A degradable sealing film and preparation method thereof
By using a biodegradable coating with polylactic acid, tapioca starch and ethylene-acrylic acid copolymer in paper sealing film, and by combining modified bamboo fibers and montmorillonite, a network interlocking structure was solved The problem of insufficient structural strength of paper sealing film has significantly improved its anti-microcrack propagation ability and overall strength.
Patent Information
- Application Number
- CN202411088301.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-09
AI Technical Summary
Traditional paper sealing films have shortcomings in structural strength, especially when the biodegradable coating is subject to external forces, resulting in insufficient overall strength.
Polylactic acid, tapioca starch and ethylene-acrylic acid copolymer are used to form a biodegradable coating, and the composite of modified bamboo fibers and montmorillonite forms a mesh interlocking structure to enhance the anti-microcrack expansion ability of the coating .
It significantly improves the overall structural strength and anti-microcrack propagation ability of the degradable sealing membrane, improves its tear strength, and enhances environmental protection performance.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of degradable packaging, and more specifically, to a degradable sealing film and a preparation method thereof. Background Art
[0002] Sealing film is a composite material used to seal the mouths of various containers to achieve the effects of preservation, dust prevention, moisture prevention, etc. It is mostly used in the packaging of food, cosmetics, pharmaceuticals and other industries. The common sealing packaging form in daily life is often used for fast food box sealing, cooked food sealing, jelly sealing, milk tea sealing, as well as packaging herbal tea, soy milk, juice, beverages or coffee desserts.
[0003] The sealing films on the market are divided into three categories according to their materials: conventional transparent plastic sealing films, frosted sealing films, and paper sealing films. With the improvement of environmental awareness and the increase of personalized needs, paper sealing films are becoming more and more popular. Paper sealing films are obtained by coating or covering the surface of paper with plastic film. As paper sealing films are constantly innovating and developing, the paper materials of paper sealing films come from plant fibers, such as trees and bamboo, which are renewable in nature and have a fast degradation rate; the coating part of paper sealing films also uses biodegradable materials such as starch and polylactic acid, which can not only bring waterproof and oil-proof effects, but also have excellent degradable properties; therefore, paper sealing films have more environmental advantages and economic benefits, can be quickly degraded in the natural environment, and will not cause long-term pollution to the environment.
[0004] Regarding the above-mentioned related technologies, the inventors believe that although paper sealing films have advantages in degradability, traditional plastic sealing films have higher structural strength. Paper sealing films are more susceptible to damage due to the limitations of paper materials and biodegradable coatings of the paper sealing films, especially the biodegradable coatings, which are prone to microcrack expansion when subjected to large external forces. Therefore, the overall structural strength of paper sealing films still needs to be improved. Summary of the invention
[0005] In order to improve the ability of the biodegradable coating to resist microcrack propagation and significantly enhance the overall structural strength of the paper sealing film, the present application provides a degradable sealing film and a preparation method thereof.
[0006] In a first aspect, the present application provides a degradable sealing film, which adopts the following technical solution:
[0007] A degradable sealing film comprises a paper substrate and a biodegradable coating disposed on the paper substrate, wherein the biodegradable coating is made of raw materials comprising the following parts by weight:
[0008] Polylactic acid 40-50 parts;
[0009] 10-20 parts of tapioca starch;
[0010] 15-25 parts of ethylene-acrylic acid copolymer;
[0011] 3-5 parts of dispersant;
[0012] 2-3 parts of cross-linking agent;
[0013] Thickener 1-3 parts;
[0014] Montmorillonite 1.5-2.5 parts;
[0015] 2-6 parts of modified bamboo fiber;
[0016] The modified bamboo fiber is prepared by the following modification steps:
[0017] S1, taking bamboo fiber raw material and soaking it in a sodium hydroxide solution with a concentration of 6-10%, washing and drying it to obtain pretreated bamboo fiber;
[0018] S2, mixing a silane coupling agent and dopamine as a modifier and placing them in deionized water to prepare a modified solution with a concentration of 3-5%, then immersing the pretreated bamboo fiber in the modified solution for treatment, taking it out and drying it to obtain the modified bamboo fiber;
[0019] The weight ratio of the silane coupling agent to dopamine is 1:(2-3).
[0020] By adopting the above technical scheme, polylactic acid is made from starch-containing agricultural products such as corn, wheat, and beets, which is fermented to generate lactic acid and then made by condensation polymerization and melt spinning. After decomposition, the high molecular weight polymer chain breaks and decomposes, and the final degradation products are carbon dioxide and water, which do not pollute the environment; cassava starch is a powder obtained by dehydration and drying after starch extraction, and has excellent renewability and degradability; ethylene-acrylic acid copolymer is produced by the reaction of ethylene and acrylic acid, and is a polymer with thermoplasticity and extremely high adhesion; polylactic acid, cassava starch and ethylene-acrylic acid copolymer are combined to form the main mixed matrix of the biodegradable coating, which can show excellent compatibility and form a close and stable combination with other raw materials, and can also show better degradability, which is conducive to obtaining a degradable sealing film with excellent quality and stability.
