A high-freedom liquid crystal molecular assembly method based on laser direct writing

Through femtosecond laser direct writing and CO2 supercritical drying technology, high-degree of freedom liquid crystal molecules are achieved, solving the problems of complex operation and low degree of freedom in the existing technology, and achieving high-precision and high degree of freedom liquid crystal molecules , suitable for a variety of laser direct writing materials.

CN118605088BActive Publication Date: 2024-11-15HUAZHONG UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410596049.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-14
Publication Date
2024-11-15
Estimated Expiration
2044-05-14

AI Technical Summary

Technical Problem

The existing liquid crystal molecular assembly technology has cumbersome operation steps, complex equipment, and low freedom, making it difficult to achieve customized three-dimensional assembly with high freedom, which limits the functional application of liquid crystal molecules.

Method used

采用基于激光直写的高自由度液晶分子组装方法,通过飞秒激光构建二维或三维扫描路径,使液晶分子按照扫描路径有序组装,结合CO2超临界干燥技术,实现高精度和高自由度的液晶分子组装。

Benefits of technology

It realizes high-precision customized assembly at the submicron scale, simplifies the process flow, is suitable for liquid crystal molecules and other direct laser writing materials, and improves the resolution and functional performance of optoelectronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118605088B_ABST
    Figure CN118605088B_ABST
Patent Text Reader

Abstract

The present invention proposes a method for assembling liquid crystal molecules with high degrees of freedom based on laser direct writing, comprising the following steps: S1, drop a liquid crystal precursor solution on a substrate, focus a femtosecond laser, the focus spot radius is ≤600nm, and a femtosecond laser direct writing technology is used to construct a separate two-dimensional or three-dimensional scanning path so that the liquid crystal molecules are assembled in order according to the scanning path, the aspect ratio of the polymer structure is ≥5:1, and the line spacing of the direct writing structure is greater than the focus spot radius; S2, after the assembly is completed, the uncured precursor on the substrate is removed by development, and for the three-dimensional polymer structure, the substrate needs to be placed in a CO2 supercritical dryer for drying to obtain a high degree of freedom liquid crystal molecule assembly. The present invention utilizes femtosecond laser path programming to achieve customized high-degree-of-freedom 2D and 3D liquid crystal molecule assembly; utilizes two-photon polymerization to achieve high-precision assembly with a resolution beyond the diffraction limit; the present invention solidifies the liquid crystal while orienting the liquid crystal, so only one step is required to achieve the assembly of liquid crystal molecules, achieving the simplicity of the process. Compared with the existing liquid crystal molecule assembly method, the present invention has the advantages of high precision and high degree of freedom (arbitrary three-dimensional orientation) at the submicron scale, simple assembly process, and a wide range of applicable materials; and there is no need to build other complex field orientation devices or special treatment of the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of liquid crystal molecule assembly, and in particular to a high-freedom liquid crystal molecule assembly method based on laser direct writing. Background Art

[0002] Liquid crystal materials are widely used in liquid crystal displays, optoelectronic devices, sensors, smart windows, actuators, etc. due to their excellent optoelectronic properties. Liquid crystal materials need to be assembled from an isotropic state to a long-range ordered state in order to achieve their excellent optical, electrical, magnetic, and mechanical properties. This assembly technology is called liquid crystal molecular assembly.

[0003] There are various methods in this field to arrange liquid crystal molecules in an orderly manner, including mechanical deformation methods, surface forced assembly, field assembly and other methods. Mechanical stretching methods are often used for simple liquid crystal molecule orientation, which orients liquid crystal molecules by curling, stamping, stretching and embossing methods, and solidifies the orientation of molecules by a two-step crosslinking method. This method has poor programmability and requires a two-step method to achieve assembly. Surface forced assembly has been used in the field of liquid crystal display. This method constructs micro-nano structures on the surface of the substrate to orient the liquid crystal molecules along the direction of the micro-nano structures. The three-dimensional assembly direction obtained by this method cannot be independently defined, and it is necessary to first construct micro-nano structures by means of photolithography, and then assemble liquid crystal molecules by photocuring. Field orientation methods include photoelectric magnetic field assembly, among which light field orientation is mainly used for two-dimensional liquid crystal molecule assembly, and electromagnetic fields can be used for three-dimensional liquid crystal molecule assembly, but the direction of this electromagnetic field is limited, and arbitrary three-dimensional spatial orientation cannot be achieved, and it is necessary to build a complex electromagnetic field device on the photocuring 3D printing equipment.

