A method for recycling high-temperature alloy powder containing rhenium
Through vacuum hot press sintering and electron beam smelting technology, combined with surface processing, the problem of high oxygen content in high-temperature alloy waste powder is solved, and the efficient recycling of rhenium elements and the production of high-purity high-temperature alloy powders are achieved, which meets the aerospace and other fields. High purity requirements reduce the cost of material use and improve material utilization.
Patent Information
- Application Number
- CN202411068377.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-06
AI Technical Summary
The prior art is difficult to effectively recover and reuse high-temperature alloy waste powder, especially rhenium-containing high-temperature alloy powder, which leads to high oxygen content and is difficult to meet the high purity requirements in the fields of aerospace and other fields.
Using powder vacuum hot press sintering and electron beam horizontal furnace smelting technology, combined with surface processing and component analysis, through vacuum environment and fine heat treatment and smelting processes, the content of harmful gases such as oxygen, nitrogen and sulfur in the alloy is reduced, and the content of impurities such as impurities is improved. Recovery of rhenium and density of the material.
It realizes efficient recycling of rhenium and high-purity high-temperature alloy powder production. The content of harmful gases and impurities such as O, N, S is extremely low, and the inclusion content is extremely low, which meets the high purity requirements in aerospace and other fields, reducing the material The cost of use and improves material utilization.
Smart Images

Figure CN118600257B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of vacuum metallurgy, and in particular to a method for recycling and reusing rhenium-containing high-temperature alloy powder. Background Art
[0002] Nickel-based high-temperature alloys are widely used in hot-end components in the aerospace and energy fields due to their excellent high-temperature strength, good corrosion resistance and thermal fatigue resistance. The manufacturing technology of nickel-based high-temperature alloys is mainly casting, forging and powder metallurgy, followed by cutting. The whole process has a long cycle and complex procedures, and it is impossible to form complex-shaped parts in one piece. Since additive manufacturing (AM) technology is not limited by processing technology, it can form parts with complex shapes as a whole, and is not affected by the cumbersome processes and low material utilization of traditional manufacturing technology. Therefore, the research and application of nickel-based high-temperature alloy parts prepared by additive manufacturing technology are becoming more and more common. The most basic raw material in the field of high-temperature alloy additive manufacturing is nickel-based high-temperature alloy powder.
[0003] The main processes for preparing high-temperature alloy powders are vacuum induction melting gas atomization (VIGA), electrode induction melting gas atomization (EIGA) and plasma rotating electrode method (PREP). The diameter of the powder used in conventional 3D printing is 15um~53um. Therefore, it is inevitable to produce fine powder of 0~15um and coarse powder larger than 53um, which cannot be used directly and can only be used as waste powder. The proportion of waste powder produced accounts for about 30%~50% of the powder. With the rapid development of the additive manufacturing industry, the demand for high-temperature alloy powders has increased year by year, and the corresponding stock of high-temperature alloy waste powders has also increased year by year. These high-temperature alloy powders contain a large amount of rare and precious elements, such as Re, W, Mo, Ta, Nb, Hf and other elements. How to reuse these high-temperature alloy waste powders is an urgent issue currently faced.
[0004] Since the size of high-temperature alloy powder is small, its specific surface area is increased, which makes it easier to add oxygen, resulting in a greatly increased oxygen content in the powder compared to the parent alloy. Liu Na et al. (Rare Metals, Vol. 35, No. 4, 481-485) studied the oxidation characteristics of argon-atomized nickel-based high-temperature alloy powders, indicating that oxygen mainly produces oxides with elements such as Ti and Cr enriched on the surface. Regardless of whether it is stored under argon or vacuum conditions, the oxygen content will increase with time. The storage conditions of high-temperature alloy waste powder are worse, which makes the O content in the waste powder higher.
[0005] At present, there have been studies on the recycling of waste high-temperature alloy powders. For example, the patent application publication number CN113458402A proposed a method for preparing high-temperature alloy powders using nickel-based high-temperature alloy powder return materials, but the O content of the alloy powders prepared by the patent application publication number CN115852184A proposed a method for preparing master alloys by remelting high-temperature alloy powders. Although the powders were wrapped with aluminum foil, the melting point of aluminum was low, and there was a risk of equipment damage caused by powder inhalation into the vacuum system, and it was difficult to effectively remove the O in the powders. The patent application publication number CN114749673A proposed printing blocks with coarse powders, and then using them as raw materials for powder making. Because the oxygen content in the coarse powders was high, there was a risk of continued oxygenation after printing. Therefore, how to achieve better reuse of waste high-temperature alloy powders still needs to be studied.
