Degradable oil-based coring sealing fluid
By using a combination of short-chain polymer film-forming thickener, nanoparticles and solvents, an easily degradable oil-based sealed liquid was prepared, which solved the problems of high cost, poor stability and insufficient temperature resistance of the existing sealed liquid, and achieved the Efficient airtightening and environmentally friendly performance.
Patent Information
- Application Number
- CN202411090166.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-09
AI Technical Summary
In the production process of existing sealed heart fluids, there are problems such as high raw material cost, poor performance stability, and difficulty in degradation, especially oil-based sealed liquids and synthetic-based sealed liquids, and the temperature resistance of water-based sealed liquids is poor.
Using a combination of short-chain polymer film-forming thickener, nanoparticles and solvents, the preparation of specific preparation methods and proportions is made to form an easily degradable oil-based sealed liquid, enhancing its viscosity and sealing properties, and adjusting density through phosphate and stability.
It achieves good degradation performance and high temperature stability of the sealed liquid, and is suitable for deep well sealing centering, with strong environmental protection performance and sealing effect.
Smart Images

Figure SMS_1 
Figure SMS_5
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of drilling coring, and in particular relates to an easily degradable oil-based coring sealing fluid. Background Art
[0002] The closed coring technology is a coring technology commonly used in oil fields. It usually uses a closed coring device including a coring barrel to carry out coring. A closed fluid is arranged in the closed coring device. When the closed coring device reaches the target layer, the closed fluid in the coring barrel is discharged, and the coring drill bit starts working at the same time. The closed fluid is coated on the surface of the drilled core to prevent external fluids such as drilling fluid from entering the core, so that the extracted core can maintain the state in the formation to the greatest extent, so that technical personnel in the field can obtain the fluid distribution in the formation to the maximum extent.
[0003] Sealing fluid is a key technology in the process of closed coring, which is related to whether the core will be contaminated by external fluids. The sealing fluids existing in the prior art are mainly oil-based sealing fluids, synthetic-based sealing fluids and water-based sealing fluids. Among them, the oil-based sealing fluid mainly uses castor oil-based sealing fluids, which are stirred by castor oil, spinning-type perchlorethylene resin, etc., wherein the raw material cost is relatively high, and the production process will produce toxic and harmful gases such as chlorine and hydrogen chloride, and its performance stability is poor, and it is difficult to degrade; the synthetic-based sealing fluid mainly uses plasticizers as solvents, and adds corresponding resins as film-forming agents to the solvents, and adds certain plugging agents to increase the sealing effect, however, the synthetic-based sealing fluid has a high cost and is difficult to degrade; the water-based sealing fluid is mainly configured using hydroxyethyl cellulose, polyacrylamide, potassium chloride, etc., however, its temperature resistance is poor, and at the same time, it uses high-viscosity high-molecular-weight polyacrylamide, which is difficult to degrade. Summary of the invention
[0004] In order to solve at least one of the above problems, the present invention provides a degradable oil-based coring sealing fluid, which not only has good temperature resistance but also has strong environmental protection performance.
[0005] The technical scheme of the present invention is as follows: comprising a film-forming thickener, nanoparticles and a solvent in a mass ratio of 12-25:5-10:100;
[0006] The preparation method of the film-forming thickener comprises the following steps: preparing an aqueous solution of a chain transfer agent, dripping a monomer and / or its solution under continuous stirring until the monomer concentration in the reaction solution is 15-35wt%, and dripping an initiator solution at the same time, reacting for 1-4h after the dripping is completed, and separating and purifying the film-forming thickener after the reaction is completed; wherein the monomer comprises acrylic acid, glycidyl methacrylate, and 2-methacryloyloxyethyl phosphorylcholine in a mass ratio of 10:5-15:1-3, the amount of the initiator added is 1-5wt% of the total amount of the monomer, and the amount of the chain transfer agent added is 10-50wt% of the total amount of the monomer.
[0007] In this embodiment, the prepared film-forming thickener is a short-chain polymer, and its number average molecular weight is about 2000~8000 according to the monomer concentration, the amount of initiator added, the amount of chain transfer agent added, and the reaction time. Compared with long-chain polymers, it is easier to degrade; at the same time, glycidyl methacrylate and 2-methacryloyloxyethyl phosphorylcholine in the monomer will also degrade under certain conditions. According to the inventor's test, the degradation rate of the film-forming thickener can reach more than 50% under ultraviolet light for about 10~23h; and its degradation rate can also reach more than 50% after being placed in a natural environment for 8~20 days.