[0004] In summary, the above assembly methods have complicated operation steps and complex devices, which restricts the simplicity of the process. At the same time, these directional assembly methods are limited by their low degree of freedom, and it is difficult to achieve customized high-freedom three-dimensional assembly of liquid crystal molecules, which seriously limits the functional application of liquid crystal molecules. Therefore, the existing technical means have great limitations in accuracy, degree of freedom, simplicity of process, and functional customization. Summary of the invention

[0005] In view of the limitations of the prior art and the demand for high-precision and customizable molecular assembly, the present invention proposes a high-freedom liquid crystal molecular assembly method based on laser direct writing.

[0006] The technical solution of the present invention is implemented as follows: The present invention provides a method for assembling liquid crystal molecules with a high degree of freedom based on laser direct writing, comprising the following steps:

[0007] S1, drop a liquid crystal precursor solution on a substrate, focus a femtosecond laser, the focus spot radius is ≤600nm, and a femtosecond laser direct writing technique is used to construct a separate two-dimensional or three-dimensional scanning path so that the liquid crystal molecules are assembled in order according to the scanning path, the aspect ratio of the polymerized structure is ≥5:1, and the line spacing of the direct writing structure is greater than the focus spot radius;

[0008] S2, after the assembly is completed, the uncured precursor on the substrate is removed by development. For the three-dimensional polymer structure, the substrate needs to be placed in a CO2 supercritical dryer for drying to obtain a liquid crystal molecule assembly with a high degree of freedom.

[0009] The assembly principle of the present invention is: by moving a small-sized tightly focused laser spot, shear orientation is achieved, and the liquid crystal molecules are oriented along the laser scanning direction. The subsequent shrinkage process (development) further achieves the orientation of the polymer main chain in the scanning direction through volume compression, thereby achieving the orientation of the liquid crystal molecules. These two processes together orient the liquid crystal molecules in the laser scanning direction.

[0010] The present invention is different from ordinary laser direct writing in that: the spot radius is ≤600nm, preferably 350-600nm, otherwise the orientation order of the liquid crystal molecules will decrease (10x oil objective); the spacing between the structural lines of direct writing is at least larger than the radius of the spot, that is, the polymerized line structures are not connected to each other and are separated line structures; the aspect ratio of the line structure of direct writing is ≥5:1, otherwise the anisotropy is lost and the assembly of liquid crystal molecules cannot be achieved; if used for printing a high-degree-of-freedom three-dimensional structure, a supercritical apparatus needs to be used for drying after the direct writing is completed to prevent the structure from collapsing due to surface tension.

[0011] Supercritical drying principle: Supercritical drying is to control the pressure and temperature to make the solvent reach its critical point during the drying process and complete the supercritical transition from liquid phase to gas phase. In the process, the solvent has no obvious surface tension. Since there is no gas-liquid interface, there is no capillary action, so it will not cause the gel to shrink or damage its structure.

[0012] On the basis of the above technical solution, preferably, during the CO2 supercritical drying in step S2, the pressure is ≥1072psi, the sample chamber temperature is 33°C to 39°C, and the drying is performed for 4 to 10 minutes.

[0013] The supercritical parameters must ensure that the pressure in the sample chamber is above 1072psi and the temperature in the sample chamber is above 31°C, generally between 33°C and 39°C. At such temperature and pressure, carbon dioxide reaches a critical state and maintains this state for at least 4 minutes, generally 4 to 10 minutes, before starting to exhaust.

[0014] On the basis of the above technical solution, preferably, the line spacing of the direct-write structure is ≥700 nm, and the polymerized structures are not connected to each other, and are separate line structures.

[0015] On the basis of the above technical solution, preferably, the liquid crystal precursor solution includes liquid crystal monomers, a cross-linking agent, a free radical inhibitor and a photoinitiator.

[0016] On the basis of the above technical scheme, preferably, the liquid crystal monomer is one or more of 4-cyanophenyl 4'-(6-acryloyloxyhexyloxy)benzoate, 1,4-bis-[4-(3-acryloyloxypropoxy)benzoyloxy]-2-methylbenzene, and 1,4-bis-[4-(6-acryloyloxyhexyloxy)benzoyloxy]-2-methylbenzene.

