Copper indium sulfur thin film solar cell and preparation method thereof

By designing multiple titanium dioxide nanorods and stacked structures in copper indium sulfur thin-film solar cells and embedding copper indium sulfur layer, the problem of short carrier diffusion length is solved, the photoelectric conversion efficiency is improved, and the process is simplified, achieving high efficiency is achieved , low-cost solar cell preparation.

CN118610290BActive Publication Date: 2024-11-12HEFEI INSTITUTE OF PHYSICAL SCIENCE CHINESE ACADEMY OF SCIENCES
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202411081772.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-12
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

Traditional copper indium sulfur thin-film solar cells have the problem of short effective carrier diffusion length, resulting in low photoelectric conversion efficiency, complex preparation process and high cost.

Method used

The design of a copper indium sulfur thin-film solar cell is adopted, which includes multiple titanium dioxide nanorods and stacked structures. The titanium dioxide nanorods extend in a direction away from the first electrode. The stacked structure consists of a cadmium sulfide layer and a copper indium sulfur layer. The indium sulfur layer is embedded in the space between the titanium dioxide nanorods, and the titanium dioxide nanorod, a cadmium sulfide layer and a copper indium sulfur layer are prepared by hydrothermal reaction and solution method.

Benefits of technology

The photoelectric conversion efficiency of copper indium sulfur thin-film solar cells has been significantly improved, reaching more than 10%, which is higher than that of traditional technology, and the preparation process is simplified and costs are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118610290B_ABST
    Figure CN118610290B_ABST
Patent Text Reader

Abstract

The present disclosure provides a copper indium sulfur thin film solar cell and a preparation method thereof. The copper indium sulfur thin film solar cell comprises a first electrode, a titanium dioxide nanorod, a laminated structure and a second electrode, wherein the titanium dioxide nanorod and the laminated structure are arranged between the first electrode and the second electrode. The titanium dioxide nanorod is arranged on the first electrode and its axial direction extends in a direction away from the first electrode; the laminated structure comprises a stacked cadmium sulfide layer and a copper indium sulfur layer, wherein the cadmium sulfide layer covers the titanium dioxide nanorod, and the copper indium sulfur layer is arranged on a side of the cadmium sulfide layer away from the titanium dioxide nanorod. The structural design enables the device to have a higher photon absorption capacity and charge collection efficiency, thereby significantly improving the conversion efficiency of the copper indium sulfur thin film solar cell and having good stability. The preparation method of the copper indium sulfur thin film solar cell is simple, has low requirements on equipment, can be prepared on a large area at a lower temperature, and has great practical application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solar cells, and in particular to a copper indium sulfur thin film solar cell and a preparation method thereof. Background Art

[0002] Solar cells need to meet two basic requirements of high efficiency and high stability in actual use. Inorganic semiconductor materials have the advantages of high carrier mobility and good structural stability. Currently, the most common solar cells are mainly crystalline silicon solar cells, which have the advantage of high energy conversion efficiency. However, the preparation process of crystalline silicon solar cells requires high-purity single crystal silicon, and the cost of raw materials is relatively high. In addition, the preparation process of crystalline silicon solar cells also needs to be carried out under high vacuum and high crystallization temperature, and the preparation process is relatively complicated. Therefore, it is necessary to explore more potential solar cell systems.

[0003] Copper indium sulfide (CuInS2) is a direct bandgap semiconductor material with a bandgap of only 1.50 eV and an absorption coefficient of 10 4 cm -1 The above, and also has excellent thermal stability, is a potential solar cell light absorption material. The actual conversion efficiency that can be achieved by traditional solar cells based on copper indium sulphide materials is often only about 6%, which has the problem of significantly low conversion efficiency. Summary of the invention

[0004] Based on this, in view of the technical problems in the above-mentioned background technology, it is necessary to provide a copper indium sulfur thin film solar cell based on copper indium sulfur, which has a significantly higher photoelectric conversion efficiency.

[0005] According to some embodiments of the present disclosure, a copper indium sulfur thin film solar cell is provided, which includes a first electrode, titanium dioxide nanorods, a stacked structure and a second electrode, wherein the titanium dioxide nanorods and the stacked structure are arranged between the first electrode and the second electrode;

[0006] The copper indium sulfide thin film solar cell includes a plurality of titanium dioxide nanorods arranged at intervals, wherein the titanium dioxide nanorods are arranged on the first electrode and their axial directions extend in a direction away from the first electrode; the laminated structure includes a stacked cadmium sulfide layer and a copper indium sulfide layer, wherein the cadmium sulfide layer covers the titanium dioxide nanorods, and the copper indium sulfide layer is arranged on a side of the cadmium sulfide layer away from the titanium dioxide nanorods.

[0007] In some embodiments of the present disclosure, the number density of the titanium dioxide nanorods is 80 / μm 2 ~120 / μm 2 .

[0008] In some embodiments of the present disclosure, the copper indium sulfur thin film solar cell further includes a titanium dioxide base film, the titanium dioxide base film is stacked on the first electrode, and the titanium dioxide nanorods are arranged on a side of the titanium dioxide base film away from the first electrode.

[0009] In some embodiments of the present disclosure, the height of the titanium dioxide nanorods is 500nm~1200nm.

[0010] In some embodiments of the present disclosure, the diameter of the titanium dioxide nanorods is 20 nm to 100 nm.

[0011] In some embodiments of the present disclosure, the thickness of the cadmium sulfide layer is 10 nm to 30 nm.

[0012] In some embodiments of the present disclosure, a hole transport layer is further included, and the hole transport layer is stacked between the stacked structure and the second electrode.

[0013] In another aspect, the present disclosure further provides a method for preparing a copper indium sulfur thin film solar cell as described in any of the above embodiments, comprising the following steps:

[0014] providing a substrate including a first electrode;

[0015] Preparing a titanium dioxide-based film on the first electrode;

[0016] Growing the titanium dioxide nanorods based on the titanium dioxide base film;

[0017] sequentially depositing the cadmium sulfide layer and the copper indium sulfide layer on the titanium dioxide nanorods to form the stacked structure; and,

[0018] The second electrode is prepared on a side of the stacked structure away from the first electrode.