[0006] At the same time, some powder high-temperature alloys used for repairing single-crystal blades of aircraft engines contain rhenium, which is a rare and precious metal element with extremely low content in the earth's crust. With the continuous development of aerospace, national defense and other fields, the demand for rhenium has increased year by year. Since rhenium-containing high-temperature alloys have high requirements for O, N elements and inclusions, if the above-mentioned patented method is used to reuse the rhenium-containing high-temperature alloy powder, the oxygen content will be high and cannot meet the existing requirements. Summary of the invention
[0007] Purpose of the invention: In view of the shortcomings in the prior art, the present application provides a method for recycling and reusing rhenium-containing high-temperature alloy powder. The method can realize the recycling and utilization of rhenium elements. At the same time, the alloy produced by this method has extremely low levels of harmful gases and impurity elements such as O, N, S, and the inclusion content in the alloy is extremely low.
[0008] Technical solution: The method provided in this application comprises the following steps:
[0009] Step (1) Powder vacuum hot pressing sintering:
[0010] First, put the waste powder of high-temperature alloy containing rhenium into the graphite mold and evacuate it to 1×10 -3 Pa, then heat to sintering temperature, apply axial pressure of 40MPa~60MPa at this sintering temperature, keep warm for 100min~120min, then cool to below 500℃ and take out electrode ingot. Graphite mold is selected because it has good high temperature resistance and low chemical activity, suitable for use in high temperature sintering process, and will not react with rhenium-containing high temperature alloy, ensuring the purity of the material. The operation in vacuum is to remove gas, prevent the alloy from reacting adversely with oxygen and other gases during sintering process to form impurities such as oxides, reduce pores, and improve the density and performance of the material. The present invention selects 1×10 -3 Below Pa ensures the purity of the sintering environment.
[0011] Step (2) Electron beam horizontal furnace melting:
[0012] Place the electrode ingot into the crucible of the horizontal furnace and close the furnace door after ensuring that the furnace is clean. Evacuate the electron beam melting furnace and electron gun. The vacuum degree of the melting chamber is required to be less than 1×10 -2 Pa, the vacuum degree of the gun body is required to be less than 1×10 -3 Pa, then start the electron gun for preheating, the preheating time is 20min~40min; use the electron gun to melt the return material in a circular scanning manner, the melting power is 240kW~280kW; after the charge is completely melted, adjust the power value to 200kW~260kW, and refine the alloy melt in a square scanning manner, the duration is 20min~30min. The circular scanning method uses the electron beam to make a circular motion on the surface of the molten material, quickly and evenly transfer energy, and achieve efficient melting. High power ensures rapid heating and avoids uneven changes in material composition. Switching to square scanning and reducing power is a refining process after melting is completed. In this way, the molten pool can be stirred more finely, the inclusions can be floated and removed, and the alloy composition can be further homogenized to improve the microstructure and performance of the material; after refining, the filament power is slowly reduced until it is zero; the alloy ingot is taken out after cooling in the furnace for a period of time.
[0013] Step (3) Surface processing and composition analysis:
[0014] The alloy ingots smelted in the horizontal furnace were sheared into 10mm×20mm plate samples by a shearing machine, the oxide layer on the surface of the alloy was removed by a shot blasting machine, and the chemical composition of the alloy was analyzed by sampling.
[0015] Step (4) Vacuum induction melting:
[0016] The alloy plate treated in step (3) is used as raw material to produce the same grade of high-temperature alloy according to the normal production process.
[0017] Specifically, in step (1), a 500-ton vacuum hot press furnace is used to sinter and press the rhenium-containing high-temperature alloy waste powder into electrode ingots.
[0018] Specifically, in step (1), the preferred conditions for hot pressing sintering are: applying an axial pressure of 50 MPa and holding time of 110 min.