[0017] On the basis of the above technical scheme, preferably, the cross-linking agent is a thiol or a multifunctional vinyl compound, selected from one or more of 2,2'-(1,2-ethylenedioxy)diethanethiol, pentaerythritol tetrakis(3-mercaptopropionic acid)ester, and 1,3,5-triallyl-1,3,5-triazine-2,4,6(1H,3H,5H)-trione.

[0018] On the basis of the above technical solution, preferably, the free radical inhibitor is one or more of dibutylhydroxytoluene, hydroquinone monomethyl ether and p-tert-butylpyrocatechol.

[0019] In order to obtain anisotropy, the aspect ratio needs to be at least 5:1. To achieve an aspect ratio greater than 5:1, the present invention adds a free radical inhibitor to the liquid crystal precursor solution. Under the same lighting conditions, the presence of the inhibitor causes free radical polymerization to occur only in the area further inside the focus, and the area where light can trigger free radical polymerization is smaller, resulting in a smaller line width for laser direct writing. After the line width is reduced, it indicates that a ratio greater than 5:1 will be easier to achieve, that is, anisotropy can be obtained with a shorter length, which means that in the preparation of optoelectronic devices, the present invention can obtain higher resolution and therefore has better optoelectronic modulation performance.

[0020] On the basis of the above technical solution, preferably, the photoinitiator is one or more of 2,4,6-trimethylbenzoyldiphenoxyphosphine, benzil and azobisisobutyronitrile.

[0021] On the basis of the above technical scheme, preferably, the molar ratio of the liquid crystal monomer: cross-linking agent is 5-8:1, the molar ratio of the liquid crystal monomer: free radical inhibitor is 25-30:1, and the molar ratio of the liquid crystal monomer: photoinitiator is 20-25:1.

[0022] On the basis of the above technical scheme, preferably, the preparation method of the liquid crystal precursor solution is: add liquid crystal monomer molecules, cross-linking agent, and free radical inhibitor to a non-polar organic solvent, heat to 70°C ~ 100°C to dissolve them, cool and centrifuge to obtain the supernatant after dissolution; then ultrasonically dissolve the photoinitiator in the supernatant, and let it stand for 10 to 12 hours to obtain a liquid crystal precursor solution.

[0023] On the basis of the above technical solution, preferably, the non-polar organic solvent is one or more of m-dichlorobenzene, toluene, benzene, cyclohexane and dichloromethane.

[0024] On the basis of the above technical solution, preferably, the substrate is selected from one of soda-lime glass, quartz sheet, ITO glass and silicon sheet.

[0025] On the basis of the above technical scheme, preferably, after the assembly is completed, the two-dimensional polymer structure is placed in propylene glycol methyl ether acetate for development for 3 to 10 minutes, and then rinsed in isopropanol and methyl nonafluorobutyl ether solvents for 1 to 3 minutes respectively; for the three-dimensional polymer structure, it needs to be placed in ethanol for cleaning after development, and then subjected to CO2 supercritical drying.

[0026] On the basis of the above technical solution, preferably, the femtosecond laser scanning speed is 10 to 200 μm / s, and the laser power is 20 to 50 mW.

[0027] The high-freedom liquid crystal molecule assembly method based on laser direct writing of the present invention has the following beneficial effects compared with the prior art:

[0028] (1) The present invention uses femtosecond laser path programming to achieve customized high-freedom 2D and 3D liquid crystal molecular assembly; uses two-photon polymerization to achieve high-precision assembly with a resolution beyond the diffraction limit; the present invention solidifies the liquid crystal while orienting the liquid crystal, so only one step is required to achieve the assembly of liquid crystal molecules, achieving the simplicity of the process. Compared with the existing liquid crystal molecular assembly method, the present invention has the advantages of high precision and high freedom (arbitrary three-dimensional orientation) at the submicron scale, simple assembly process, and a wide range of applicable materials; and there is no need to build other complex field orientation devices or special treatment of the substrate.

[0029] (2) The free radical inhibitor in the liquid crystal precursor solution of the present invention has the function of preventing dark reaction and making the precursor more stable. It also has the technical effect of reducing the line width and achieving high-precision liquid crystal molecules. This means that in the preparation of optoelectronic devices, the present invention can obtain higher resolution and thus has better optoelectronic modulation performance.