[0019] In some embodiments of the present disclosure, the titanium dioxide nanorods are grown by hydrothermal reaction, and the steps of growing the titanium dioxide nanorods include:

[0020] The substrate prepared with the titanium dioxide-based film is placed in a hydrothermal container, and hydrothermal reactants are added into the hydrothermal container to carry out a hydrothermal reaction, wherein the hydrothermal reactants include water, hydrochloric acid and isopropyl titanate; the reaction temperature during the hydrothermal reaction is controlled to be 150°C to 200°C, and the reaction time is 1h to 5h.

[0021] In some embodiments of the present disclosure, the step of depositing the cadmium sulfide layer includes:

[0022] The titanium dioxide nanorods are immersed in a first precursor solution containing cadmium ions and alkaline solution, and thiourea is added to perform a first heating reaction to form the cadmium sulfide layer. The reaction temperature during the first heating reaction is controlled to be 40° C. to 60° C., and the reaction time is 5 min to 15 min.

[0023] In some embodiments of the present disclosure, the step of depositing the copper indium sulfide layer includes:

[0024] Spin coating a second precursor solution on the cadmium sulfide layer, and performing a second heating reaction in a protective gas atmosphere to deposit a copper indium sulfide material on the surface of the cadmium sulfide layer, wherein the second heating reaction comprises: first heating at a temperature of 120° C. to 180° C. for 4 min to 6 min, and then heating at a temperature of 200° C. to 300° C. for 5 min to 15 min;

[0025] The second precursor solution includes indium ions, copper ions and thiourea, and the molar ratio of the indium ions, copper ions and thiourea is 1:(1.1-1.9):(6-10).

[0026] In some embodiments of the present disclosure, the step of depositing the copper indium sulfide layer also includes: after depositing the copper indium sulfide material, placing the substrate and thiourea in a heating chamber, and controlling the temperature in the heating chamber to 120° C.~200° C. to perform a sulfurization treatment on the deposited copper indium sulfide material.

[0027] Traditional copper indium sulfur thin film solar cells are flat-plate cells. For example, a copper indium sulfur thin film cell is provided with a stacked titanium dioxide layer, a cadmium sulfide layer and a copper indium sulfur layer. The flat-plate copper indium sulfur thin film cell has the advantages of a relatively simple structure and preparation process, but has the disadvantage of a short effective diffusion length of carriers, which seriously restricts the photoelectric conversion efficiency of the thin film solar cell.

[0028] The copper indium sulfur thin film solar cell in at least one embodiment of the present disclosure includes a first electrode, a plurality of titanium dioxide nanorods, a laminated structure, and a second electrode. The titanium dioxide nanorods extend in a direction away from the first electrode, and the cadmium sulfide layer and the copper indium sulfur layer in the laminated structure are stacked on the titanium dioxide nanorods. Among them, the composite structure composed of titanium dioxide and cadmium sulfide can be used to transmit electrons, and the copper indium sulfur layer is used as the main light absorption material. The titanium dioxide nanorods, the cadmium sulfide layer and the copper indium sulfur layer form a heterojunction. The copper indium sulfur thin film solar cell is provided with more titanium dioxide nanorods and cadmium sulfide layers in the space in the thickness direction, and the copper indium sulfur layer is embedded in the space between the titanium dioxide nanorods accordingly. This structural design can effectively overcome the problem of short effective diffusion length of carriers existing in traditional technologies, so that the device has higher photon absorption capacity and charge collection efficiency, thereby significantly improving the conversion efficiency of the copper indium sulfur thin film solar cell. After experimental verification, the conversion efficiency of the copper indium sulfur thin film solar cell can reach more than 10%, which is significantly higher than the conversion efficiency of the currently known copper indium sulfur-based thin film solar cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a schematic diagram of the cross-sectional structure of a copper indium sulfur thin film solar cell;

[0030] Figure 2 The figure is a schematic diagram of the steps of the preparation method of copper indium sulfur thin film solar cells;

[0031] Figure 3 This is a result diagram of an X-ray diffraction test on the substrate after the titanium dioxide nanorod array is prepared in Example 1;

[0032] Figure 4 This is an image characterized by scanning electron microscopy of the substrate after the titanium dioxide nanorod arrays are prepared in Example 1;

[0033] Figure 5 This is a result diagram of an X-ray diffraction test on the substrate after the cadmium sulfide layer is prepared in Example 1;

[0034] Figure 6 This is an image characterized by using a scanning electron microscope on the substrate after the cadmium sulfide layer is prepared in Example 1;

[0035] Figure 7 The images and crystal structure diagram of the titanium dioxide nanorods and cadmium sulfide layer in Example 1 characterized by transmission electron microscopy;

[0036] Figure 8 This is a result diagram of an X-ray diffraction test on the substrate after the copper indium sulfide layer is prepared in Example 1;

[0037] Fig. 9This is an image characterized by scanning electron microscopy of the substrate after the copper indium sulfide layer is prepared in Example 1;

[0038] Fig.10 The absorption spectra of the substrate in Example 1 after preparing the titanium dioxide nanorod array, the cadmium sulfide layer, and the copper indium sulfide layer;

[0039] Fig.11 This is a test diagram of the external quantum efficiency of the copper indium sulfur thin film solar cell of Example 1;

[0040] Fig.12 This is the current-voltage relationship curve of the copper indium sulfur thin film solar cell of Example 1 under light illumination;

[0041] Fig.13 The graphs show the photoelectric conversion efficiency of the copper indium sulfur thin film solar cell of Example 1 after being stored in an air environment for 6 months and 12 months respectively.

[0042] The reference numerals and their meanings are as follows:

[0043] 1. Second electrode; 2. Hole transport layer; 3. Copper indium sulfide layer; 4. Cadmium sulfide layer; 5. Titanium dioxide nanorods; 6. Titanium dioxide base film; 7. First electrode; 8. Substrate. DETAILED DESCRIPTION

[0044] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0045] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items, and "more" used herein includes two or more items.