[0019] Specifically, in step (1), the powder is heated to 1180°C~1220°C at 20°C~40°C per minute. In the present invention, the heating rate needs to be precisely controlled. Too fast may lead to a large temperature difference between the inside and outside, causing stress concentration and deformation; too slow will extend the process cycle and reduce efficiency. Therefore, the most suitable heating rate in the present invention is 20°C to 40°C per minute. The selection of sintering temperature depends on the specific composition of the alloy and the required microstructure. It is usually much higher than the melting point of the alloy, but not enough to completely melt the material, but to achieve bonding between particles through atomic diffusion. The preferred sintering temperature of the present invention is 1200°C, and the preferred heating rate of the present invention is 30°C / min.
[0020] Specifically, in step (2), the preheating time is preferably 30 minutes.
[0021] Specifically, in step (2), the preferred process is: using an electron gun to melt the return material in a circular scanning manner, with a melting power of 260 W; after the charge is completely melted, adjusting the power value to 230 kW, and refining the alloy melt in a square scanning manner, with a duration of 25 minutes.
[0022] Specifically, in step (2), the alloy ingot is removed from the furnace after cooling for 2 hours. Slowly reducing the filament power avoids local overheating or sudden changes in alloy properties that may be caused by sudden interruption of the electron beam. Cooling in the furnace gradually cools the alloy ingot, which helps reduce internal stress, prevent cracking, and ensure the stability of the alloy structure.
[0023] Specifically, in step (3), the shot blasting time of the sheared alloy plate is 2 hours. The shot blasting time is set to 2 hours. This time length is based on the hardness of the alloy, the thickness of the oxide layer, and the desired surface cleanliness. Long-term shot blasting can more thoroughly remove the oxide layer, but it may also increase the risk of surface damage.
[0024] Furthermore, in step (4), the composition of the alloy block after electron beam melting and surface treatment may be different from the target alloy composition, and new pure metal raw materials need to be added before alloy production melting.
[0025] Beneficial effects: Compared with the prior art:
[0026] 1. The present invention can greatly reduce the content of harmful gases and impurity elements such as O, N, S, etc. in Re-containing high-temperature alloy powder by adopting electron beam melting, wherein the O and N elements can be controlled within 5ppm, and the S element can be controlled within 1ppm.
[0027] 2. The rhenium element recovery rate of the method of the present invention is greater than 99.0%, realizing the recovery and reuse of the rare and precious metal rhenium element.
[0028] 3. The rhenium-containing high-temperature alloy produced by the method of the present invention has extremely low inclusion content and fully meets the subsequent application of the alloy.
[0029] 4. The method of the present invention can realize the recycling and reuse of high-temperature alloy powder, solving the problem that high-temperature alloy powder is difficult to reuse due to high content of harmful gas elements such as O and N. At the same time, it reduces the use cost of high-temperature alloy and improves material utilization. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is a metallographic photograph (×100) of inclusions in a rhenium-containing high-temperature alloy produced by the method of Example 1;
[0031] Figure 2 This is a metallographic photograph (×100) of inclusions in a rhenium-containing high-temperature alloy produced by the method of Comparative Example 1;
[0032] Figure 3 is a photograph of the slag of the rhenium-containing high-temperature alloy produced by the method of Example 1 (HB5406 method);
[0033] Figure 4 This is a photo of the slag of the rhenium-containing high-temperature alloy produced by the method of Example 1 (HB5406 method). DETAILED DESCRIPTION
[0034] The technical solution of the present application is described in detail below through embodiments, but the protection scope of the present application is not limited to the embodiments. Example 1
[0035] This example is DD5 second generation single crystal high temperature alloy powder, and the chemical composition results are shown in Table 1:
[0036] Table 1 Chemical composition of DD5 superalloy powder (wt%)
[0037]
[0038] 1. Powder vacuum hot pressing sintering:
[0039] The DD5 alloy waste powder was pressed into electrode ingots using a 500-ton vacuum hot press furnace. The sintering process parameters are as follows: first, the DD5 alloy waste powder was placed in a graphite mold and vacuumed to 1×10 -3 Pa, and then the powder is heated to sintering temperature at 30°C per minute, and the sintering temperature is 1200°C. At this sintering temperature, an axial pressure of 50MPa is applied and the heat preservation time is 110min. After that, it is cooled to below 500°C and the electrode ingot is taken out.