[0021] Bamboo fiber is a fiber extracted from bamboo. It can be decomposed and degraded by microorganisms in the natural environment, and the degradation speed is fast, with excellent environmental performance. The bamboo fiber is modified by first treating it with sodium hydroxide to make the surface of the bamboo fiber rough, and then treating it with a mixture of silane coupling agent and dopamine as a modifier, which not only makes the bamboo fiber softer and fluffier, but also forms a special surface modification, acting as a stable bridge and bond between the polymer mixed matrix and the bamboo fiber. At the same time, the modified bamboo fiber can also build a mesh interlocking structure in the biodegradable coating after use, which has a significant effect on improving the structural strength and resistance to microcrack expansion of the biodegradable coating. Montmorillonite is dispersed in the biodegradable coating, and uses its own lamellar structure with a large specific surface area to have a strong interaction with the polymer mixed matrix, and can effectively prevent the cracks from continuing to expand. In the biodegradable coating of the present application, when the modified bamboo fiber and montmorillonite are used in combination, they can also exert an excellent combination effect with each other, and can form an intercalated network structure with montmorillonite as the structural point. In addition, by utilizing the unique hollow thin-walled multi-tube structure of the modified bamboo fiber and the special layered structure of montmorillonite, not only can a stable and tight combination with polylactic acid, cassava starch and ethylene-acrylic acid copolymer be formed, but also a significant effect can be shown in improving the biodegradable coating's resistance to microcrack propagation, thereby significantly improving the overall structural strength of the final degradable sealing film.
[0022] Preferably, the weight ratio of the silane coupling agent to dopamine is 1:2.5.
[0023] By adopting the above technical scheme, when the modifier composed of silane coupling agent and dopamine in the above weight ratio is applied to the modification of bamboo fiber, the bonding effect of the silane coupling agent and the self-polymerization modification effect of dopamine are more compatible, so that the surface performance of the modified bamboo fiber is relatively stable, and thus after application, it can exert a relatively excellent corresponding effect.
[0024] Preferably, the weight ratio of the montmorillonite to the modified bamboo fiber is 2:5.
[0025] By adopting the above technical scheme, when montmorillonite and modified bamboo fiber in the above weight ratio are mixed for use, the coordination system formed between them is relatively stable, and the mixing with other raw materials is also relatively uniform, so that the biodegradable coating has better resistance to microcrack propagation, and thus the degradable sealing film as a whole has better structural strength.
[0026] Preferably, the specific surface area of the montmorillonite is 240-280 m 2 / g, interlayer spacing of 30-50 nm, and particle size of 60-100 nm; the diameter of the modified bamboo fiber is 20-25 μm.
[0027] By adopting the above technical scheme, the montmorillonite and modified bamboo fiber of the above specifications can not only be fully dispersed among the raw materials when used, and play an excellent role in the biodegradable coating, but also can be combined with the montmorillonite and modified bamboo fiber, and the combination system formed by the two can show excellent bonding with polylactic acid, cassava starch and ethylene-acrylic acid copolymer, thereby performing better in exerting the corresponding effects, so that the biodegradable coating has a better ability to resist microcrack propagation, and the structural strength of the degradable sealing film finally obtained is also better.
[0028] Preferably, the raw materials of the biodegradable coating are further added with 1-5 parts by weight of modified microcrystalline cellulose, and the modified microcrystalline cellulose is prepared by the following steps:
[0029] S1. Take plant residue powder and place it in a mixed solution of hydrogen peroxide and sodium hydroxide at a material-liquid ratio of 1: (25-35), treat it at 80-90°C for 3.5-4.5h, filter and dry it, then add it to a mixed solution of acetic acid and sodium hypochlorite, treat it at 70-75°C for 0.5-1.5h, wash it with deionized water and dry it to obtain cellulose material;
[0030] S2, placing the cellulose material obtained in S1 in a sulfuric acid solution, treating at 45-55° C. for 2.5-3.5 hours, washing with deionized water and drying to obtain microcrystalline cellulose material;
[0031] S3. After mixing the microcrystalline cellulose material obtained in S2 and styrene, add deionized water containing sodium carbonate and stir, add sodium dodecylbenzene sulfonate and potassium persulfate during the process, react at 70-75° C. for 10-12 hours under a nitrogen environment, cool, centrifuge, and extract with toluene to remove the styrene homopolymer to obtain modified microcrystalline cellulose.