[0046] In the present invention, unless otherwise stated, the sum of the parts of each component in the composition can be 100 parts by weight. Unless otherwise specified, the basis of the percentages (including weight percentages) in the present invention is the total weight of the composition. In addition, "wt%" herein means mass percentage, and "at%" means atomic percentage.

[0047] In this article, unless otherwise stated, each reaction step may be carried out in the order described herein or may not be carried out in the order described herein. For example, other steps may be included between each reaction step, and the order of the reaction steps may also be appropriately swapped. This can be determined by the technician based on common knowledge and experience. Preferably, the reaction method herein is carried out sequentially.

[0048] The present disclosure provides a copper indium sulfur thin film solar cell, which includes a first electrode, titanium dioxide nanorods, a laminated structure and a second electrode, wherein the titanium dioxide nanorods and the laminated structure are arranged between the first electrode and the second electrode. The copper indium sulfur thin film solar cell includes a plurality of titanium dioxide nanorods arranged at intervals, wherein the titanium dioxide nanorods are arranged on the first electrode and their axial directions extend in a direction away from the first electrode; the laminated structure includes a stacked cadmium sulfide layer and a copper indium sulfur layer, wherein the cadmium sulfide layer covers the titanium dioxide nanorods, and the copper indium sulfur layer is arranged on a side of the cadmium sulfide layer away from the titanium dioxide nanorods.

[0049] The copper indium sulfur thin film solar cell disclosed in the present invention includes a first electrode, a plurality of titanium dioxide nanorods, a laminated structure and a second electrode. The titanium dioxide nanorods extend in a direction away from the first electrode, and the cadmium sulfide layer and the copper indium sulfur layer in the laminated structure are stacked on the titanium dioxide nanorods. Among them, the composite structure composed of titanium dioxide and cadmium sulfide can be used to transmit electrons, and the copper indium sulfur layer is used as the main light absorption material. The titanium dioxide nanorods, the cadmium sulfide layer and the copper indium sulfur layer form a heterojunction. The copper indium sulfur thin film solar cell is provided with more titanium dioxide nanorods and cadmium sulfide layers in the space in the thickness direction, and the copper indium sulfur layer is embedded in the space between the titanium dioxide nanorods accordingly. This structural design can effectively overcome the problem of short effective diffusion length of carriers existing in traditional technologies, so that the device has higher photon absorption capacity and charge collection efficiency, thereby significantly improving the conversion efficiency of the copper indium sulfur thin film solar cell. After experimental verification, the conversion efficiency of the copper indium sulfur thin film solar cell can reach more than 10%, which is significantly higher than the conversion efficiency of the currently known copper indium sulfur-based thin film solar cells.

[0050] Figure 1 This is a schematic diagram of the cross-sectional structure of a copper indium sulfur thin film solar cell provided by the present disclosure. Figure 1 As shown, the copper indium sulfur thin film solar cell includes a first electrode 7, titanium dioxide nanorods 5, a laminated structure and a second electrode 1. The copper indium sulfur thin film solar cell includes a plurality of titanium dioxide nanorods 5 arranged at intervals, the titanium dioxide nanorods 5 are arranged on the first electrode 7 and their axial direction extends in a direction away from the first electrode 7; the laminated structure includes a stacked cadmium sulfide layer 4 and a copper indium sulfur layer 3, the cadmium sulfide layer 4 covers the titanium dioxide nanorods 5, and the copper indium sulfur layer 3 is arranged on the side of the cadmium sulfide layer 4 away from the titanium dioxide nanorods 5. Figure 1, the first electrode 7 can be arranged on the substrate 8.

[0051] In the above copper indium sulfur thin film solar cell, the titanium dioxide nanorods 5 serve as a carrier template of the laminated structure, the cadmium sulfide layer 4 covers the titanium dioxide nanorods 5, and forms a core-shell structure with the titanium dioxide nanorods 5. The titanium dioxide nanorods 5 can be used as a core material, and the cadmium sulfide layer 4 can be used as a shell material. The two can form a composite electron transport film and are used to transport electrons. The copper indium sulfur layer 3 is located on the side of the cadmium sulfide layer 4 away from the titanium dioxide nanorods 5, and serves as a light absorbing material for absorbing photons and generating electron-hole pairs.

[0052] It can be understood that a plurality of titanium dioxide nanorods 5 can form an array of titanium dioxide nanorods 5. The axial direction of the titanium dioxide nanorods 5 can extend in a direction away from the first electrode 7, that is, there is a height difference between the top and bottom ends of the titanium dioxide nanorods 5. The "direction away from the first electrode 7" can be perpendicular to the surface of the first electrode 7, or obliquely intersecting the surface of the first electrode 7, which is not particularly limited here. Figure 1 Although the axial direction of the titanium dioxide nanorods 5 is shown to be perpendicular to the surface of the first electrode 7 , the axial direction of the titanium dioxide nanorods 5 may also be arranged to be inclined with respect to the surface of the first electrode 7 , which is related to the actual preparation process.

[0053] In this embodiment, the gaps between the titanium dioxide nanorods 5 are used as the arrangement area of ​​the stacked structure. As some examples of this embodiment, the number density of the titanium dioxide nanorods 5 is 80 / μm. 2 ~120 / μm 2 Here, “number density” refers to the unit area (here in μm 2 The number density of titanium dioxide nanorods 5 can be observed and statistically obtained under an electron microscope. By controlling the number density of titanium dioxide nanorods 5 within the above range, sufficient space can be left between the titanium dioxide nanorods 5 to facilitate the coating of the stacked structure, while preventing the thickness of the stacked structure from being too high, which is not conducive to the effective diffusion of carriers.

[0054] In this example, the number density of the titanium dioxide nanorods 5 may be 80 / μm 2 , 90 / μm 2 , 100 / μm 2 , 110 / μm 2 , 120 / μm 2 Alternatively, the number density of titanium dioxide nanorods 5 may also be between any two of the above number densities.