[0040] 2. Electron beam horizontal furnace melting:
[0041] Electrode ingots are melted in an electron beam furnace, and the melting process parameters are:
[0042] a. Place the electrode ingot into the crucible of the horizontal furnace and close the furnace door after making sure the furnace is clean.
[0043] b. Evacuate the electron beam melting furnace and electron gun. The vacuum degree of the melting chamber is required to be less than 1×10 -2 Pa, the vacuum degree of the gun body is required to be less than 1×10 -3 Pa, and then start the electron gun for preheating, the preheating time is 30 minutes.
[0044] c. Use an electron gun to melt the return material in a circular scanning manner with a melting power of 260kW. After the charge is completely melted, adjust the power value to 230kW and refine the alloy melt in a square scanning manner for 25 minutes.
[0045] d. After refining, slowly reduce the filament power until it reaches zero; the alloy ingot is cooled in the furnace for 2 hours and then removed. 3. Surface processing and composition analysis:
[0046] The alloy ingot melted in the horizontal furnace was sheared into a 10mm×20mm plate sample by a shearing machine, and the oxide layer on the surface of the alloy was removed by a shot blasting machine for 2 hours, and then the chemical composition of the alloy was analyzed. The chemical composition results are shown in Table 2. It can be seen that after electron beam melting, the Cr and Al elements in the alloy were lost, the other alloy elements were slightly increased, and the harmful gases and impurity elements such as O, N, and S were greatly reduced.
[0047] Table 2 Composition results of DD5 alloy after electron beam melting (wt%)
[0048]
[0049] 4. Vacuum induction melting:
[0050] The treated DD5 alloy plate is used as raw material, Cr and Al elements are appropriately added during the batching, and the DD5 high temperature alloy is produced according to the normal alloy production process. The chemical composition results of the produced DD5 master alloy ingot are shown in Table 3, and it can be seen that the O and N elements in the alloy are less than 5ppm, and the S element is less than 1ppm.
[0051] Table 3 Composition results of DD5 alloy by vacuum induction melting (wt%)
[0052]
[0053] 5. Rhenium recovery rate
[0054] DD5 high-temperature alloy powder was sintered by vacuum hot pressing to produce an electrode ingot of 20 kg. After electron beam horizontal furnace melting, 19.4 kg of alloy was obtained. The recovery rate of rhenium element during electron beam melting was (19.4 kg × 3.12%) / (20 kg × 3.04%) × 100% = 99.55%, which is greater than 99.5%. There is basically no loss of rhenium element during vacuum induction melting, so the actual recovery rate of rhenium element exceeds 99.5%. Example 2
[0055] The steps of this embodiment are roughly the same as those of embodiment 1, except that:
[0056] Step (1): Place the DD5 alloy waste powder into a graphite mold and evacuate to 1×10 -3 Pa, then the powder is heated to sintering temperature at 20℃ per minute, and the sintering temperature is 1180℃. At this sintering temperature, an axial pressure of 40MPa is applied and the heat preservation time is 120min. After that, it is cooled to below 500℃ and the electrode ingot is taken out.
[0057] The recovery rate of rhenium element is greater than 99.0%. Example 3
[0058] The steps of this embodiment are roughly the same as those of embodiment 1, except that:
[0059] Step (2): Use an electron gun to melt the return material in a circular scanning manner with a melting power of 280 kW; after the charge is completely melted, adjust the power value to 260 kW and refine the alloy melt in a square scanning manner for 20 minutes.
[0060] The recovery rate of rhenium element is greater than 99.0%.
[0061] Through Examples 1 to 3, it can be seen that for the recycling of DD5 second-generation single crystal high-temperature alloy, the process conditions of Example 1 are better. Example 4
[0062] This example is Rene142 second generation directionally solidified high temperature alloy powder, and the chemical composition results are shown in Table 4:
[0063] Table 4 Chemical composition of Rene142 high temperature alloy powder (wt%)
[0064]
[0065] 1. Powder vacuum hot pressing sintering:
[0066] A 500-ton vacuum hot press furnace is used to press the waste powder of rhenium-containing high-temperature alloy into electrode ingots. The sintering process parameters are as follows: first, the waste powder of Rene142 alloy is placed in a graphite mold and vacuumed to 1×10 -3 Pa, and then the powder is heated to sintering temperature at 30°C per minute, and the sintering temperature is 1200°C. At this sintering temperature, an axial pressure of 50MPa is applied and the heat preservation time is 110min. After that, it is cooled to below 500°C and the electrode ingot is taken out.