[0030] (3) The assembly method disclosed in the present invention can realize high-precision customized assembly at the submicron scale. In addition to being used for liquid crystal molecular assembly, it can also be used for isotropic laser direct writing materials such as acrylate monomer molecules, hydrogel monomer molecules, acrylamide monomer molecules, SU8-type epoxy resins, etc., and has broad application prospects in the fields of micro-nano optics, microfluidic systems, and micro-nano robotics research. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0032] Figure 1 A single-line structure diagram of the liquid crystal molecules assembled in Example 1;

[0033] Figure 2 This is a schematic diagram of anisotropic assembly of liquid crystal molecules obtained by laser direct writing and development in Example 1;

[0034] Figure 3 It is a single line structure diagram of continuous and separated;

[0035] Figure 4 It is the single line structure diagram with different aspect ratios;

[0036] Figure 5 This is a three-dimensional anisotropic structure diagram of liquid crystal molecules assembled in Example 6;

[0037] Figure 6 The three-dimensional anisotropic structure diagram of different drying methods;

[0038] Figure 7 Schematic diagram of anisotropic assembly of hydrogel molecules;

[0039] Figure 8 POM image of anisotropically assembled acrylate resin molecules;

[0040] Fig. 9 This is the SEM image of the single wire structure of Comparative Example 4. DETAILED DESCRIPTION

[0041] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] The substrate used in the present invention is ultrasonically cleaned in acetone and deionized water before use to remove organic and inorganic impurities, and then the liquid residue on the substrate is blown away with a nitrogen gun. If necessary, a sandwich layer can be made on the substrate to prevent the liquid from flowing out, and the sandwich layer is composed of a polyimide tape with a height of 50 to 100 μm.

[0043] The laser scanning path method in the present invention is to control the scanning of the galvanometer in the xy direction in a two-dimensional plane or to control the movement of the piezoelectric displacement stage in a three-dimensional space, thereby realizing the two-dimensional or three-dimensional directional assembly of molecules.

[0044] Method 1 for determining anisotropic assembly of liquid crystal materials of the present invention: The anisotropy of the liquid crystal structure is observed through a polarized light microscope (POM). The bright part in the POM photo indicates that the structure is anisotropic, and the dark part in the POM photo indicates that the structure is isotropic. The brightness and darkness in the POM image are used to determine whether the printed liquid crystal structure is anisotropic.

[0045] Method 2 for determining the anisotropic assembly of liquid crystal materials: The degree of anisotropic order of liquid crystal materials is measured by microscopic Fourier transform infrared spectroscopy. The maximum absorption value of the liquid crystal material at different polarization angles is divided by the minimum absorption value to obtain the dichroic ratio. The degree of order S = (D-1) / (D+2). The greater the degree of order, the stronger the degree of anisotropy. <S<1。

[0046] Example 1 Two-dimensional anisotropic assembly of liquid crystal monomer molecules

[0047] In this implementation case, reactive liquid crystal molecules are used as monomers, and a thiol-ene click chemistry reaction system is used to prepare the precursor required for laser direct writing. The obtained precursor does not require any orientation treatment. The liquid crystal molecules are assembled by programming using a laser scanning path defined by a galvanometer. After laser direct writing and development, the isotropic reactive liquid crystal molecules are orderly assembled into an anisotropic structure along the laser scanning direction. The specific steps are as follows:

[0048] S1, take 4-cyanophenyl 4'-(6-acryloyloxyhexyloxy)benzoate reactive liquid crystal monomer, and the free radical inhibitor butylated hydroxytoluene and the crosslinking agent 2,2'-(1,2-ethylenedioxy)bis(ethyl mercaptan) are heated in a water bath at 100°C and dissolved in a non-polar solvent m-dichlorobenzene; the molar ratio of the monomer to the crosslinking agent is 5:1, and the molar ratio of the monomer to the free radical inhibitor is 25:1.

[0049] S2, placing the precursor solution in step S2 in a centrifuge, centrifuging at 300 rpm for 3 min, and taking the supernatant for later use.

[0050] S3, dissolving 2,4,6-trimethylbenzoyldiphenoxy phosphorescent photoinitiator in the supernatant in step S2 by ultrasonication, and letting it stand for 12 hours; the molar ratio of monomer to photoinitiator is 20:1.

[0051] S4, drop the precursor solution obtained in step S3 onto the transparent substrate soda-lime glass, then fix the substrate on the sample stage, use a 25x oil objective to focus the near-infrared femtosecond laser, the radius of the laser spot after focusing is 600nm, and adjust the focus position to the substrate.