[0032] By adopting the above technical scheme, in the preparation of modified microcrystalline cellulose, plant residue powder is first used as raw material and processed in step S1 and step S2 to obtain microcrystalline cellulose material. At this time, the size of the microcrystalline cellulose material is small and the surface has high activity. Then, step S3 is processed for functionalization to complete polystyrene grafting. The modified microcrystalline cellulose is applied to the biodegradable coating, which can have a good interface bonding strength with the mixed matrix of polylactic acid, cassava starch and ethylene-acrylic acid copolymer, and improve the strength and toughness of the biodegradable coating; at the same time, the modified microcrystalline cellulose can also deepen and supplement the action system of montmorillonite and modified bamboo fiber, thereby further improving the ability of the biodegradable coating to resist microcrack expansion, and finally the structural strength of the degradable sealing film is also significantly improved.
[0033] Preferably, the weight ratio of the montmorillonite, the modified bamboo fiber and the modified microcrystalline cellulose is 2:5:3.
[0034] By adopting the above technical scheme, when the montmorillonite, modified bamboo fiber and modified microcrystalline cellulose in the above weight ratio are used in combination, the overall coordination effect is relatively excellent, and the constructed system is more suitable for the mixed matrix of polylactic acid, cassava starch and ethylene-acrylic acid copolymer, and can bring excellent effects, thereby making the biodegradable coating have better resistance to microcrack propagation, and obtaining a degradable sealing film with better structural strength quality.
[0035] Preferably, the dispersant is one or a combination of sodium tripolyphosphate, sodium hexametaphosphate, sodium pyrophosphate, sodium lauryl sulfate, methylpentyl alcohol, cellulose derivatives, polyacrylamide, guar gum and fatty acid polyethylene glycol esters.
[0036] By adopting the above technical scheme, the above types of dispersants can exert excellent and stable effects after application, so that the raw materials can be fully dispersed and combined, and exert excellent self-effects and coordinated effects, thereby ensuring that the biodegradable coating has excellent and stable quality.
[0037] Preferably, the cross-linking agent is one or a combination of dicumyl peroxide, benzoyl peroxide, di-tert-butyl peroxide, dicumyl hydroperoxide, polyethyleneimine, isocyanate and aziridine.
[0038] By adopting the above technical scheme, the above types of cross-linking agents can stably act on the combination of polylactic acid, cassava starch and ethylene-acrylic acid copolymer after application, which is conducive to forming a stable mixed matrix and obtaining a biodegradable coating with excellent structural properties and stability.
[0039] Preferably, the thickener is one or a combination of sodium carboxymethyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl cellulose, sodium alginate and polyacrylamide.
[0040] By adopting the above technical solution, the thickener can increase the viscosity and consistency of the material, thereby improving the texture, stability and usage experience of the product. The above types of thickeners can all exert excellent corresponding effects in the raw material mixing system of the biodegradable coating, thereby ensuring that a biodegradable coating of excellent quality can be obtained.
[0041] In a second aspect, the present application provides a method for preparing a degradable sealing film, which adopts the following technical solution:
[0042] A method for preparing a degradable sealing film comprises the following steps:
[0043] (1) preparing raw materials including polylactic acid, cassava starch, ethylene-acrylic acid copolymer, dispersant, cross-linking agent, thickener, montmorillonite and modified bamboo fiber according to a ratio;
[0044] (2) heating the polylactic acid and ethylene-acrylic acid copolymer in step (1) to a molten state and mixing them uniformly, then adding cassava starch, a dispersant, a cross-linking agent and a thickener and mixing them, and finally adding montmorillonite and modified bamboo fiber and mixing them, and extruding and granulating them to obtain biodegradable coated particles;
[0045] (3) The paper substrate is fed into a laminating machine, and the biodegradable coating particles obtained in step (2) are melted and then laminarized on the surface of the paper substrate, and a biodegradable coating is formed after cooling to obtain a degradable sealing film.
[0046] By adopting the above technical scheme, the above preparation method is simple to operate, and each raw material is added and used in steps, which is convenient for quality control in the process, and is conducive to obtaining a degradable sealing film with stable and excellent quality, which is suitable for large-scale industrial production. At the same time, in the preparation of biodegradable coating particles, polylactic acid and ethylene-acrylic acid copolymer are first heated and melted and mixed, and then cassava starch, dispersant, cross-linking agent and thickener are added, which is conducive to obtaining a uniform and stable degradable matrix, and then montmorillonite and modified bamboo fiber are added, so that montmorillonite and modified bamboo fiber can fully play their own role, and can also cooperate with each other and play an excellent compounding effect, which is conducive to the subsequent acquisition of a biodegradable coating with excellent resistance to microcrack extension, and finally obtain a degradable sealing film with excellent structural strength.
