magnetic powder, and the sieve particle size of the magnetic powder is 300-400 mesh;

[0013] And / or, the mass ratio of the sulfur to the auxiliary material is 20-22:1.

[0014] In one embodiment of the present application, in step S2, a twin-screw melt extruder is used to carry out propulsion, mixing, heating, melting and extrusion molding;

[0015] The conveying and extrusion speed is 0.1~10cm / s.

[0016] In one embodiment of the present application, in step S2, mixing and heating and melting during the conveying process are performed by segmented temperature-controlled heating and melting, including 5 to 10 temperature-controlled sections.

[0017] In one embodiment of the present application, in the segmented temperature-controlled heating and melting, the temperature of the front-end temperature-controlled section is lower than the temperature of the rear-end temperature-controlled section, and the temperature of the rear-end temperature-controlled section is lower than the temperature of the middle temperature-controlled section.

[0018] In one embodiment of the present application, the segmented temperature-controlled heating and melting includes 10 temperature control sections, the heating and melting temperature is 145~170°C, and the temperature control ranges of the temperature control sections from front end to rear end are 145~150°C, 150~155°C, 155~160°C, 160~165°C, 165~170°C, 165~170°C, 165~170°C, 165~170°C, 160~165°C, and 155~160°C respectively.

[0019] In one embodiment of the present application, step S3 includes:

[0020] S3-1, water-cooling or air-cooling the extruded strip mixture to set the shape, air-drying the strip mixture after setting the shape, cutting the strip mixture into shapes after drying, and sieving the strip mixture to obtain a denitrification carrier;

[0021] or,

[0022] S3-2, the extruded strip mixture is water-cooled or air-cooled to set the shape, air-dried after setting, cut into shapes after drying, and then crushed and sieved to obtain a denitrification carrier.

[0023] In one embodiment of the present application, in step S3-1, the cross-sectional area of ​​the extrusion port of the extrusion molding is 0.1~0.2cm2 , cutting length is 3~10mm;

[0024] In step S3-2, the cross-sectional area of ​​the extrusion port during extrusion molding is 0.2 to 0.5 cm 2 , the crushed particle size is controlled at 3~6mm.

[0025] In one embodiment of the present application, the screened undersize material is returned to step S1 as a raw material mixture.

[0026] A sewage denitrification carrier, the denitrification carrier is prepared by any of the above sewage denitrification carrier preparation methods, the particle size of the denitrification carrier is 3-6 mm, and it also satisfies one or more of the following properties:

[0027] Uneven coefficient K 80 ≤1.5;

[0028] Uniformity coefficient K 60 ≤1.35;

[0029] Mechanical compressive strength ≥135N;

[0030] Crushing rate ≤ 0.02%;

[0031] The breakage rate is ≤0.04%.

[0032] In one embodiment of the present application, the auxiliary materials include calcium carbonate and magnetic powder.

[0033] A sewage denitrification carrier preparation system applicable to any of the above sewage denitrification carrier preparation methods, comprising:

[0034] Powder mixing device;

[0035] A first feeding device, the front end of which is connected to the discharge port of the powder mixing device;

[0036] A melt extrusion device, comprising a twin-screw mainframe and a heating module, wherein the inlet of the twin-screw mainframe corresponds to the rear end of the first feeding device, and the heating module is arranged outside the barrel of the twin-screw mainframe to heat and melt the material in the barrel of the twin-screw mainframe, and the twin-screw mainframe conveys and mixes the material, and extrudes and forms it from the end;

[0037] A cooling and cutting device, arranged after the melt extrusion device, is used to cool and cut the extruded material;

[0038] A screening device, arranged after the cooling and cutting device;

[0039] The second feeding device is connected to the undersize material of the screening device and the first feeding device, and recovers the undersize material to the first feeding device.

[0040] In one embodiment of the present application, the cooling and cutting device comprises a cooling water tank, an air dryer and a pelletizer;

[0041] And / or, it also includes a crusher, which is arranged between the cooling and cutting device and the screening device to crush the coarse carrier formed by cooling and cutting.