[0055] As some examples of this embodiment, the copper indium sulfur thin film solar cell may also include a titanium dioxide base film 6, which is stacked on the first electrode 7, and the titanium dioxide nanorods 5 are arranged on the side of the titanium dioxide base film 6 away from the first electrode 7. Further, the titanium dioxide nanorods 5 can be grown based on the titanium dioxide base film 6. The provision of the titanium dioxide base film 6 can, on the one hand, make the titanium dioxide nanorods 5 more firmly combined, and on the other hand, it is also helpful to achieve the control of the number density of the titanium dioxide nanorods 5, so as to obtain titanium dioxide nanorods 5 with relatively sparse distribution, and on the other hand, it is also helpful to collect the carriers on the titanium dioxide nanorods 5 and conduct them to the first electrode 7.

[0056] As some examples of this embodiment, the titanium dioxide base film 6 may be a dense titanium dioxide thin film.

[0057] As some examples of this embodiment, the thickness of the titanium dioxide base film 6 is 50 nm to 150 nm. Controlling the thickness of the titanium dioxide base film 6 to 50 nm to 150 nm can provide a better ability to collect carriers.

[0058] In this example, the thickness of the titanium dioxide base film 6 can be 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, or the thickness of the titanium dioxide base film 6 can be between any two of the above thicknesses.

[0059] As some examples of this embodiment, the height of the titanium dioxide nanorod 5 is 500nm~1200nm. Among them, the height of the titanium dioxide nanorod 5 refers to the distance between the top of the titanium dioxide and its bottom in the direction perpendicular to the surface of the first electrode 7. It can be understood that the higher the height of the titanium dioxide nanorod 5, the larger the area of ​​the laminated structure that can be attached to a single titanium dioxide nanorod 5. Setting the height of the titanium dioxide nanorod 5 to 500nm~1200nm is conducive to increasing the surface area of ​​the laminated structure while ensuring sufficient attachment of the laminated structure, so that the copper indium sulfur thin film solar cell has a higher photoelectric conversion efficiency.

[0060] In this example, the height of the titanium dioxide nanorods 5 may be 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1000 nm, 1100 nm, or 1200 nm, or the height of the titanium dioxide nanorods 5 may be between any two of the above thicknesses.

[0061] As some examples of this embodiment, the diameter of the titanium dioxide nanorod 5 is 20 nm to 100 nm. Setting the diameter of the titanium dioxide nanorod 5 to 20 nm to 100 nm is conducive to ensuring the structural stability of the titanium dioxide nanorod 5.

[0062] In this example, the diameter of the titanium dioxide nanorods 5 may be 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, or 100 nm, or the diameter of the titanium dioxide nanorods 5 may be between any two of the above diameter ranges.

[0063] As some examples of this embodiment, the thickness of the cadmium sulfide layer 4 may be 20 nm to 30 nm. Setting the thickness of the cadmium sulfide layer 4 to 20 nm to 30 nm can provide a larger arrangement space for the copper indium sulfide layer 3 while ensuring good quality of the stacked structure.

[0064] In this example, the thickness of the cadmium sulfide layer 4 may be 20 nm, 21 nm, 22 nm, 23 nm, 24 nm, 25 nm, 26 nm, 27 nm, 28 nm, 29 nm, or 30 nm, or the thickness of the cadmium sulfide layer 4 may be between any two of the above thickness ranges.

[0065] As some examples of this embodiment, the copper indium sulfide layer 3 in the stacked structure may also be extended to a side of the titanium dioxide nanorod 5 away from the first electrode 7 , that is, above the top of the titanium dioxide nanorod 5 .

[0066] Reference Figure 1 As shown in some examples of this embodiment, the copper indium sulfur thin film solar cell further includes a hole transport layer 2, and the hole transport layer 2 is stacked between the stacked structure and the second electrode 1. The hole transport layer 2 is used to conduct carriers generated by the stacked structure.

[0067] In this example, the material of the hole transport layer 2 may include Spiro-OMeTAD.

[0068] In this example, the thickness of the hole transport layer 2 is 80 nm to 200 nm. Further, the thickness of the hole transport layer 2 can be 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, 130 nm, 150 nm, 180 nm, 200 nm, or the thickness of the hole transport layer 2 can also be between any two of the above thickness ranges.

[0069] As some examples of this embodiment, the material of the first electrode 7 is a conductive material, for example, the material of the first electrode 7 can be selected from one or more of transparent conductive metal oxides and metals. In this embodiment, the material of the first electrode 7 is a transparent conductive metal oxide.

[0070] As some examples of this embodiment, the material of the second electrode 1 is a conductive material, for example, the material of the second electrode 1 can be selected from one or more of transparent conductive metal oxides and metals. In this embodiment, the material of the second electrode 1 is metal.

[0071] As some examples of this embodiment, the thickness of the second electrode 1 may be 100 nm to 500 nm. For example, the thickness of the second electrode 1 may be 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, or the thickness of the second electrode 1 may be between any two of the above thicknesses.

[0072] Furthermore, the present disclosure also provides a method for preparing a copper indium sulfur thin film solar cell. Figure 2 is a schematic diagram of the steps of the preparation method, referring to Figure 2 As shown, the preparation method includes the following steps S1 to S5.

[0073] Step S1, providing a substrate including a first electrode.

[0074] As some examples of this embodiment, the material of the first electrode may be selected from a conductive material, for example, the material of the first electrode may be selected from one or more of a metal or a transparent conductive metal oxide.

[0075] As some specific examples of this embodiment, conductive glass can be used as a substrate and a first electrode. The conductive glass includes a glass substrate and a transparent conductive metal oxide located on the glass substrate, wherein the glass substrate serves as a substrate and the transparent conductive metal oxide serves as a first electrode.

[0076] As some examples of this embodiment, the step of cleaning the substrate is also included. The method of cleaning the substrate may include ultrasonic cleaning. In this example, acetone, isopropanol and ultrapure water may be used to ultrasonically clean the substrate in sequence, and the time of each ultrasonic cleaning may be controlled to be 3 minutes to 10 minutes.

[0077] Step S2, preparing a titanium dioxide-based film on the first electrode.