[0047] In summary, this application has the following beneficial effects:
[0048] 1. In the present application, polylactic acid, cassava starch and ethylene-acrylic acid copolymer are combined to form the main mixed matrix of the biodegradable coating, and modified bamboo fiber and montmorillonite are compounded to improve the anti-microcrack propagation ability of the biodegradable coating, thereby significantly improving the overall structural strength of the degradable sealing film obtained in the end;
[0049] 2. The present application adds specially prepared modified microcrystalline cellulose, which not only has good interface bonding strength with the mixed matrix of polylactic acid, cassava starch and ethylene-acrylic acid copolymer, but also has a deepening and supplementary effect on the action system of montmorillonite and modified bamboo fiber, thereby further improving the ability of the biodegradable coating to resist microcrack propagation, and finally significantly improving the structural strength of the degradable sealing film. DETAILED DESCRIPTION
[0050] The present application is further described in detail below in combination with preparation examples, embodiments and comparative examples.
[0051] Unless otherwise specified, the raw materials used in the preparation examples and embodiments of the present application are commercially available:
[0052] Polylactic acid was purchased from Dongguan Hesheng Plastic Co., Ltd., model number Fengyuan FY201;
[0053] Cassava starch was purchased from Dongying Huaxuan Biotechnology Co., Ltd., model hx-05;
[0054] Ethylene-acrylic acid copolymer was purchased from Dongguan Xinmiao New Materials Co., Ltd., model number 21312;
[0055] Montmorillonite was purchased from Lingshou County Hongrun Mineral Products Processing Plant;
[0056] Bamboo fiber was purchased from Sichuan Changsheng New Material Technology Co., Ltd.
[0057] The silane coupling agent is KH-550 type silane coupling agent;
[0058] The plant residue powder was bagasse powder, purchased from Guangxi Senbaiyuan Agriculture Co., Ltd.;
[0059] The paper substrate was purchased from Dongguan Baimao Paper Co., Ltd., model BM-0002.
[0060] Preparation examples of raw materials and / or intermediates
[0061] Preparation Example 1
[0062] A modified bamboo fiber is prepared by the following modification steps:
[0063] S1, taking bamboo fiber raw material and putting it into 8% sodium hydroxide solution for immersion treatment for 24 hours, controlling the bath ratio to 1:20, washing with water and drying at 80°C for 8 hours to obtain pretreated bamboo fiber;
[0064] S2, mixing a silane coupling agent and dopamine as a modifier and placing them in deionized water to prepare a modified solution with a concentration of 4%, then immersing the pretreated bamboo fiber in the modified solution for treatment for 10 hours, taking out and drying at 80° C. for 8 hours to obtain the modified bamboo fiber;
[0065] In the above operation, the weight ratio of the silane coupling agent to dopamine is 1:2.5.
[0066] Preparation Example 2
[0067] A modified bamboo fiber, which is different from Preparation Example 1 in that it is prepared by the following modification steps:
[0068] S1, taking bamboo fiber raw material and putting it into a sodium hydroxide solution with a concentration of 6% and soaking it for 24 hours, controlling the bath ratio to be 1:20, washing with water and drying at 80°C for 8 hours to obtain pretreated bamboo fiber;
[0069] S2. A silane coupling agent and dopamine were mixed as a modifier and placed in deionized water to prepare a modified solution with a concentration of 3%. The pretreated bamboo fiber was then immersed in the modified solution for 10 hours, and then taken out and dried at 80° C. for 8 hours to obtain the modified bamboo fiber.
[0070] Preparation Example 3
[0071] S1, taking bamboo fiber raw material and putting it into 10% sodium hydroxide solution for immersion treatment for 24 hours, controlling the bath ratio to 1:20, washing with water and drying at 80°C for 8 hours to obtain pretreated bamboo fiber;
[0072] S2. A silane coupling agent and dopamine are mixed as a modifier and placed in deionized water to prepare a modified solution with a concentration of 5%. The pretreated bamboo fiber is then immersed in the modified solution for 10 hours, and then taken out and dried at 80° C. for 8 hours to obtain the modified bamboo fiber.
[0073] Preparation Example 4
[0074] A modified bamboo fiber, which is different from Preparation Example 1 in that the weight ratio of the silane coupling agent to dopamine is 1:2.
[0075] Preparation Example 5
[0076] A modified bamboo fiber, which is different from Preparation Example 1 in that the weight ratio of the silane coupling agent to dopamine is 1:3.