[0042] In one embodiment of the present application, the heating module includes 5-10 temperature control sections, and the 5-10 temperature control sections are connected in sequence to control the heating temperature respectively.

[0043] In one embodiment of the present application, a natural exhaust port is provided in the middle of the barrel of the twin-screw main engine, and a vacuum exhaust port is provided at the rear end.

[0044] Compared with the prior art, the present invention has the following beneficial effects:

[0045] 1. The sewage denitrification carrier of the present invention and its preparation method and preparation system directly produce the raw materials after mixing them, and directly prepare the carrier by heating, melting, mixing and extrusion molding during the transportation process, without step-by-step addition of processed materials, continuous production, accurate control of extrusion speed, avoiding the problem of uncontrollable extrusion speed during gravity dripping, and the prepared denitrification carrier material is evenly mixed and has high particle strength; through extrusion and cutting control, the particle size uniformity is good, the yield is high, the waste is small and the recycling is convenient. In addition, the method is not affected by the production scale and can be applied to large, medium and small production scales.

[0046] 2. The shape and particle size of sulfur as the main material and calcium carbonate, magnetic powder, etc. as auxiliary materials need to be controlled, and they need to be initially mixed before spiral conveying and heating to ensure that the materials can be completely melted and mixed evenly during the spiral conveying and heating process, thereby ensuring that the obtained carrier materials are mixed evenly.

[0047] 3. By heating and melting in sections with temperature control, and controlling the temperature in a relatively high range of 145~190℃ (the traditional process temperature control is 120~140℃, and the sulfur is in a fluidized state), the sulfur can be quickly melted into a viscous state, and pushed and mixed in the viscous state, which can wrap other auxiliary materials well and make it easier to shape; the sulfur can be mechanically extruded, cooled, and cut in a viscous state, and the carrier obtained has good uniformity (non-uniformity coefficient K 80 ≤1.5, uniformity coefficient K 60 ≤1.35, crushing rate ≤0.02%, breakage rate ≤0.04%); and the carrier particles obtained by cooling and molding from the viscous molten state are denser and have higher hardness. The mechanical compressive strength can reach 138N and above, and can be used in denitrification filter facilities with high filling height and high compressive strength requirements.

[0048] 4. Crushing treatment after cutting can effectively reduce the roughness of the carrier surface, increase its specific surface area and microbial attachment capacity, and improve the denitrification effect of the carrier.

[0049] 5. The sewage denitrification carrier preparation system has simple equipment, eliminating the liquid sulfur insulation system, liquid sulfur insulation transportation system and melting tank in the front end of the traditional process equipment, greatly simplifying the preparation process. The heating module is used to realize segmented temperature control heating and melting during the pushing and mixing process. The temperature control is precise, and the sulfur can be melted to a viscous state in a very short time (1~2min) (the traditional process uses a melting tank that takes about 1~2h to completely melt). The mechanical propulsion extrusion mode is used instead of the traditional melting tank stirring and gravity dripping mode. While streamlining the stirring device, it realizes precise control of the extrusion speed, which can effectively avoid the problem of uncontrollable extrusion speed during gravity dripping, and can realize continuous production. Compared with traditional intermittent production, it can greatly improve production efficiency, and the morphology and particle size of the extruded products are more controllable and uniform. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0051] Figure 1 The figure is a schematic flow chart of the method for preparing a wastewater denitrification carrier according to the present invention.

[0052] Figure 2 The present invention is a flowchart of the system for preparing a wastewater denitrification carrier.

[0053] Figure 3 It is a schematic structural diagram of the melt extrusion device in the present invention.

[0054] Figure 4 These are pictures of the denitrification carrier product obtained by the method for preparing a wastewater denitrification carrier of the present invention; wherein, a, is a picture of the carrier; and b, is a SEM picture of the carrier.