[0078] In this embodiment, the method of preparing the titanium dioxide-based film may include but is not limited to physical vapor deposition, chemical vapor deposition and solution film formation.

[0079] As some examples of this embodiment, the step of preparing a titanium dioxide-based film on the first electrode includes: spin coating a titanium dioxide precursor sol on the first electrode to form a sol film, and sintering the sol film to form a titanium dioxide-based film.

[0080] In this example, the titanium dioxide precursor sol includes anhydrous ethanol, alkyl titanate and glacial acetic acid. The volume ratio of anhydrous ethanol, alkyl titanate and glacial acetic acid can be (2-5):1:(0.05-0.2). Among them, the alkyl titanate can be n-butyl titanate.

[0081] In this example, during the sintering process of the sol film, the sintering temperature can be controlled to be 500° C. to 600° C., and the sintering time can be controlled to be 10 min to 60 min.

[0082] In step S2, a dense titanium dioxide film can be formed by spin coating the sol and sintering the film, which is beneficial for controlling the growth density of titanium dioxide nanorods in subsequent processes.

[0083] Step S3, growing titanium dioxide nanorods based on the titanium dioxide base film.

[0084] As some examples of this embodiment, the method of growing titanium dioxide nanorods is a hydrothermal reaction.

[0085] As a further example of this embodiment, the step of growing titanium dioxide nanorods includes: placing a substrate prepared with a titanium dioxide base film in a hydrothermal container, and adding hydrothermal reactants into the hydrothermal container to perform a hydrothermal reaction, wherein the hydrothermal reactants include water, hydrochloric acid, and alkyl titanate. The alkyl titanate may be isopropyl titanate.

[0086] In this example, the hydrothermal reactants can be configured in the following proportions: concentrated hydrochloric acid and water are mixed in a volume ratio of 1:1, and alkyl titanate is added, wherein the volume ratio between the mixture of concentrated hydrochloric acid and water and the alkyl titanate can be (20~80):(0.5~1.5).

[0087] In this example, the reaction temperature during the hydrothermal reaction can be controlled to be 150° C. to 200° C. For example, the reaction temperature can be controlled to be 150° C., 160° C., 170° C., 180° C., 190° C., 200° C., or the reaction temperature can be controlled to be between any two of the above temperatures.

[0088] In this example, the reaction time during the hydrothermal reaction can be controlled to be 1 h to 5 h. For example, the reaction time can be controlled to be 1 h, 2 h, 3 h, 4 h, 5 h, or the reaction time can be controlled to be between any two of the above times.

[0089] By controlling the conditions of the above hydrothermal reaction, a titanium dioxide nanorod array with a relatively suitable number density, height and diameter can be prepared on the titanium dioxide base film.

[0090] Step S4, depositing a cadmium sulfide layer and a copper indium sulfide layer on the titanium dioxide nanorods in sequence to form a stacked structure.

[0091] As some examples of this embodiment, the cadmium sulfide layer can be deposited by a solution method. Further, the step of depositing the cadmium sulfide layer includes: immersing the titanium dioxide nanorods in a first precursor solution containing cadmium ions and alkaline solution, adding thiourea, and performing a first heating reaction to form the cadmium sulfide layer.

[0092] In this example, the first precursor solution can be prepared as follows: add alkali solution to the cadmium sulfate aqueous solution to form the first precursor solution. The mass concentration of cadmium sulfate in the cadmium sulfate aqueous solution can be 0.4 g / L to 0.6 g / L, and the alkali solution can be, but is not limited to, ammonia water. In addition, the mass concentration of the added alkali solution can be 25% to 28%, and the volume ratio of the cadmium sulfate aqueous solution to the ammonia water can be 6.25:1.

[0093] In this example, thiourea can be added by adding a thiourea aqueous solution, wherein the mass concentration of thiourea in the thiourea aqueous solution can be 50 g / L to 60 g / L. Furthermore, the volume ratio of the first precursor solution to the thiourea aqueous solution can be 9:1.

[0094] In this example, the reaction temperature in the first heating reaction process can be controlled to be 40° C. to 60° C. For example, the reaction temperature can be controlled to be 40° C., 42° C., 45° C., 48° C., 50° C., 52° C., 55° C., 58° C., 60° C., or the reaction temperature can be controlled to be between any two of the above temperatures.

[0095] In this example, the reaction time in the first heating reaction process can be controlled to be 5 min to 15 min. For example, the reaction time can be controlled to be 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, or the reaction time can be controlled to be between any two of the above times.

[0096] In the first heating reaction process, the cadmium ions in the first precursor solution react with thiourea to produce cadmium sulfide nanoparticles attached in situ to the titanium dioxide nanorods. As the reaction proceeds, the cadmium sulfide nanoparticles eventually combine to form a cadmium sulfide layer covering the titanium dioxide nanorods. The cadmium sulfide layer and the titanium dioxide nanorods form an array of core-shell structures.

[0097] It is understandable that in the process of preparing the cadmium sulfide layer, if the titanium dioxide nanorods are too dense or the cadmium sulfide generation rate is too fast, it may make it difficult for the cadmium sulfide to evenly cover the titanium dioxide nanorods, thereby affecting the actual structure of the final copper indium sulfur thin film solar cell.

[0098] As some examples of this embodiment, after the cadmium sulfide layer is formed, there are still gaps between the plurality of titanium dioxide nanorods to serve as preparation areas for a subsequent copper indium sulfide layer.

[0099] As some examples of this embodiment, the step of depositing the copper indium sulfide layer includes: spin coating a second precursor solution on the cadmium sulfide layer, and performing a second heating reaction in an atmosphere of a protective gas to deposit a copper indium sulfide material on the surface of the cadmium sulfide layer. It can be understood that during the spin coating of the second precursor solution, the second precursor solution can penetrate into the gaps between the titanium dioxide nanorods to further grow the copper indium sulfide layer on the cadmium sulfide layer.