[0077] Preparation Example 6
[0078] A modified bamboo fiber, which is different from Preparation Example 1 in that no silane coupling agent is used in the modifier.
[0079] Preparation Example 7
[0080] A modified bamboo fiber, which is different from Preparation Example 1 in that silane dopamine is not used in the modifier.
[0081] Preparation Example 8
[0082] A modified microcrystalline cellulose is prepared by the following steps:
[0083] S1. Take plant residue powder and place it in a mixed solution of hydrogen peroxide and sodium hydroxide at a material-liquid ratio of 1:30, treat it at 85°C for 4 hours, filter and dry it, then add it to a mixed solution of acetic acid and sodium hypochlorite, treat it at 72.5°C for 1 hour, wash it with deionized water and dry it at 65°C for 4 hours to obtain a cellulose material;
[0084] S2, placing the cellulose material obtained in S1 in a sulfuric acid solution, treating at 50°C for 3 hours, washing with deionized water, and drying at 45°C for 8 hours to obtain microcrystalline cellulose material;
[0085] S3. After mixing the microcrystalline cellulose material obtained in S2 and styrene, add deionized water containing 0.5 wt% of sodium carbonate and stir, add sodium dodecylbenzene sulfonate and potassium persulfate during the process, react at 72.5° C. for 11 hours under a nitrogen environment, cool, centrifuge, and extract with toluene to remove the styrene homopolymer to obtain modified microcrystalline cellulose.
[0086] Note: In the above operation, in step S1, when hydrogen peroxide, sodium hydroxide, acetic acid and sodium hypochlorite are used respectively, the mass fraction of hydrogen peroxide is 0.8%, the mass fraction of sodium hydroxide is 4%, the concentration of acetic acid is 30 mol / L, and the concentration of sodium hypochlorite is 8 g / L; in step S2, the volume fraction of sulfuric acid solution is 65%; in step S3, the mass ratio of microcrystalline cellulose material to styrene is 40:1, the ratio of "mixture of microcrystalline cellulose material and styrene" to "deionized water containing 0.5 wt% sodium carbonate" is 1 g:2.6 mL, the amount of sodium dodecylbenzene sulfonate used is 8% of the weight of styrene, and the amount of potassium persulfate used is 3% of the weight of styrene.
[0087] Preparation Example 9
[0088] A modified microcrystalline cellulose, which is different from Preparation Example 8 in that it is prepared by the following steps:
[0089] S1. Take plant residue powder and place it in a mixed solution of hydrogen peroxide and sodium hydroxide at a material-liquid ratio of 1:25, treat it at 80°C for 4.5 hours, filter and dry it, then add it to a mixed solution of acetic acid and sodium hypochlorite, treat it at 70°C for 1.5 hours, wash it with deionized water, and dry it at 65°C for 4 hours to obtain a cellulose material;
[0090] S2, placing the cellulose material obtained in S1 in a sulfuric acid solution, treating at 45°C for 2.5 hours, washing with deionized water, and drying at 45°C for 8 hours to obtain microcrystalline cellulose material;
[0091] S3. After mixing the microcrystalline cellulose material obtained in S2 and styrene, add deionized water containing 0.5 wt% of sodium carbonate and stir, add sodium dodecylbenzene sulfonate and potassium persulfate during the process, react at 70° C. for 12 h under a nitrogen environment, cool, centrifuge, and extract with toluene to remove the styrene homopolymer to obtain modified microcrystalline cellulose.
[0092] Preparation Example 10
[0093] A modified microcrystalline cellulose, which is different from Preparation Example 8 in that it is prepared by the following steps:
[0094] S1. Take plant residue powder and place it in a mixed solution of hydrogen peroxide and sodium hydroxide at a material-liquid ratio of 1:35, treat it at 90°C for 3.5 hours, filter and dry it, then add it to a mixed solution of acetic acid and sodium hypochlorite, treat it at 75°C for 0.5 hours, wash it with deionized water, and dry it at 65°C for 4 hours to obtain a cellulose material;
[0095] S2, placing the cellulose material obtained in S1 in a sulfuric acid solution, treating at 55°C for 2.5 hours, washing with deionized water, and drying at 45°C for 8 hours to obtain microcrystalline cellulose material;
[0096] S3. After mixing the microcrystalline cellulose material obtained in S2 and styrene, add deionized water containing 0.5 wt% of sodium carbonate and stir, add sodium dodecylbenzene sulfonate and potassium persulfate during the process, react at 75° C. for 10 h under a nitrogen environment, cool, centrifuge, and extract with toluene to remove the styrene homopolymer to obtain modified microcrystalline cellulose.