[0055] Reference numerals:

[0056] 1. Melt extrusion device; 11. Twin-screw main machine; 12. Heating module; 121. Natural exhaust port; 122. Vacuum exhaust port. DETAILED DESCRIPTION

[0057] In the following, only some exemplary embodiments are briefly described. As those skilled in the art will appreciate, the described embodiments may be modified in various ways without departing from the spirit or scope of the present invention. Therefore, the drawings and descriptions are considered to be exemplary and non-restrictive in nature.

[0058] In the description of the present invention, it should be understood that the terms "upper", "lower", "front", "back", "inside", "outside", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, or are the orientations or positional relationships in which the products of the present invention are conventionally placed when in use, or are the orientations or positional relationships conventionally understood by those skilled in the art. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0059] The terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0060] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or a communication; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0061] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.

[0062] The disclosure below provides many different embodiments or examples to realize different structures of the present invention. In order to simplify the disclosure of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention.

[0063] The embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0064] The embodiment of the present invention provides a wastewater denitrification carrier and a preparation method and a preparation system thereof, such as Figure 1 As shown, the preparation method comprises the following steps:

[0065] S1, solid raw materials such as sulfur and auxiliary materials are crushed to a certain degree, weighed and configured according to the formula ratio, and after configuration, added into a powder mixing device for preliminary mixing to obtain a raw material mixture.

[0066] S2, mixing and heating the raw material mixture obtained in step S1 during the conveying process, and then extruding and molding the mixture to obtain a strip-shaped mixture.

[0067] Mixing during the conveying process can be achieved by screw conveying, further mixing can be performed during the conveying process, and heating and melting can be performed during the conveying process. Mixing can ensure that the melt and the solid are fully mixed, and ensure that the strip mixture obtained by extrusion has good uniformity.

[0068] S3, cooling and cutting the strip-shaped mixture obtained by extrusion molding in step S2, and obtaining the desired denitrification carrier after cutting and molding.

[0069] The method can directly produce after mixing solid raw materials. By utilizing the fusible property of sulfur, the carrier is directly prepared by heating, melting, mixing and extruding during the transportation process. There is no need to add and process materials in steps, continuous production can be achieved, and the extrusion speed can be accurately controlled to avoid the problem of uncontrollable extrusion speed during traditional gravity dripping. The prepared carrier material is evenly mixed and has high particle strength. The mechanical compressive strength can reach 135N or even above 138N. Through extrusion and cutting control, the particle size uniformity is good, and the uneven coefficient K can be achieved. 80 ≤1.5, uniformity coefficient K 60 ≤1.35; high yield rate, less waste, the crushing rate can reach ≤0.02%, the breakage rate ≤0.04%, and the waste is easy to recycle.

[0070] Among the above raw materials, sulfur is preferably sulfur flakes, and the thickness of the sulfur flakes is controlled to be 0.5~1.0mm and the diameter is 5~10mm. The auxiliary materials include calcium carbonate and / or magnetic powder, and calcium carbonate is preferably calcium carbonate powder, and the sieve particle size of the calcium carbonate powder is controlled to be 3000~5000 mesh; and the sieve particle size of the magnetic powder is controlled to be 300~400 mesh. And the mass ratio of sulfur flakes to auxiliary materials / calcium carbonate powder is controlled to be 20~22:1. Among them, sulfur is mainly used as an electron donor, calcium carbonate is mainly used as an alkalinity donor, and magnetic powder is used as an auxiliary electron donor. Controlling the particle size of the above raw materials within this range can well ensure that the heating is completely melted and mixed evenly during the transportation process, and ensure that the obtained carrier has good uniformity. Controlling the mass ratio of sulfur flakes to auxiliary materials within the above range can not only ensure that the carrier provides electron donors well for autotrophic denitrification and denitrification and solve the problem of water acidification, but also well ensure that the carrier is easy to shape during the preparation process, and the obtained carrier has a stable structure and high hardness.

[0071] In one embodiment, in step S2, the raw material mixture is mixed and heated to melt during the conveying process, and then extruded to form, specifically: a twin-screw melt extruder is used for advancing and conveying, and the mixture is heated, melted and mixed during the advancing and conveying process, and then extruded to form a strip-shaped mixture. The twin-screw method is used for advancing and conveying, and mixing can be performed while conveying, and heating is convenient.