[0100] In this example, the second precursor solution includes indium ions, copper ions and thiourea, and the ratio of the amount of indium ions, copper ions and thiourea is 1: (1.1-1.9): (6-10). Further, the second precursor solution may include indium chloride (InCl3), cuprous iodide (CuI) and thiourea, indium chloride as an indium ion source, and cuprous iodide as a copper ion source. The solvent in the second precursor solution may be an organic solvent, such as N,N-dimethylformamide, to avoid hydrolysis of indium chloride and cuprous iodide.

[0101] In this example, the second heating reaction process includes: first heating at a temperature of 120°C to 180°C for 4min to 6min, and then heating at a temperature of 200°C to 300°C for 5min to 15min. During the second heating reaction, the solvent in the second precursor solution gradually evaporates, and the indium ions, copper ions, and sulfur elements in thiourea combine to form a copper indium sulfur material.

[0102] It can be understood that by spin-coating the second precursor solution and performing the second heating reaction, the deposition rate of the copper indium sulfide material can be more effectively controlled to form an appropriate and uniform copper indium sulfide material on the cadmium sulfide layer. Further, in this example, the spin-coating of the second precursor solution and the second heating reaction can be performed only once. In other examples, the spin-coating of the second precursor solution and the second heating reaction can also be repeated multiple times to form more copper indium sulfide material.

[0103] As some examples of this embodiment, the step of depositing the copper indium sulfide layer further includes: after depositing the copper indium sulfide material, placing the substrate and thiourea in a heating chamber, controlling the temperature in the heating chamber to be 120° C. to 200° C., so as to perform a sulfurization treatment on the deposited copper indium sulfide material. The sulfurization treatment can passivate the deposited copper indium sulfide material, thereby effectively improving the efficiency of the solar cell.

[0104] In this example, the temperature in the heating chamber can be controlled to be 120° C., 130° C., 140° C., 150° C., 160° C., 170° C., 180° C., 190° C., 200° C., or the temperature in the heating chamber can be controlled to be between any two of the above temperatures. By using thiourea as the vulcanizing raw material, the heating temperature of the vulcanization treatment can be lowered, thereby minimizing the impact of the vulcanization process on the already formed structure.

[0105] Step S5, preparing a second electrode on a side of the stacked structure away from the first electrode.

[0106] As some examples of this embodiment, before preparing the second electrode, a step of preparing a hole transport layer is also included.

[0107] Furthermore, the step of preparing the hole transport layer includes: spin coating a third precursor solution on a side of the stacked structure away from the first electrode, and performing annealing to form the hole transport layer.

[0108] In this example, the third precursor solution includes Spiro-OMeTAD, LiTFSI and TBP, wherein the molar ratio of Spiro-OMeTAD, LiTFSI and TBP is 1:(0.4~0.6):(2~4). Furthermore, the solvent in the third precursor solution can be an organic solvent, such as chlorobenzene. Spiro-OMeTAD is an organic hole transport material, which can effectively avoid the local short circuit problem generated in the subsequent preparation of the second electrode, so that the copper indium sulfur thin film solar cell has a higher open circuit voltage.

[0109] In this example, during the annealing process, the annealing process is performed at a temperature of 50° C. to 150° C. for 5 min to 15 min.

[0110] As some examples of this embodiment, the second electrode may be prepared by deposition, for example, by vacuum evaporation.

[0111] It can be understood that the copper indium sulfur thin film solar cell in the present disclosure can be prepared through the above steps S1 to S5.

[0112] The present disclosure also provides the following embodiments to more specifically illustrate the copper indium sulfur thin film solar cell.

[0113] Example 1

[0114] Provide FTO (fluorine-doped tin dioxide) conductive glass as a substrate and a first electrode, and the FTO layer on the glass surface is used as the first electrode with a thickness of 400 nm. The substrate is ultrasonically cleaned in acetone, isopropanol and ultrapure water for 5 minutes respectively, and then dried for use.

[0115] Anhydrous ethanol, n-butyl titanate, and glacial acetic acid were mixed in a volume ratio of 4:1:0.1 to prepare a colorless titanium dioxide precursor sol. The titanium dioxide precursor sol was spin-coated twice on a substrate, and then placed in a muffle furnace in an air atmosphere, heated to 550°C and maintained for 30 minutes for sintering to form a dense titanium dioxide base film.

[0116] Concentrated hydrochloric acid and deionized water were mixed in a volume ratio of 1:1, and then isopropyl titanate was added and stirred evenly to form a hydrothermal reactant, wherein the volume ratio of the mixed solution of concentrated hydrochloric acid and deionized water to isopropyl titanate was 40:0.7. The front side of the substrate (i.e., the surface with the titanium dioxide base film) was suspended downward in a reactor, and after the hydrothermal reactant was added and sealed, the reaction was carried out at a temperature of 180°C for 2h to form a titanium dioxide nanorod array, and then the substrate was removed and cleaned and dried.

[0117] Prepare a 0.48 g / L cadmium sulfate aqueous solution, add concentrated ammonia water (concentration of 25% to 28%) as the first precursor solution, wherein the volume ratio of the cadmium sulfate aqueous solution to the concentrated ammonia water is 6.25:1. Vertically immerse the substrate in the first precursor solution, stir and add 55 g / L thiourea aqueous solution in a 50°C water bath, the volume ratio of the first precursor solution to the thiourea aqueous solution is 9:1, continue stirring for 15 minutes and then take out to complete the deposition of the cadmium sulfide layer, then wash and dry for use.

[0118] Indium chloride is added to N,N-dimethylformamide, and cuprous iodide and thiourea are added in sequence, and stirred at room temperature for 20 hours to dissolve it to obtain a second precursor solution, in which the amount ratio of indium chloride, cuprous iodide and thiourea is 1:1.5:8. The second precursor solution is spin-coated twice on the substrate, which is placed at a temperature of 65°C and vacuum dried for 15 minutes and then transferred to a heating table, heated to 150°C and maintained for 5 minutes, and then heated to 270°C and maintained for 10 minutes for a second heat treatment. The above process is carried out twice to deposit copper indium sulfur material, and then cooled to room temperature. The substrate after the copper indium sulfur material is deposited is placed in a tubular furnace, and thiourea is used as a sulfur source in a nitrogen environment, and heated to 180°C for low-temperature atmospheric pressure sulfurization to form a copper indium sulfur layer.