[0008] At the same time, the prepared film-forming thickener contains a large number of ether bonds and quaternary ammonium groups, which can be well adsorbed on the core and form a protective film to prevent external fluids from entering the core. Although the molecular weight is low, due to the different lengths of the side chains of its monomers, it is easy to form comb-like molecules, so it also has a higher viscosity. At the same time, since the polymer has a high solubility, its addition amount can be increased to increase the viscosity of the confining fluid; when the addition amount is large, the degree of viscosity decrease with temperature is low, so that it still has a strong viscosity under high temperature conditions.
[0009] Nanoparticles can be existing commercial nanoparticles, such as conventional nano-silicon dioxide, nano-calcium carbonate, nano-iron oxide, and nano-zinc oxide. In actual use, the nanoparticles used are usually hydrophobic nanoparticles, such as gas-phase nano-silicon dioxide, hydrophobically modified nanoparticles, etc., which are conventional commercial products. On the one hand, nanoparticles can form a certain degree of blockage, and at the same time, under the action of nanoparticles, the viscosity and stability of the confining fluid can be increased to a certain extent.
[0010] The solvent is a mixture of a first solvent and glycerol, wherein the first solvent is at least one of n-butanol and n-propanol, wherein the mass ratio of the first solvent to glycerol is 5 to 20:10. These solvents can dissolve the aforementioned film-forming thickener well, and the addition of n-butanol and n-propanol is, on the one hand, to dilute the viscous glycerol so as to better dissolve the film-forming agent and disperse the nanoparticles, and at the same time, it can also increase the sealing performance of the sealing fluid.
[0011] One embodiment of the present invention is that the sealing liquid also includes phosphate, and the mass ratio of the phosphate to the solvent is 1~15:100. The added phosphate can not only adjust the density of the sealing liquid, but also enhance the high temperature stability of the sealing liquid.
[0012] One embodiment of the present invention is that the chain transfer agent is isopropanol, which is a common chain transfer agent in the art.
[0013] One embodiment of the present invention is that in the preparation method of the film-forming thickener, the glycidyl methacrylate is dissolved in methanol or ethanol to form a solution; and the 2-methacryloyloxyethyl phosphorylcholine is prepared into a solution in water. Glycidyl methacrylate is insoluble in water, but soluble in most organic solvents. The reason why methanol or ethanol is used in the present invention is that it will not affect the reaction. At the same time, methanol or ethanol is miscible with water, making it easier for glycidyl methacrylate to contact and react with other materials.
[0014] One embodiment of the present invention is that the initiator is one of potassium persulfate, ammonium persulfate, and sodium persulfate, and the reaction temperature is 50-70°C. When used, the initiator is configured into a solution with water. Generally speaking, the reaction temperature is related to the type of initiator. The persulfate initiator used in this embodiment has a suitable temperature of 50-70°C; other initiators, such as oxidation-reduction initiators, can also be used, and the reaction temperature can be adjusted according to these initiators.
[0015] The present invention is beneficial in that:
[0016] The easily degradable oil-based coring sealing fluid of the present invention adopts a short-chain film-forming thickener compared to conventional sealing fluids, so it has better degradation performance and stronger environmental protection performance compared to other sealing fluids in the field; at the same time, the viscosity decreases less under high temperature conditions and can withstand higher temperatures, so it can be suitable for closed coring in deep wells. DETAILED DESCRIPTION
[0017] The present invention is further described below in conjunction with embodiments. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0018] In the following examples, unless otherwise specified, all operations used are routine operations in the art.
[0019] In the following examples, unless otherwise specified, all materials used are conventional materials in the art and mature commercial products.
[0020] In the following examples, unless otherwise specified, the parts are by mass.
[0021] Example 1: In this example, the composition of the easily degradable oil-based coring sealing fluid is as follows: 18 parts of a film-forming thickener, 8 parts of nano-silicon dioxide, and 100 parts of a solvent, wherein the 100 parts of the solvent are composed of 60 parts of n-butanol and 40 parts of glycerol; when used, the solvent is added to ultrasonically disperse the nano-silicon dioxide, and then the film-forming thickener is added and continuously stirred to make it evenly mixed.