[0072] It is preferred to control the heating and melting temperature during the pushing and conveying process to 145-190°C, and the conveying and extruding speed to 0.1-10 cm / s. This can ensure that the sulfur of the raw material is completely melted to a viscous state during the conveying process, mixed evenly and easy to extrude and shape.

[0073] The conventional wet underwater process generally controls the temperature in the range of 120-140°C, and the sulfur is in a fluidized state and suitable for drop-out molding; when the temperature is too high to around 160°C, the viscosity of the sulfur will increase, reaching a maximum viscosity at 190°C, and then decreasing again after exceeding 190°C. This method utilizes this characteristic of sulfur, controls its melting temperature in a relatively high range, and melts it to a viscous state for extrusion, cooling, cutting and molding. It is suitable for mechanical extrusion molding, easy to shape, and convenient to control the extrusion speed. The obtained carrier has uniform particle size, dense particles, and high hardness, and can save the addition of binders, saving costs.

[0074] Preferably, in step S2, the mixture is mixed and heated and melted during the transportation process, and the heating and melting is segmented temperature-controlled heating and melting, and the heating and melting is usually divided into 5 to 10 continuous temperature-controlled sections; more preferably, the heating and melting can be divided into 7 to 10 continuous temperature-controlled sections. By controlling the temperature separately in multiple temperature-controlled sections, the heating control can be made more precise, ensuring that the sulfur can be melted to a viscous state during the transportation process, and the carrier of the desired shape can be obtained by extrusion molding, and the obtained carrier is dense and has high hardness.

[0075] Furthermore, in the segmented temperature-controlled heating and melting part, the temperature of the temperature-controlled section at the front end is lower than that of the temperature-controlled section at the rear end, and the temperature of the temperature-controlled section at the rear end is lower than that of the temperature-controlled section in the middle. The temperature of the temperature-controlled section in the middle should be within the range of 160-190°C to ensure that the sulfur melts to a viscous state.

[0076] Specifically, in one embodiment, the segmented temperature-controlled heating and melting portion includes 10 temperature control sections, and the heating and melting temperature is controlled within the range of 145-170°C. The segmented temperature-controlled heating and melting portion is sequentially provided with temperature control sections according to the direction of the raw material pushing from front to back, and the temperature control ranges of the temperature control sections from the front end to the rear end are sequentially 145-150°C, 150-155°C, 155-160°C, 160-165°C, 165-170°C, 165-170°C, 165-170°C, 165-170°C, 165-170°C, 160-165°C, and 155-160°C.

[0077] The front end temperature is relatively low, which makes the sulfur melt quickly and has good fluidity, making it easy to fully mix the raw materials during transportation; the middle temperature is relatively high, which makes the sulfur fully melt to a viscous state, and wraps the auxiliary materials well to ensure shaping and extrusion control; the rear end temperature is slightly lower, which is conducive to extrusion molding and rapid cooling molding.

[0078] In step S3, the extruded strip mixture is cooled and cut into shapes to obtain a denitrification carrier, which may specifically include the following embodiments:

[0079] S3-1, the extruded strip mixture is cooled and shaped by water cooling or air cooling, and then air-dried to form a solid and dry strip, and then cut into strips according to the cutting length set as needed, and the cut product is sieved to remove debris to obtain the desired denitrification carrier.

[0080] When step S3-1 is used, the cross-sectional area of ​​the extrusion port is preferably controlled to be 0.1 to 0.2 cm 2 The cutting length is controlled within the range of 3~10mm. Figure 4 As shown, the denitrification carrier prepared by this method has good uniformity in particle size, and carrier particles of different shapes can be obtained by replacing the extrusion head (columnar particles of various shapes can be obtained), which can better meet the use requirements.

[0081] S3-2, the extruded strip mixture is cooled and shaped by water cooling or air cooling, and then air-dried to form a solid and dry strip. After drying, it is first cut and shaped, and then crushed to a certain extent. After the crushing treatment, it is screened to remove debris to obtain the desired denitrification carrier.