[0067] 2. Electron beam horizontal furnace melting:
[0068] Electrode ingots are melted in an electron beam furnace, and the melting process parameters are:
[0069] a. Place the electrode ingot into the crucible of the horizontal furnace and close the furnace door after making sure the furnace is clean.
[0070] b. Evacuate the electron beam melting furnace and electron gun. The vacuum degree of the melting chamber is required to be less than 1×10 -2 Pa, the vacuum degree of the gun body is required to be less than 1×10 -3 Pa, and then start the electron gun for preheating, the preheating time is 30 minutes.
[0071] c. Use an electron gun to melt the return material in a circular scanning manner with a melting power of 260kW. After the charge is completely melted, adjust the power value to 230kW and refine the alloy melt in a square scanning manner for 25 minutes.
[0072] d. After refining, slowly reduce the filament power until it reaches zero; the alloy ingot is cooled in the furnace for 2 hours and then removed. 3. Surface processing and composition analysis:
[0073] The alloy ingot melted in the horizontal furnace was sheared into a 10mm×20mm plate sample by a shearing machine, and the oxide layer on the surface of the alloy was removed by a shot blasting machine for 2 hours, and then the chemical composition of the alloy was analyzed. The chemical composition results are shown in Table 5. It can be seen that after electron beam melting, the Cr and Al elements in the alloy were lost, the other alloy elements were slightly increased, and the harmful gases and impurity elements such as O, N, and S were greatly reduced.
[0074] Table 5 Composition results of Rene142 alloy after electron beam melting (wt%)
[0075]
[0076] 4. Vacuum induction melting:
[0077] The treated Rene142 alloy plate is used as raw material, Cr and Al elements are appropriately added during the batching, and the Rene142 high temperature alloy is produced according to the normal alloy production process. The chemical composition results of the produced Rene142 master alloy ingot are shown in Table 6, and it can be seen that the O and N elements in the alloy are less than 5ppm, and the S element is less than 1ppm.
[0078] Table 6 Composition results of Rene142 alloy by vacuum induction melting (wt%)
[0079]
[0080] 5. Rhenium recovery rate
[0081] Rene142 high temperature alloy powder was sintered by vacuum hot pressing to produce 20 kg of electrode ingots. After electron beam horizontal furnace melting, 19.5 kg of alloy was obtained. The recovery rate of rhenium element during electron beam melting was (19.5 kg × 2.88%) / (20 kg × 2.82%) × 100% = 99.57%, which is greater than 99.5%. There is basically no loss of rhenium element during vacuum induction melting, so the actual recovery rate of rhenium element exceeds 99.5%. Example 5
[0082] The steps of this embodiment are roughly the same as those of embodiment 4, except that:
[0083] Step (1): Place the Rene142 alloy waste powder into a graphite mold and evacuate to 1×10 -3 Pa, and then the powder is heated to sintering temperature at 40℃ per minute, and the sintering temperature is 1220℃. At this sintering temperature, an axial pressure of 40MPa~60MPa is applied, and the heat preservation time is 100min. After that, it is cooled to below 500℃ and the electrode ingot is taken out.
[0084] The recovery rate of rhenium element is greater than 99.0%. Example 6
[0085] The steps of this embodiment are roughly the same as those of embodiment 4, except that:
[0086] Step (2) uses an electron gun to melt the return material in a circular scanning manner with a melting power of 240 kW; after the charge is completely melted, adjust the power value to 200 kW and refine the alloy melt in a square scanning manner for 30 minutes.
[0087] The recovery rate of rhenium element is greater than 99.0%.
[0088] Through Examples 4 to 6, it can be seen that for the recycling of Rene142 second-generation directional solidification high-temperature alloy, the process conditions of Example 4 are better. Comparative Example 1
[0089] The DD5 alloy powder of Example 1 was directly cold pressed into an ingot, and then used as a raw material to remelt into a DD5 master alloy ingot in a vacuum induction furnace. The chemical composition results are shown in Table 7. The results show that the contents of O, N, and S are all relatively high.