[0097] Example:
[0098] Example 1
[0099] A degradable sealing film comprises a paper substrate and a biodegradable coating disposed on the paper substrate. The raw materials used to prepare the biodegradable coating and their corresponding weights are shown in Table 1, and the biodegradable coating is prepared by the following steps:
[0100] (1) preparing raw materials including polylactic acid, cassava starch, ethylene-acrylic acid copolymer, dispersant, cross-linking agent, thickener, montmorillonite and modified bamboo fiber according to a ratio;
[0101] (2) putting the polylactic acid and ethylene-acrylic acid copolymer prepared in step (1) into an internal mixer, heating them to a molten state, and mixing them uniformly, then adding cassava starch, a dispersant, a cross-linking agent, and a thickener, and mixing them for 10 minutes, and finally adding montmorillonite and modified bamboo fiber, and mixing them for 20 minutes, and extruding and granulating them to obtain biodegradable coated particles;
[0102] (3) The paper substrate is fed into a laminating machine, and the biodegradable coating particles obtained in step (2) are melted and then laminarized on the surface of the paper substrate. The laminating temperature is 150° C. After cooling, a biodegradable coating is formed to obtain a degradable sealing film.
[0103] Note: The modified bamboo fiber used was obtained from Preparation Example 1; the specific surface area of montmorillonite is 260 m 2 / g, interlayer spacing is 40nm, particle size is 80nm; the diameter of the modified bamboo fiber is 22.5μm; the dispersant is sodium tripolyphosphate; the cross-linking agent is diisopropyl peroxide; and the thickener is sodium carboxymethyl cellulose.
[0104] Example 2-3
[0105] A degradable sealing film, which is different from Example 1 in that the raw materials used to prepare the biodegradable coating and their corresponding weights are shown in Table 1.
[0106]
[0107] Example 4
[0108] A degradable sealing film, which is different from Example 1 in that the specific surface area of montmorillonite is 240 m 2 / g, interlayer spacing is 50μm, particle size is 100nm; the diameter of modified bamboo fiber is 20μm.
[0109] Example 5
[0110] A degradable sealing film, which is different from Example 1 in that the specific surface area of montmorillonite is 280 m 2 / g, interlayer spacing is 30 nm, particle size is 60 nm; the diameter of the modified bamboo fiber is 25 μm.
[0111] Example 6
[0112] A degradable sealing film, which is different from Example 1 in that the modified bamboo fiber is obtained from Preparation Example 2.
[0113] Example 7
[0114] A degradable sealing film, which is different from Example 1 in that the modified bamboo fiber is obtained from Preparation Example 3.
[0115] Example 8
[0116] A degradable sealing film, which is different from Example 1 in that the modified bamboo fiber is obtained from Preparation Example 4.
[0117] Example 9
[0118] A degradable sealing film, which is different from Example 1 in that the modified bamboo fiber is obtained from Preparation Example 5.
[0119] Example 10
[0120] A degradable sealing film is different from Example 1 in that the total amount of montmorillonite and modified bamboo fiber remains unchanged, and the weight ratio of the two is adjusted to 2:5.
[0121] Embodiment 11
[0122] A degradable sealing film, which is different from Example 1 in that 3 parts by weight of modified microcrystalline cellulose are also added to the raw materials of the biodegradable coating, and the modified microcrystalline cellulose is obtained by Preparation Example 8 and is added and used together with montmorillonite and modified bamboo fiber in the preparation of the degradable sealing film.
[0123] Example 12
[0124] A degradable sealing film, which is different from Example 11 in that the weight portion of modified microcrystalline cellulose added is 1 part.
[0125] Example 13
[0126] A degradable sealing film, which is different from Example 11 in that the weight portion of modified microcrystalline cellulose added is 5 parts.
[0127] Embodiment 14
[0128] A degradable sealing film, which is different from Example 11 in that the modified microcrystalline cellulose is obtained from Preparation Example 9.
[0129] Embodiment 15
[0130] A degradable sealing film, which is different from Example 11 in that the modified microcrystalline cellulose is obtained from Preparation Example 10.
[0131] Comparative Example
[0132] Comparative Example 1
[0133] A degradable sealing film, which is different from Example 1 in that montmorillonite and modified bamboo fiber are not used in the raw materials for preparing the biodegradable coating.
[0134] Comparative Example 2
[0135] A degradable sealing film, which is different from Example 1 in that montmorillonite is not used in the raw materials for preparing the biodegradable coating.
[0136] Comparative Example 3
[0137] A degradable sealing film, which is different from Example 1 in that modified bamboo fiber is not used in the raw materials for preparing the biodegradable coating.
[0138] Comparative Example 4
[0139] A degradable sealing film, which is different from Example 1 in that the modified bamboo fiber is obtained from Preparation Example 6.