[0082] When step S3-2 is used, the cross-sectional area of ​​the extrusion port is preferably controlled to be 0.2 to 0.5 cm 2 The crushing particle size is controlled within the range, so that the obtained carrier particle size is about 3-6 mm. This method further crushes the obtained carrier particles after cutting and forming, which can make the surface of the obtained carrier particles rougher, effectively increase their specific surface area, and have a more irregular morphology. When filling, a carrier filler layer with a higher filling density and better filtration effect can be obtained.

[0083] Furthermore, after the screening process, the sieved debris is recycled back to step S1 as a raw material mixture and further used in steps S2 and S3 to prepare a denitrification carrier. This method can directly recycle waste materials for use, and waste recycling is convenient.

[0084] Based on the same purpose of the invention, an embodiment of the present invention further provides a system for preparing a sewage denitrification carrier, which is suitable for preparing a sewage denitrification carrier using the above method.

[0085] like Figure 2 and Figure 3 As shown, the system includes a powder mixing device, a first feeding device, a melt extrusion device 1, a cooling and cutting device, a screening device and a second feeding device.

[0086] The powder mixing device may include a raw material adding mechanism and a stirring and mixing mechanism, and the raw materials are added according to a proportion and then mixed evenly.

[0087] The first feeding device may be a screw conveyor or a belt conveyor, the front end of which is connected to the discharge port of the powder mixing device, and the rear end is connected to the inlet end of the melt extrusion device 1, for conveying the mixed raw materials to the melt extrusion device 1.

[0088] like Figure 3 As shown, the melt extrusion device 1 includes a twin screw mainframe 11 and a heating module 12. The inlet of the twin screw mainframe 11 corresponds to the rear end of the first feeding device. The twin screw mainframe 11 is used to transport and mix the materials and extrude them from the end. The heating module 12 is arranged outside the barrel of the twin screw mainframe 11 and is used to heat and melt the materials in the barrel of the twin screw mainframe 11. A detachable extrusion head is arranged at the rear end of the twin screw mainframe 11, and an extrusion head with different sizes and shapes of extrusion ports can be selected according to needs.

[0089] The cooling and cutting device is arranged after the melt extrusion device 1, and is used to cool and cut the extruded material. The cooling and cutting device may include a cooling water tank, an air dryer and a pelletizer arranged in sequence, and the extruded material is quickly cooled by water, and then quickly dried by the air dryer before cutting and forming, so that the obtained carrier particles have uniform particle size.

[0090] The screening device is arranged after the cooling and cutting device to screen the cut materials, remove the waste materials and obtain the required carrier. The screening device can be a vibrating screen.

[0091] The second feeding device can be a screw conveyor or a belt conveyor, which is connected to the under-screen of the screening device and the top of the first feeding device to convey the under-screen material (waste material) to the first feeding device for recycling.

[0092] Preferably, the heating module of the melt extrusion device 1 can be set to 5 to 10 temperature control sections, and the 5-10 temperature control sections are connected in sequence to control the heating temperature respectively, so as to realize the precise temperature control heating of the conveyed material in the twin-screw main unit 11, and ensure the precise temperature of the material. More preferably, it can be set to 7 to 10 temperature control sections. The heating module can be temperature-controlled by the thermal oil heating module and the water cooling circulation module in coordination to ensure the precise temperature control of each temperature control section.

[0093] When in use, the temperature of the temperature control section at the front end (close to the inlet end of the twin-screw main body 11) of the heating module 12 is controlled to be lower than the temperature of the temperature control section at the rear end; the temperature of the temperature control section at the rear end is lower than the temperature of the temperature control section in the middle. This can better achieve the melting, mixing and extrusion shaping of materials.