[0022] The preparation method of the film-forming thickener is as follows: 12 parts of glycidyl methacrylate is added to ethanol to prepare a solution, 1.5 parts of 2-methacryloyloxyethyl phosphorylcholine is added to water to prepare a solution, and 0.5 parts of potassium persulfate is added to water to prepare a solution;
[0023] Take 4.3 parts of isopropanol and add it to 100 parts of water, stir to dissolve it, and add 10 parts of acrylic acid, glycidyl methacrylate solution, 2-methacryloyloxyethyl phosphorylcholine solution and potassium persulfate solution dropwise to the aqueous solution of chain transfer agent under the condition of nitrogen deoxygenation and 65°C. After the addition is completed, keep warm for 2 hours. After the insulation is completed, remove low boiling points by reduced pressure distillation to obtain the product.
[0024] The film-forming thickener of this embodiment has a degradation rate of 50% under different conditions: about 17 hours under ultraviolet conditions and about 15 days under natural conditions, which shows that it has good self-degradation performance. Therefore, it is shown that the sealing fluid of this embodiment has good degradation performance.
[0025] Example 2: In this example, the composition of the easily degradable oil-based coring sealing fluid is as follows: 22 parts of a film-forming thickener, 9 parts of nano zinc oxide, and 100 parts of a solvent, wherein the 100 parts of the solvent are composed of 40 parts of n-butanol and 60 parts of glycerol; when used, the solvent is added to ultrasonically disperse the nano zinc oxide, and then the film-forming thickener is added and continuously stirred to make it evenly mixed.
[0026] The preparation method of the film-forming thickener is as follows: 8 parts of glycidyl methacrylate are added to ethanol to prepare a solution, 2.5 parts of 2-methacryloyloxyethyl phosphorylcholine are added to water to prepare a solution, and 0.25 parts of potassium persulfate are added to water to prepare a solution;
[0027] Take 2.8 parts of isopropanol and add it to water, stir to dissolve it, add 10 parts of acrylic acid, glycidyl methacrylate solution, 2-methacryloyloxyethyl phosphorylcholine solution and potassium persulfate solution dropwise to the aqueous solution of chain transfer agent under the condition of nitrogen deoxygenation and 65°C, keep warm for 2 hours after the addition is completed, and after the insulation is completed, remove low boiling points by reduced pressure distillation to obtain the product.
[0028] The film-forming thickener of this embodiment has a degradation rate of 50% under different conditions in about 30 hours under ultraviolet conditions and about 18 days under natural conditions, which indicates that it has good self-degradation performance. Therefore, it is shown that the sealing fluid of this embodiment has good degradation performance.
[0029] Example 3: This comparative example differs from Example 1 in that 12 g of potassium phosphate is further added, and the rest are the same.
[0030] Example 4: The difference between this comparative example and Example 1 is that, during the preparation of the film-forming thickener, the amount of isopropyl alcohol added is 12 parts, the amount of glycidyl methacrylate added is 17 parts, the amount of 2-methacryloyloxyethyl phosphorylcholine added is 2.5 parts, the amount of acrylic acid added is 12 parts, and the rest are the same.
[0031] The film-forming thickener of this embodiment has a degradation rate of 50% under different conditions in about 16 hours under ultraviolet conditions and about 9 days under natural conditions, which indicates that it has good self-degradation performance. Therefore, it is shown that the sealing fluid of this embodiment has good degradation performance.
[0032] Example 5: The difference between this example and Example 1 is that the sealing liquid includes: 14 parts of film-forming thickener, 5.5 parts of nano-silicon dioxide, and 100 parts of solvent, wherein the 100 parts of solvent are composed of 60 parts of n-butanol and 40 parts of glycerol, and the rest are the same.
[0033] Example 6: The difference between this example and Example 1 is that the sealing liquid includes: 24 parts of film-forming thickener, 9.5 parts of nano-silicon dioxide, and 100 parts of solvent, wherein the 100 parts of solvent are composed of 50 parts of n-propanol and 50 parts of glycerol, and the rest are the same.
[0034] Comparative Example 1
[0035] The difference between this comparative example and Example 1 is that the comparative example does not contain nanoparticles, and the rest is the same.