[0052] S5, the galvanometer is programmed to achieve arbitrary 2D scanning. The femtosecond laser scanning speed is 10-200 μm / s, the laser power is 20-50 mW, the line spacing is 700 nm, the direct writing structure is a separated single line structure, and the single line structure aspect ratio is 5:1, so that anisotropy can be maintained (see Figure 1 ).

[0053] S6, after processing, the substrate is placed in propylene glycol methyl ether acetate for development for 3 minutes, and then rinsed in isopropyl alcohol and methyl nonafluorobutyl ether solvents for 1 minute in turn to prevent structural damage caused by surface tension.

[0054] Figure 1 Figures a and e show the laser direct writing separation line structures at different angles, and θ is the angle between the direct writing direction and the horizontal direction. Figures b and c show the POM images of the separated single line structure θ=0° under different polarizations, proving the anisotropy of the separated single line structure θ=0°. Figures f and g show the POM images of the separated single line structure θ=45° under different polarizations, proving the anisotropy of the separated single line structure θ=45°.

[0055] Figure 2 After the display laser is scanned and developed, the liquid crystal molecules are oriented in the direction of the laser scanning and arranged in order into an anisotropic structure.

[0056] Example 2 Two-dimensional anisotropic assembly of liquid crystal monomer molecules

[0057] S1, take 1,4-bis-[4-(3-acryloxypropoxy)benzoyloxy]-2-methylbenzene reactive liquid crystal monomer, and the free radical inhibitor hydroquinone monomethyl ether and the cross-linking agent pentaerythritol tetrakis(3-mercaptopropionic acid) ester, heat them in a water bath at 100°C and dissolve them in a non-polar solvent cyclohexane; the molar ratio of the monomer to the cross-linking agent is 6:1, and the molar ratio of the monomer to the free radical inhibitor is 30:1.

[0058] S2, placing the precursor solution in step S2 in a centrifuge, centrifuging at 500 rpm for 3 min, and taking the supernatant for later use.

[0059] S3, dissolving the azobisisobutyronitrile photoinitiator in the supernatant in step S2 by ultrasonication, and letting it stand for 10 hours; the molar ratio of the monomer to the photoinitiator is 25:1.

[0060] S4, drop the precursor solution obtained in step S3 onto an opaque substrate silicon wafer, then fix the substrate on a sample stage, use a 60x oil objective to focus the near-infrared femtosecond laser, the laser spot radius after focusing is 350nm, and adjust the focal position to the substrate.

[0061] S5, program the galvanometer to achieve arbitrary 2D scanning, the femtosecond laser scanning speed is 10-200μm / s, the laser power is 20-50mW, the line spacing is 800nm, the direct writing structure is a separated single line structure, and the single line structure aspect ratio is 8:1.

[0062] S6, after processing, the substrate is placed in propylene glycol methyl ether acetate for development for 5 minutes, and then rinsed in isopropyl alcohol and methyl nonafluorobutyl ether solvents for 3 minutes in sequence to prevent structural damage caused by surface tension.

[0063] Example 3 Two-dimensional anisotropic assembly of liquid crystal monomer molecules

[0064] S1, take 1,4-bis-[4-(6-acryloyloxyhexyloxy)benzoyloxy]-2-methylbenzene reactive liquid crystal monomer, and the free radical inhibitor p-tert-butylpyrocatechol and the cross-linking agent pentaerythritol tetrakis(3-mercaptopropionic acid) ester, heat in a water bath at 100°C and dissolve in a non-polar solvent dichloromethane; the molar ratio of the monomer to the cross-linking agent is 8:1, and the molar ratio of the monomer to the free radical inhibitor is 28:1.

[0065] S2, placing the precursor solution in step S2 in a centrifuge, centrifuging at 400 rpm for 5 min, and taking the supernatant for later use.

[0066] S3, dissolving the benzil photoinitiator in the supernatant in step S2 by ultrasonication, and letting it stand for 11 hours; the molar ratio of the monomer to the photoinitiator is 23:1.

[0067] S4, drop the precursor solution obtained in step S3 onto a transparent substrate quartz plate, then fix the substrate on the sample stage, use a 60x oil objective to focus the near-infrared femtosecond laser, the radius of the laser spot after focusing is 350nm, and adjust the focal position to the substrate.

[0068] S5, program and control the galvanometer to achieve arbitrary 2D scanning, the femtosecond laser scanning speed is 10-200μm / s, the laser power is 20-50mW, the line spacing is at least 1000nm, the direct writing structure is a separated single line structure, and the single line structure aspect ratio is 10:1.