[0094] Preferably, a natural exhaust port 121 is provided in the middle of the barrel of the twin-screw main body 11, corresponding to the temperature control section in the middle of the heating module 12; a vacuum exhaust port 122 is provided at the rear end of the barrel of the twin-screw main body 11, corresponding to the temperature control section at the rear end of the heating module 12, and the vacuum exhaust port 122 is connected to the vacuum pump via a pipeline. The natural exhaust port 121 is provided to timely discharge the air in the barrel of the twin-screw main body 11, which can avoid the generation of bubbles, so that the material fills the barrel, and is better mixed and transported, ensuring the continuity of production and the uniformity of the product; the vacuum exhaust port 122 is provided at the rear end, and the air in the barrel of the twin-screw main body 11 near the extruder head is extracted by negative pressure, ensuring that the final extruded material has no bubbles, a denser texture, a high hardness, and meets the requirements of rapid extrusion preparation.

[0095] In one embodiment, the preparation system further includes a crusher, which is arranged between the cooling and cutting device and the screening device, and is used to crush the coarse carrier formed by cooling and cutting, and then screen it through the screening device after crushing. The crusher can be arranged to crush the carrier after cutting and forming, increase the roughness of the carrier surface, obtain carrier particles with a larger specific surface area, and make the obtained carrier morphology more irregular, which is conducive to filling and obtaining a high-density filler layer.

[0096] The wastewater denitrification carrier preparation system has simple equipment, eliminating the liquid sulfur insulation system, liquid sulfur insulation transportation system and melting tank in the front end of the traditional process equipment, which can greatly simplify the preparation process. The heating module can realize segmented temperature control heating and melting in the pushing and mixing process, and the temperature control is accurate. It can melt the sulfur to a viscous state in a very short time (1~2min) (the traditional process uses a melting tank that takes about 1~2h to completely melt). The mechanical propulsion extrusion mode replaces the traditional melting tank stirring and gravity dripping mode. While streamlining the stirring device, it can achieve precise control of the extrusion speed, which can effectively avoid the problem of uncontrollable extrusion speed during gravity dripping, and can realize continuous production. Compared with traditional intermittent production, it can greatly improve production efficiency, and the morphology and particle size of the extruded product are more controllable and uniform. The system occupies a small area, can realize simple, efficient and miniaturized production, and is suitable for large, medium and small production scales.

Claims

1. A method for preparing a wastewater denitrification carrier, It is characterized in that The steps include: S1, mixing crushed sulfur and auxiliary materials according to a formula to obtain a raw material mixture; S2, mixing and heating the raw material mixture during transportation, wherein the heating and melting temperature is 145-190° C., and then extruding and molding; S3, cooling and cutting the extruded strip mixture into shapes to obtain a denitrification carrier; Wherein, the auxiliary materials include calcium carbonate powder and magnetic powder; In step S2, mixing and heating and melting during the conveying process are staged temperature-controlled heating and melting, wherein the temperature of the front temperature-controlled section is lower than the temperature of the rear temperature-controlled section, and the temperature of the rear temperature-controlled section is lower than the temperature of the middle temperature-controlled section, and the temperature of the middle temperature-controlled section is 160-190°C.

2. The method for preparing a wastewater denitrification carrier according to claim 1, Features: The sulfur is a sulfur sheet with a thickness of 0.5-1.0 mm and a diameter of 5-10 mm; And / or, the sieve particle size of the calcium carbonate powder is 3000-5000 mesh; And / or, the screening particle size of the magnetic powder is 300-400 mesh; And / or, the mass ratio of the sulfur to the auxiliary material is 20-22:

1.

3. The method for preparing a wastewater denitrification carrier according to claim 1 or 2, It is characterized in that In step S2, a twin-screw melt extruder is used to carry out pushing, conveying, mixing, heating, melting and extrusion molding; The conveying and extrusion speed is 0.1~10cm / s.

4. The method for preparing a wastewater denitrification carrier according to claim 3, It is characterized in that The segmented temperature-controlled heating and melting includes 5 to 10 temperature-controlled sections.

5. The method for preparing a wastewater denitrification carrier according to claim 4, It is characterized in that The segmented temperature-controlled heating and melting includes 10 temperature control sections, the heating and melting temperature is 145-170°C, and the temperature control ranges of the temperature control sections from the front end to the rear end are 145-150°C, 150-155°C, 155-160°C, 160-165°C, 165-170°C, 165-170°C, 165-170°C, 165-170°C, 160-165°C, and 155-160°C respectively.