[0119] Spiro-OMeTAD was added to chlorobenzene, and then LiTFSI in acetonitrile solution and TBP were added in sequence, and stirred to mix to form a third precursor solution. The third precursor solution was spin-coated onto the substrate and annealed at 100°C in air for 10 minutes to form a hole transport layer with a thickness of about 100 nm. A 100 nm gold film was evaporated on the hole transport layer as the second electrode.

[0120] Example 2

[0121] Example 2 is substantially the same as Example 1, except that: in Example 2, no sulfurization treatment is performed after the copper indium sulfide material is deposited, and the unsulfurized copper indium sulfide material is used as the copper indium sulfide layer.

[0122] Comparative Example 1

[0123] Comparative Example 1 is substantially the same as Example 1, except that: in Comparative Example 1, no titanium dioxide nanorod array is prepared, and the subsequent cadmium sulfide layer and copper indium sulfide layer are directly deposited on the titanium dioxide base film in the form of a planar thin film.

[0124] Comparative Example 2

[0125] Comparative Example 2 is substantially the same as Example 1, except that: in Comparative Example 2, no cadmium sulfide layer is prepared, and the copper indium sulfide layer is directly deposited on the titanium dioxide nanorod array.

[0126] Experiment 1: X-ray diffraction (XRD) test was performed on the substrate after the titanium dioxide nanorod array was prepared in Example 1. The test results can be seen in Figure 3 The substrate after the titanium dioxide nanorod array was prepared in Example 1 was characterized by scanning electron microscopy. The characterization results can be seen in Figure 4 .

[0127] Reference Figure 3 As shown, the XRD test results show that the crystal form of the prepared titanium dioxide base film is anatase phase structure, and the crystal form of the titanium dioxide nanorods is rutile phase structure. Figure 4 As shown, the thickness of the titanium dioxide base film is about 120nm, and the titanium dioxide base film is composed of nanoparticles with a particle size of approximately 10nm~20nm. The titanium dioxide nanorods extend away from the substrate, with an overall height of about 700nm and a diameter of approximately 30nm~50nm, and a number density of about 90 / μm 2 .

[0128] Experiment 2: X-ray diffraction (XRD) test was performed on the substrate after the cadmium sulfide layer was prepared in Example 1. The test results can be seen in Figure 5 The substrate after the cadmium sulfide layer was prepared in Example 1 was characterized by scanning electron microscopy. The characterization results can be seen at Figure 6 The titanium dioxide nanorods and cadmium sulfide layer in Example 1 were characterized by transmission electron microscopy. The characterization results can be seen in Figure 7 .

[0129] Reference Figure 5 As shown, the crystal form of cadmium sulfide is cubic phase, and there is no obvious impurity peak, indicating that the purity of cadmium sulfide is high. Figure 6As shown in the figure, the thickness of the cadmium sulfide layer is about 25nm, and the cadmium sulfide layer is composed of cadmium sulfide particles with a particle size of approximately 3nm~5nm. The surface of the titanium dioxide nanorods appears rough due to being covered by the cadmium sulfide layer, but there are still wide gaps between the titanium dioxide nanorods, indicating that the overall structure of the array is not significantly affected. Figure 7 The left picture at the bottom is a schematic diagram of the crystal structure of the cadmium sulfide layer, which shows that the cadmium sulfide layer has a polycrystalline structure. Figure 7 The right picture at the bottom is a schematic diagram of the crystal structure of titanium dioxide nanorods, which shows that titanium dioxide nanorods grow along the

[001] crystal plane.

[0130] Experiment 3: The substrate after the copper indium sulfide layer was prepared in Example 1 was subjected to a grazing angle X-ray diffraction test. The test results can be seen in Figure 8 The substrate after the copper indium sulfide layer was prepared in Example 1 was characterized by scanning electron microscopy. The characterization results can be seen at Fig. 9 .

[0131] Reference Figure 8 As shown in the figure, in addition to the diffraction peaks of FTO, titanium dioxide and cadmium sulfide, the diffraction results also show the crystal diffraction peaks of copper indium sulfide, and no other impurity peaks are seen, indicating that the copper indium sulfide layer prepared by this method has a high purity. Fig. 9 As shown in the figure, the surface of the copper indium sulfide layer has a scaly structure and fills into the gaps between the titanium dioxide nanorods. The particle size of the copper indium sulfide particles in the copper indium sulfide layer is approximately 10nm~20nm. This shows that the copper indium sulfide layer covers the side of the cadmium sulfide away from the titanium dioxide nanorods.

[0132] Experiment 4: The absorption spectra of the substrate in Example 1 after preparing the titanium dioxide nanorod array, the cadmium sulfide layer, and the copper indium sulfide layer are tested respectively. The test results can be seen in Fig.10 , Fig.10 Curve "1" in the figure represents the absorption spectrum of titanium dioxide nanorod array, curve "2" represents the absorption spectrum of titanium dioxide nanorod array after preparing cadmium sulfide layer, and curve "3" represents the absorption spectrum of titanium dioxide nanorod array after preparing cadmium sulfide layer and copper indium sulfide layer.

[0133] Reference Fig.10 As shown in the figure, the absorption spectrum of the titanium dioxide nanorod array alone is mainly in the ultraviolet band (wavelength < 400nm). After the cadmium sulfide layer is further formed, the absorption spectrum is expanded to the visible light region with a wavelength of < 550nm. The titanium dioxide nanorod array, cadmium sulfide layer and copper indium sulfide layer as a whole have absorption in the larger band of 300nm~900nm.

[0134] Experiment 5: Testing the external quantum efficiency of the copper indium sulfur thin film solar cell of Example 1. The results can be seen in Fig.11 The current-voltage relationship curve of the copper indium sulfur thin film solar cell of Example 1 under light irradiation is shown in Fig.12 The photoelectric conversion efficiency of the copper indium sulfur thin film solar cell of Example 1 after being stored in air for 6 months and 12 months was tested. The results are shown in Fig.13 .