[0069] S6, after processing, the substrate is placed in propylene glycol methyl ether acetate for development for 10 minutes, and then rinsed in isopropyl alcohol and methyl nonafluorobutyl ether solvents for 1 minute in turn to prevent structural damage caused by surface tension.

[0070] Example 4

[0071] Compared with Example 1, the ratio of the single-line structure in Example 4 is 10:1, and the rest of the contents are the same.

[0072] Example 5

[0073] Compared with Example 1, Example 5 uses a 60x oil objective, and the radius of the focused spot is 350nm. The rest of the contents are the same.

[0074] Example 6 Three-dimensional anisotropic assembly of liquid crystal monomer molecules

[0075] The specific steps of the high degree of freedom liquid crystal molecule assembly method based on laser direct writing in this embodiment are as follows:

[0076] S1, take 4-cyanophenyl 4'-(6-acryloyloxyhexyloxy)benzoate reactive liquid crystal monomer, free radical inhibitor dibutyl hydroxytoluene, crosslinking agent 2,2'-(1,2-ethylenedioxy)bisethanethiol, tetrakis(3-mercaptopropionic acid) pentaerythritol ester, 1,3,5-triallyl-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, heat in a water bath at 100°C and dissolve in a non-polar solvent m-dichlorobenzene; the molar ratio of the liquid crystal monomer to the crosslinking agent is 5:1, and the molar ratio of 2,2'-(1,2-ethylenedioxy)bisethanethiol:tetrakis(3-mercaptopropionic acid) pentaerythritol ester:1,3,5-triallyl-1,3,5-triazine-2,4,6(1H,3H,5H)-trione in the crosslinking agent is 2.5:2.5:1.

[0077] S2, placing the precursor solution in step S1 in a centrifuge and centrifuging at 300 rpm for 3 minutes, and taking the supernatant for later use.

[0078] S3, dissolving 2,4,6-trimethylbenzoyldiphenoxyphosphine free radical photoinitiator in the supernatant in step S2 by ultrasonication, and letting it stand for 12 hours.

[0079] S4, drop the precursor solution obtained in step S3 onto the transparent substrate soda-lime glass, then fix the substrate on the sample stage, use a 60x oil objective to focus the near-infrared femtosecond laser, the radius of the laser spot after focusing is 350nm, and adjust the focus position to the substrate.

[0080] S5, programs the path of the piezoelectric translation stage to achieve arbitrary 3D scanning, the femtosecond laser scanning speed is 10-200μm / s, the laser power is 20-50mW, the line spacing is 700nm, the direct writing structure is a three-dimensional curved structure, and the structural aspect ratio is 5:1.

[0081] S6, after processing, the substrate was placed in propylene glycol methyl ether acetate for 3 minutes, then rinsed with ethanol for 1 minute, and immediately dried in a CO2 supercritical dryer at a pressure of 1072 psi and a sample chamber temperature of 33°C for 4 minutes to prevent structural damage caused by surface tension. The results are shown in Figure 5 and Figure 6 .

[0082] Figure 5 In the figure a, the spiral structure of three-dimensional assembly is shown. Similar to the two-dimensional assembly, the liquid crystal molecules are assembled in order along the scanning path. Here, they are assembled along the spiral line. Figure 5 In the figure bd, the anisotropy is shown. Under normal polarization conditions, both the top and bottom sides of the liquid crystal spiral structure show birefringence. Figure 5 As shown in c, when the polarizer is parallel to the top edge, only the bottom edge shows birefringence. Conversely, when the polarizer is parallel to the bottom edge, only the top edge shows birefringence. Figure 5 This proves that the liquid crystal molecules in the spiral structure are oriented along the three-dimensional spiral direction, which means that this technology can achieve high-degree-of-freedom three-dimensional assembly of liquid crystal molecules in any direction.

[0083] Figure 6 Figure a is the SEM image of the sample under supercritical drying conditions, and figure b is the SEM image of the sample under ordinary drying conditions (Comparative Example 5). In figure b, the three-dimensional structure collapses due to the influence of surface tension.

[0084] With reference to the two-dimensional or three-dimensional assembly method of the embodiment of the present invention, corresponding anisotropic structures can also be obtained by replacing other types of monomer materials.