6. The method for preparing a wastewater denitrification carrier according to claim 1, It is characterized in that Step S3 includes: S3-1, water-cooling or air-cooling the extruded strip mixture to set the shape, air-drying the strip mixture after setting the shape, cutting the strip mixture into shapes after drying, and sieving the strip mixture to obtain a denitrification carrier; or, S3-2, the extruded strip mixture is water-cooled or air-cooled to set the shape, air-dried after setting, cut into shapes after drying, and then crushed and sieved to obtain a denitrification carrier.

7. The method for preparing a wastewater denitrification carrier according to claim 6, Features: In step S3-1, the cross-sectional area of ​​the extrusion port during extrusion molding is 0.1-0.2 cm 2 , cutting length is 3~10mm; In step S3-2, the cross-sectional area of ​​the extrusion port during extrusion molding is 0.2 to 0.5 cm 2 , the crushed particle size is controlled at 3~6mm.

8. The method for preparing a wastewater denitrification carrier according to claim 6, It is characterized in that The screened undersize material is returned to step S1 as a raw material mixture.

9. A wastewater denitrification carrier, It is characterized in that The denitrification carrier is prepared by the method for preparing a sewage denitrification carrier according to any one of claims 1 to 8, the particle size of the denitrification carrier is 3 to 6 mm, and also satisfies one or more of the following properties: Uneven coefficient K 80 ≤1.5; Uniformity coefficient K 60 ≤1.35; Mechanical compressive strength ≥135N; Crushing rate ≤ 0.02%; The breakage rate is ≤0.04%.

10. The sewage denitrification carrier according to claim 9, It is characterized in that The auxiliary materials include calcium carbonate and magnetic powder.

11. A system for preparing a wastewater denitrification carrier applicable to the method for preparing a wastewater denitrification carrier according to any one of claims 1 to 8, It is characterized in that include: Powder mixing device; A first feeding device, the front end of which is connected to the discharge port of the powder mixing device; A melt extrusion device, comprising a twin-screw mainframe and a heating module, wherein the inlet of the twin-screw mainframe corresponds to the rear end of the first feeding device, and the heating module is arranged outside the barrel of the twin-screw mainframe to heat and melt the material in the barrel of the twin-screw mainframe, and the twin-screw mainframe conveys and mixes the material, and extrudes and forms it from the end; A cooling and cutting device, arranged after the melt extrusion device, is used to cool and cut the extruded material; A screening device, arranged after the cooling and cutting device; The second feeding device is connected to the undersize material of the screening device and the first feeding device, and recovers the undersize material to the first feeding device.

12. The system for preparing a wastewater denitrification carrier according to claim 11, It is characterized in that The cooling and cutting device comprises a cooling water tank, an air dryer and a pelletizer; And / or, it also includes a crusher, which is arranged between the cooling and cutting device and the screening device to crush the coarse carrier formed by cooling and cutting.

13. The system for preparing a wastewater denitrification carrier according to claim 11, It is characterized in that The heating module comprises 5-10 temperature control sections, which are connected in sequence to control the heating temperature respectively.

14. The system for preparing a wastewater denitrification carrier according to claim 13, It is characterized in that The barrel of the twin-screw main engine is provided with a natural exhaust port in the middle and a vacuum exhaust port at the rear end.

Citation Information

Patent Citations

  • Building sealing strip based on thermoplastic ethylene-propylene-diene monomer (EPDM) rubber material and preparation method of building sealing strip

    CN102181101A

  • Carrier with autotrophic denitrification function and preparation method thereof

    CN113044961A

  • Denitrification material based on sulfur autotrophic denitrification, preparation method and application

    CN113044974A

  • Sulfur autotrophic nitrogen removal material prepared from sulfur paste or sulfur residues as well as preparation and application methods of sulfur autotrophic nitrogen removal material

    CN114634247A

  • Sewage denitrification carrier as well as preparation method and application thereof

    CN114920351A