[0036] Comparative Example 2
[0037] The difference between this comparative example and Example 1 is that 2-methacryloyloxyethyl phosphorylcholine is not contained in the preparation process of the film-forming thickener, and the rest are the same.
[0038] Comparative Example 3
[0039] The difference between this comparative example and Example 1 is that glycidyl methacrylate is not contained in the preparation process of the film-forming thickener, and the rest are the same.
[0040] In order to further highlight the technical effects of the present invention, performance tests are performed on the above embodiments below.
[0041] 1. Salt spray resistance test
[0042] The sealing liquids of Examples 1 to 6 and Comparative Examples 1 to 3 were taken, and their viscosities were measured at room temperature. They were then aged at 120° C. for 24 h. After the aging, their viscosities were measured. The final results are shown in Table 1.
[0043] Table 1 Salt spray resistance test results
[0044]
[0045] It can be seen from Table 1 that the sealing fluid prepared in the embodiment of the present invention has strong temperature resistance and can meet the actual coring requirements.
[0046] 2. Sealing performance test
[0047] Take the sealing liquid of Examples 1 to 6 and Comparative Examples 1 to 3, then take the core and soak it in the sealing liquid for 10 minutes; prepare a 1% ammonium nitrate tracer aqueous solution, take out the soaked core and place it in the tracer aqueous solution for 16 hours. After the end, measure the intrusion amount of the tracer aqueous solution, and use the core not soaked in the sealing liquid as a blank. The final sealing performance is shown in Table 2.
[0048] The calculation formula of the sealing rate is as follows: , where is the sealing rate, represents the equivalent intrusion volume of the core not soaked in confined fluid, b It indicates the equivalent intrusion volume of the core immersed in the confined fluid. At the same time, the equivalent intrusion volume is obtained by the following method: take the core after the test, cut a piece along its axis in a fixed area and crush it, add 10ml of water and continue to stir to extract for 10min, and then use a UV spectrophotometer to measure its concentration.
[0049] Table 2 Sealing test results
[0050]
[0051] It can be seen from Table 2 that the sealing fluid prepared in the embodiment of the present invention has a strong sealing effect and can be applied to the closed coring operation in the oil field.
[0052] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.
Claims
1. A degradable oil-based coring sealing fluid, characterized in that: It includes a film-forming thickener, nanoparticles and a solvent in a mass ratio of 12 to 25:5 to 10:100; The preparation method of the film-forming thickener comprises the following steps: preparing an aqueous solution of a chain transfer agent, dripping a monomer and / or its solution under continuous stirring until the monomer concentration in the reaction solution is 15-35wt%, and dripping an initiator solution at the same time, reacting for 1-4h after the dripping is completed, and separating and purifying the film-forming thickener after the reaction is completed; wherein the monomer comprises acrylic acid, glycidyl methacrylate, and 2-methacryloyloxyethyl phosphorylcholine in a mass ratio of 10:5-15:1-3, the amount of the initiator added is 1-5wt% of the total amount of the monomer, and the amount of the chain transfer agent added is 10-50wt% of the total amount of the monomer; The solvent is a mixture of a first solvent and glycerol, the first solvent is at least one of n-butanol and n-propanol, wherein the mass ratio of the first solvent to glycerol is 5-20:10; The nanoparticles are one of nano silicon dioxide, nano calcium carbonate, nano iron oxide and nano zinc oxide.
2. The easily degradable oil-based coring sealing fluid according to claim 1, characterized in that: The sealing liquid also includes phosphate, and the mass ratio of the phosphate to the solvent is 1-15:
100.
3. The easily degradable oil-based coring sealing fluid according to claim 1, characterized in that: The chain transfer agent is isopropyl alcohol.
4. The easily degradable oil-based coring sealing fluid according to claim 1, characterized in that: In the preparation method of the film-forming thickener, the glycidyl methacrylate is dissolved in methanol or ethanol to form a solution; and the 2-methacryloyloxyethyl phosphorylcholine is dissolved in water to form a solution.
5. The easily degradable oil-based coring sealing fluid according to claim 1, characterized in that: The initiator is one of potassium persulfate, ammonium persulfate and sodium persulfate, the reaction temperature is 50-70° C. When used, the initiator is configured into a solution with water.