[0085] For example, acrylic acid ester monomer molecules such as 2-hydroxyethyl acrylate and pentaerythritol triacrylate; hydrogel monomer molecules such as polyethylene glycol diacrylate; acrylamide and other monomer molecules such as N-isopropylacrylamide; SU8 type epoxy resins, etc. can all be used for laser direct writing materials. Figure 7 Schematic diagram of anisotropic assembly of hydrogel molecules. Figure 8POM image of anisotropically assembled acrylate resin molecules. Anisotropic structures can be obtained simply by replacing the monomer material.

[0086] Comparative Example 1

[0087] Comparative Example 1 Compared with Example 1, a larger laser spot is used, and the rest of the contents are the same. Specifically, a 10x mirror (NA=0.3) is used to focus the near-infrared femtosecond laser, and the radius of the laser spot after focusing is 1580nm. The results are shown in Table 1.

[0088] Table 1 Order degree under different laser focal spot sizes

[0089] Order Assembly effect Example 5 0.7 good Example 1 0.4 generally Comparative Example 1 0.1 Difference

[0090] It can be seen from Table 1 that due to the excessive size of the laser focal spot, the anisotropic effect is deteriorated and the degree of order is reduced to S=0.1.

[0091] Comparative Example 2

[0092] Comparative Example 1 Compared with Example 1, the line spacing of the structure is less than 700nm, specifically 300nm, and the rest of the contents are the same. The results are shown in Figure 3 .

[0093] Figure 3 In the figure, a and c are SEM and POM images of separated single-line structures (Example 1), and b and d are SEM and POM images of continuous single-line structures (Comparative Example 2). Figure 3 It can be seen that due to the small line spacing, the single-line structure is connected, resulting in the disappearance of the anisotropic effect and becoming an isotropic structure. The single-line structure with sufficient line spacing (i.e., separated single-line structure) can be seen as anisotropic from the POM image, while the single-line structure with too small line spacing (i.e., continuous single-line structure) can be seen as isotropic from the POM image.

[0094] Comparative Example 3

[0095] Comparative Example 3 Compared with Example 1, the ratio of the single-line structure is 3:1, and the rest is the same. Figure 4 .

[0096] Figure 4 Figure a is a POM image of a single wire structure with different aspect ratios, and b and c are SEM images of a single wire structure with different aspect ratios. The single wire structure with an aspect ratio greater than 5:1 is anisotropic, while the single wire structure with an aspect ratio less than 5:1 is isotropic.

[0097] Comparative Example 4

[0098] Comparative Example 4 Compared with Example 1, the precursor solution lacks a free radical inhibitor, and the rest of the contents are the same. The results are shown in Fig. 9 .

[0099] Fig. 9 As shown, the free radical inhibitor affects the stability and size line width of the precursor solution system. The precursor solution lacking the free radical inhibitor has poor stability. After being placed for 30 days, the precursor solution undergoes solidification caused by a free radical dark reaction. At the same length, the line width of Example 1 is 129.6nm, and the line width of Comparative Example 4 is 290.4nm. It can be seen that the free radical inhibitor does have the technical effect of reducing the line width.

[0100] Comparative Example 5

[0101] Compared with Example 6, in Comparative Example 5, pentaerythritol triacrylate is selected as the crosslinking agent, and the rest of the contents are the same.

[0102] The results show that when pentaerythritol triacrylate (PETA) acrylate material is used as a cross-linking agent, the required direct writing speed becomes slower, specifically 1-20μm / s, and the laser power is 30-40mW; secondly, the mechanical properties are also weaker, and the structure still collapses after using supercritical drying with carbon dioxide.

[0103] Comparative Example 6

[0104] Comparative Example 6 Compared with Example 6, the drying process does not use a CO2 supercritical dryer for drying. After being taken out, it is dried naturally or the methyl nonafluorobutyl ether solvent used in the two-dimensional assembly is used. The results are shown in Figure 6 .

[0105] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for assembling liquid crystal molecules with high degree of freedom based on laser direct writing, characterized in that: The following steps are involved: S1, drop a liquid crystal precursor solution on a substrate, focus a femtosecond laser, the focus spot radius is ≤600nm, and a femtosecond laser direct writing technique is used to construct a separate two-dimensional or three-dimensional scanning path so that the liquid crystal molecules are assembled in order according to the scanning path, the aspect ratio of the polymerized structure is ≥5:1, and the line spacing of the direct writing structure is greater than the focus spot radius; S2, after the assembly is completed, the uncured precursor on the substrate is removed by development. For the three-dimensional polymer structure, the substrate needs to be placed in a CO2 supercritical dryer for drying to obtain a liquid crystal molecule assembly with a high degree of freedom.