[0090] Table 7 Chemical composition results of alloy of comparative example 1 (wt%)
[0091]
[0092] The results of Example 1 and Comparative Example 1 are compared and analyzed. As shown in Tables 1, 2, 3 and 7, the O and N elements of the DD5 alloy produced in Example 1 are less than 5 ppm, and the S element is less than 1 ppm, while the O, N and S elements of the DD5 alloy produced in Comparative Example 1 are reduced but still relatively high.
[0093] Example 1 and Comparative Example 1 both use metallographic examination and slag testing to examine the inclusion level in the alloy. Figure 1~Figure 4 It can be seen that the DD5 alloy produced in Example 1 has basically no inclusions in the metallographic examination. According to the HB5406 method, the scum detection is carried out, and the alloy liquid surface is clean, without scum, and the scum area is less than 0.5%; while the DD5 alloy produced in Comparative Example 1 has inclusions in the inspection. According to the HB5406 method, the scum detection is carried out, and a small amount of scum is present on the alloy liquid surface, and the scum area is about 2%. Therefore, it can be seen that the rhenium-containing high-temperature alloy produced by the patent method has extremely low inclusion content and high purity.
[0094] The parts not described in detail in the present invention are all known technologies to those skilled in the art. The above description is only a preferred embodiment of the present application and is not intended to limit the present application.
Claims
1. A method for recycling rhenium-containing high-temperature alloy powder, characterized in that: The steps include: Step (1) Powder vacuum hot pressing sintering: First, put the waste powder of high-temperature alloy containing rhenium into the graphite mold and evacuate it to 1×10 -3 Pa, then heated to sintering temperature, applied axial pressure of 50MPa at this sintering temperature, kept warm for 100min, then cooled to below 500℃ and took out electrode ingots; used 500-ton vacuum hot press furnace to sinter and press rhenium-containing high-temperature alloy waste powder into electrode ingots; Step (2) Electron beam horizontal furnace melting: Place the electrode ingot into the crucible of the horizontal furnace and close the furnace door after ensuring that the furnace is clean. Evacuate the electron beam melting furnace and electron gun. The vacuum degree of the melting chamber is required to be less than 1×10 -2 Pa, the vacuum degree of the gun body is required to be less than 1×10 -3 Pa, and then start the electron gun for preheating, the preheating time is 30 minutes; use the electron gun to melt the return material in a circular scanning manner, the melting power is 260W; after the charge is completely melted, adjust the power value to 230kW, and refine the alloy melt in a square scanning manner, the duration is 25 minutes; after the refining is completed, slowly reduce the filament power until it is zero; the alloy ingot is taken out after cooling in the furnace for 2 hours; Step (3) Surface processing and composition analysis: The alloy ingot melted in the horizontal furnace was sheared into 10mm×20mm plate samples by a shearing machine, and the oxide layer on the surface of the alloy was removed by a shot blasting machine, and the chemical composition of the alloy was analyzed by sampling; Step (4) Vacuum induction melting: The alloy plate treated in step (3) is used as raw material to produce the same grade of high-temperature alloy according to the normal production process.
2. The method for recycling and reusing rhenium-containing high-temperature alloy powder according to claim 1, characterized in that: In step (1), the powder is heated to 1180°C~1220°C at a rate of 20°C~40°C per minute.
3. The method for recycling and reusing rhenium-containing high-temperature alloy powder according to claim 1, characterized in that: In step (1), the powder is heated at 30°C per minute to 1200°C.
4. The method for recycling and reusing rhenium-containing high-temperature alloy powder according to claim 1, characterized in that: In step (3), the shot blasting time of the sheared alloy plate is 2 hours.
5. The method for recycling and reusing rhenium-containing high-temperature alloy powder according to claim 1, characterized in that: In step (4), the composition of the alloy block after electron beam melting and surface treatment will be different from the target alloy composition, and new pure metal raw materials need to be added before alloy production melting.
Citation Information
Patent Citations
Method for preparing high-temperature alloy powder by using nickel-based high-temperature alloy powder return scrap
CN113458402A
Purification recovery method of DD5 single crystal casting high-temperature alloy return scrap
CN117701899A
Preparation method of rhenium plate
CN117758093A