[0140] Comparative Example 5
[0141] A degradable sealing film, which is different from Example 1 in that the modified bamboo fiber is obtained from Preparation Example 7.
[0142] Comparative Example 6
[0143] A degradable sealing film, which is different from Example 1 in that the modified bamboo fiber is replaced by unmodified bamboo fiber raw material.
[0144] Comparative Example 7
[0145] A degradable sealing film, which is different from Example 11 in that montmorillonite and modified bamboo fiber are not used in the preparation raw materials of the biodegradable coating.
[0146] Performance testing
[0147] Test samples: The degradable sealing films obtained in Examples 1-15 and Comparative Examples 1-7 were used as test samples 1-15 and control samples 1-7, and the thickness of the paper substrate was 0.20 mm, and the thickness of the biodegradable coating was 0.07 mm.
[0148] Test method: Evaluate the tear strength improvement rate of the biodegradable coating on the paper substrate; use the domestic NBC-563B touch screen paper microcomputer tear tester to test the tear strength of the paper substrate for three times, and take the average value as A; then take the degradable sealing film, and use the domestic NBC-563B touch screen paper microcomputer tear tester to test the tear strength of the paper substrate in the same way, for three times, and take the average value as B; calculate the tear strength improvement rate, tear strength improvement rate (%) = (BA) / A, the greater the tear strength improvement rate, the stronger the biodegradable coating's ability to resist microcrack propagation, and the better the overall structural strength of the paper sealing film; after completing the tests of test samples 1-15 and control samples 1-7 in turn, the corresponding records are recorded in Table 2.
[0149]
[0150]
[0151] Combining Examples 1-3 and Comparative Examples 1-3 and Table 2, it can be seen that by using the modified bamboo fiber and montmorillonite in the biodegradable coating, the microcrack extension resistance of the biodegradable coating can be significantly improved, and the tear strength improvement rate is excellent; if only any one of the modified bamboo fiber and montmorillonite is used in the biodegradable coating, it is found that compared with the biodegradable coating without using modified bamboo fiber and montmorillonite, although the microcrack extension resistance is improved, the improvement effect is limited. At the same time, it is also found that the sum of the improvement effects brought by the modified bamboo fiber and montmorillonite is far less than the excellent effect brought by the combination of the two, indicating that the modified bamboo fiber and montmorillonite have a significant effect on improving the overall structural strength of the degradable sealing film.
[0152] Combining Example 1 and Example 6-9 with Table 2, it can be seen that in the preparation of modified bamboo fiber, when the weight ratio of silane coupling agent and dopamine in the modifier used is 1: (2-3), it can be ensured that the modified bamboo fiber obtained can exert excellent and stable effects after application; combined with Comparative Example 6 and Table 2, it can be seen that if the modified bamboo fiber is replaced with unmodified bamboo fiber raw material, it is found that the unmodified bamboo fiber cannot exert an excellent compounding effect with montmorillonite, and the tear strength improvement rate obtained by the test will also be significantly reduced; combined with Comparative Examples 4-5 and Table 2, it can be seen that in the preparation of modified bamboo fiber, if only silane coupling agent or dopamine is used as a modifier alone, it is found that the modified bamboo fiber obtained cannot exert an excellent compounding effect with montmorillonite, and is only slightly improved compared to the unmodified bamboo fiber raw material. It can be seen that the modified bamboo fiber obtained by the combined modification of silane coupling agent and dopamine is a necessary raw material for achieving an excellent compounding effect with montmorillonite and is irreplaceable. Combined with Example 10 and Table 2, it can be seen that when the weight ratio of montmorillonite to modified bamboo fiber is 2:5, the biodegradable coating has better resistance to microcrack propagation, and thus the degradable sealing film as a whole has better structural strength.
[0153] Combining Example 1 and Examples 11-15 with Table 2, it can be seen that by adding specially prepared modified microcrystalline cellulose, the tear strength improvement rate can be significantly improved, indicating that the resistance of the biodegradable coating to microcrack propagation is further improved; Combining Comparative Example 7 with Table 2, it can be seen that without the presence of montmorillonite and modified bamboo fiber, the effect brought by the modified microcrystalline cellulose is greatly discounted, indicating that the excellent effect of modified microcrystalline cellulose is inseparable from montmorillonite and modified bamboo fiber, and only when modified microcrystalline cellulose, montmorillonite and modified bamboo fiber are present together in the biodegradable coating, the resistance to microcrack propagation of the biodegradable coating is best improved.