2. A method for assembling liquid crystal molecules with high degree of freedom based on laser direct writing as claimed in claim 1, characterized in that: The focus spot radius is 350-600nm, and the direct writing structure line spacing is ≥700nm.

3. A method for assembling liquid crystal molecules with high degree of freedom based on laser direct writing as claimed in claim 1, characterized in that: During the CO2 supercritical drying in step S2, the pressure is ≥1072psi, the sample chamber temperature is 33°C to 39°C, and the drying time is 4 to 10 minutes.

4. A method for assembling liquid crystal molecules with high degree of freedom based on laser direct writing as claimed in claim 1, characterized in that: The liquid crystal precursor solution includes liquid crystal monomers, a cross-linking agent, a free radical inhibitor and a photoinitiator; The liquid crystal monomer is one or more of 4-cyanophenyl 4'-(6-acryloyloxyhexyloxy)benzoate, 1,4-bis-[4-(3-acryloyloxypropoxy)benzoyloxy]-2-methylbenzene, and 1,4-bis-[4-(6-acryloyloxyhexyloxy)benzoyloxy]-2-methylbenzene; The crosslinking agent is a thiol or a multifunctional vinyl compound, selected from one or more of 2,2'-(1,2-ethylenedioxy)bis(ethanediol), pentaerythritol tetrakis(3-mercaptopropionic acid) ester, and 1,3,5-triallyl-1,3,5-triazine-2,4,6(1H,3H,5H)-trione; The free radical inhibitor is one or more of butylated hydroxytoluene, hydroquinone monomethyl ether, and p-tert-butyl pyrocatechol; The photoinitiator is one or more of 2,4,6-trimethylbenzoyldiphenoxyphosphine, benzil and azobisisobutyronitrile.

5. A method for assembling liquid crystal molecules with high degree of freedom based on laser direct writing as claimed in claim 4, characterized in that: The molar ratio of the liquid crystal monomer to the cross-linking agent is 5 to 8:1, the molar ratio of the liquid crystal monomer to the free radical inhibitor is 25 to 30:1, and the molar ratio of the liquid crystal monomer to the photoinitiator is 20 to 25:

1.

6. A method for assembling liquid crystal molecules with high degree of freedom based on laser direct writing as claimed in claim 4, characterized in that: The preparation method of the liquid crystal precursor solution is as follows: adding liquid crystal monomers, crosslinking agents, and free radical inhibitors into a non-polar organic solvent, heating to 70°C to 100°C to dissolve them, cooling after dissolution, and centrifuging to obtain a supernatant; then ultrasonically dissolving a photoinitiator in the supernatant, and standing for 10 to 12 hours to obtain a liquid crystal precursor solution.

7. A method for assembling liquid crystal molecules with high degree of freedom based on laser direct writing as claimed in claim 6, characterized in that: The non-polar organic solvent is one or more of m-dichlorobenzene, toluene, benzene, cyclohexane and dichloromethane.

8. A method for assembling liquid crystal molecules with high degree of freedom based on laser direct writing as claimed in claim 1, characterized in that: The substrate is selected from one of soda lime glass, quartz plate, ITO glass and silicon plate.

9. A method for assembling liquid crystal molecules with high degree of freedom based on laser direct writing as claimed in claim 1, characterized in that: After assembly, the two-dimensional polymer structure is placed in propylene glycol methyl ether acetate for development for 3 to 10 minutes, and then rinsed in isopropanol and methyl nonafluorobutyl ether solvents for 1 to 3 minutes respectively; for the three-dimensional polymer structure, it needs to be placed in ethanol for cleaning after development, and then subjected to CO2 supercritical drying.

10. The method for assembling liquid crystal molecules with high degree of freedom based on laser direct writing according to claim 1, characterized in that: The femtosecond laser scanning speed is 10-200 μm / s, and the laser power is 20-50 mW.

Citation Information

Patent Citations

  • Liquid crystal device, production method and imaging polarization detection system

    CN106249458A

  • Cholesteric liquid crystal device, preparation method and light beam control system

    CN107193160A

  • Composite photoresist for preparing multi-material three-dimensional micro-nano structure and application of composite photoresist

    CN113064325A

  • Preparation method of metal and metal compound three-dimensional micro-nano structure

    CN115555578A

  • Method for orientation of liquid crystals in micro / nano region on basis of laser direct writing and system thereof

    US20160291414A1