[0154] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A degradable sealing film, characterized in that: It comprises a paper substrate and a biodegradable coating disposed on the paper substrate, wherein the biodegradable coating is made of the following raw materials in parts by weight: Polylactic acid 40-50 parts; 10-20 parts of tapioca starch; 15-25 parts of ethylene-acrylic acid copolymer; 3-5 parts of dispersant; 2-3 parts of cross-linking agent; Thickener 1-3 parts; 1.5-2.5 parts of montmorillonite; 2-6 parts of modified bamboo fiber; The modified bamboo fiber is prepared by the following modification steps: S1, taking bamboo fiber raw materials and soaking them in a sodium hydroxide solution with a concentration of 6-10%, washing and drying them to obtain pretreated bamboo fibers; S2, mixing a silane coupling agent and dopamine as a modifier and placing them in deionized water to prepare a modified solution with a concentration of 3-5%, then immersing the pretreated bamboo fiber in the modified solution for treatment, taking it out and drying it to obtain the modified bamboo fiber; The weight ratio of silane coupling agent to dopamine is 1:(2-3); The raw materials of the biodegradable coating are further added with 1-5 parts by weight of modified microcrystalline cellulose, and the modified microcrystalline cellulose is prepared by the following steps: S1. Take plant residue powder and place it in a mixed solution of hydrogen peroxide and sodium hydroxide at a material-liquid ratio of 1: (25-35), treat it at 80-90°C for 3.5-4.5h, filter and dry it, then add it to a mixed solution of acetic acid and sodium hypochlorite, treat it at 70-75°C for 0.5-1.5h, wash it with deionized water and dry it to obtain cellulose material; S2, placing the cellulose material obtained in S1 in a sulfuric acid solution, treating at 45-55° C. for 2.5-3.5 hours, washing with deionized water and drying to obtain microcrystalline cellulose material; S3, mixing the microcrystalline cellulose material obtained in S2 with styrene, adding deionized water containing sodium carbonate and stirring, adding sodium dodecylbenzene sulfonate and potassium persulfate during the process, reacting at 70-75° C. for 10-12 hours under a nitrogen environment, cooling, centrifuging, and then extracting with toluene to remove the styrene homopolymer to obtain modified microcrystalline cellulose; The weight ratio of the montmorillonite, the modified bamboo fiber and the modified microcrystalline cellulose is 2:5:
3.
2. The degradable sealing film according to claim 1, characterized in that: The weight ratio of the silane coupling agent to dopamine is 1:2.
5.
3. The degradable sealing film according to claim 1, characterized in that: The weight ratio of the montmorillonite to the modified bamboo fiber is 2:
5.
4. The degradable sealing film according to claim 1, characterized in that: The specific surface area of the montmorillonite is 240-280 m 2 / g, interlayer spacing of 30-50 nm, and particle size of 60-100 nm; the diameter of the modified bamboo fiber is 20-25 μm.
5. The degradable sealing film according to claim 1, characterized in that: The dispersant is one or a combination of sodium tripolyphosphate, sodium hexametaphosphate, sodium pyrophosphate, sodium lauryl sulfate, methyl amyl alcohol, cellulose derivatives, polyacrylamide, guar gum and fatty acid polyethylene glycol ester.
6. The degradable sealing film according to claim 1, characterized in that: The crosslinking agent is one or a combination of dicumyl peroxide, benzoyl peroxide, di-tert-butyl peroxide, dicumyl hydroperoxide, polyethyleneimine, isocyanate and aziridine.
7. The degradable sealing film according to claim 1, characterized in that: The thickener is one or a combination of sodium carboxymethyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl cellulose, sodium alginate and polyacrylamide.
8. The method for preparing a degradable sealing film according to claim 1, characterized in that: The following steps are involved: (1) preparing raw materials including polylactic acid, cassava starch, ethylene-acrylic acid copolymer, dispersant, cross-linking agent, thickener, montmorillonite, modified bamboo fiber and modified microcrystalline cellulose according to a proportion; (2) heating the polylactic acid and ethylene-acrylic acid copolymer in step (1) to a molten state and mixing them uniformly, then adding cassava starch, a dispersant, a cross-linking agent and a thickener and mixing them, and finally adding montmorillonite, modified bamboo fiber and modified microcrystalline cellulose and mixing them, and extruding and granulating them to obtain biodegradable coated particles; (3) The paper substrate is fed into a laminating machine, and the biodegradable coating particles obtained in step (2) are melted and then laminarized on the surface of the paper substrate, and a biodegradable coating is formed after cooling to obtain a degradable sealing film.
Citation Information
Patent Citations
Biodegradable films
CN103003338A
Easily-degradable film
CN104893065A
Biodegradable starch membrane material and membrane thereof
CN107722570A
Flame-retardant and antibacterial towel fabric and preparation process thereof
CN113417143A
Coating as well as preparation method and application thereof
CN116289304A