[0135] Reference Fig.11 As shown, the copper indium sulfur thin film solar cell has good photocurrent generation performance in the spectral range of 300nm~900nm.

[0136] Reference Fig.12 As shown, the open circuit voltage (V oc ) can reach 0.81V, the short circuit current (J sc ) can reach 24.24mA / cm 2 , the fill factor (FF) can reach 64.68%, and the photoelectric conversion efficiency can reach 12.68%. The photoelectric conversion efficiency that can be achieved by known copper indium sulfur-based thin-film solar cells is usually only about 6%. The photoelectric conversion efficiency of the solar cell of Example 1 is significantly higher than that of known copper indium sulfur-based thin-film solar cells, indicating that it has a very significant improvement in photoelectric conversion efficiency performance.

[0137] Reference Fig.13 As shown, after the solar cell of Example 1 was stored in an air environment for 6 months, the photoelectric conversion efficiency was basically not attenuated. After being stored in an air environment for 12 months, the conversion efficiency of the solar cell was still able to reach 94% of its initial state, indicating that the solar cell has high stability.

[0138] Experiment 6: The photoelectric conversion efficiency of the copper indium sulfur thin film solar cells of Examples 1-2 and Comparative Examples 1-2 was tested. The results are shown in Table 1.

[0139] Table 1

[0140]

[0141] Referring to the contents shown in Table 1, the photoelectric conversion efficiencies of Example 1 containing sulfur and Example 2 not containing sulfur are 12.68% and 10.07%, respectively. The photoelectric conversion efficiency of Example 1 is significantly higher than that of Example 2, indicating that sulfur has a significant effect on improving battery efficiency.

[0142] In addition, referring to the contents shown in Table 1, the photoelectric conversion efficiency of Comparative Example 1 is only 6.06%, and the photoelectric conversion efficiency of Examples 1 and 2 is significantly higher than that of Comparative Example 1. This is mainly due to the fact that both Examples 1 and 2 use titanium dioxide nanorod arrays as the matrix, and stack cadmium sulfide layers and copper indium sulfide layers on the side walls of the titanium dioxide nanorods. This structural design can effectively overcome the problem of short effective diffusion length of carriers in traditional technologies, so that the device has higher photon absorption capacity and charge collection efficiency. In contrast, Comparative Example 1 directly prepares cadmium sulfide layers and copper indium sulfide layers on the titanium dioxide base film, in which the problem of short effective diffusion length of carriers still exists. Although Comparative Example 2 uses titanium dioxide nanorod arrays as the matrix, it does not provide a cadmium sulfide layer, which makes it difficult for the electrons generated therein to be effectively extracted and transmitted. Therefore, the photoelectric conversion efficiency of Comparative Example 2 is not only significantly lower than that of Example 1, but also significantly lower than that of Comparative Example 1.

[0143] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0144] The above embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A copper indium sulfur thin film solar cell, characterized in that: It comprises a first electrode, titanium dioxide nanorods, a laminated structure and a second electrode, wherein the titanium dioxide nanorods and the laminated structure are arranged between the first electrode and the second electrode; The copper indium sulfide thin film solar cell comprises a plurality of titanium dioxide nanorods arranged at intervals, wherein the titanium dioxide nanorods are arranged on the first electrode and their axial directions extend in a direction away from the first electrode; the laminated structure comprises a stacked cadmium sulfide layer and a copper indium sulfide layer, wherein the cadmium sulfide layer covers the titanium dioxide nanorods, the copper indium sulfide layer is arranged on a side of the cadmium sulfide layer away from the titanium dioxide nanorods, the cadmium sulfide layer contacts the titanium dioxide nanorods and the copper indium sulfide layer, and the titanium dioxide nanorods, the cadmium sulfide layer and the copper indium sulfide layer form a heterojunction; The copper indium sulfur thin film solar cell also includes a titanium dioxide base film, which is stacked on the first electrode. The titanium dioxide nanorods grow on the titanium dioxide base film through a hydrothermal reaction, and the number density of the titanium dioxide nanorods is 80 / μm. 2 ~120 / μm 2 ; The preparation step of the copper indium sulfide layer includes: spin coating a second precursor solution on the cadmium sulfide layer, and performing a second heating reaction in a protective gas atmosphere to deposit a copper indium sulfide material on the surface of the cadmium sulfide layer, wherein the second heating reaction process includes: first heating at a temperature of 120° C. to 180° C. for 4 min to 6 min, and then heating at a temperature of 200° C. to 300° C. for 5 min to 15 min; The conversion efficiency of the copper indium sulfur thin film solar cell is above 10%.

2. The copper indium sulfur thin film solar cell according to claim 1, characterized in that: The height of the titanium dioxide nanorods is 500nm to 1200nm; and / or, The diameter of the titanium dioxide nanorods is 20 nm to 100 nm; and / or, The thickness of the cadmium sulfide layer is 10nm-30nm.

3. The copper indium sulfur thin film solar cell according to any one of claims 1 to 2, characterized in that: It also includes a hole transport layer, which is stacked between the stacked structure and the second electrode.

4. The copper indium sulfur thin film solar cell according to claim 3, characterized in that: The material of the hole transport layer includes Spiro-OMeTAD.

5. A method for preparing a copper indium sulfur thin film solar cell according to any one of claims 1 to 4, characterized in that: The steps include: providing a substrate including a first electrode; A titanium dioxide-based film is prepared on the first electrode, and the titanium dioxide nanorods are grown by a hydrothermal reaction; Growing the titanium dioxide nanorods based on the titanium dioxide base film; sequentially depositing the cadmium sulfide layer and the copper indium sulfide layer on the titanium dioxide nanorods to form the stacked structure; and, The second electrode is prepared on a side of the stacked structure away from the first electrode.

6. The method for preparing a copper indium sulfur thin film solar cell according to claim 5, characterized in that: The steps of growing the titanium dioxide nanorods include: The substrate prepared with the titanium dioxide-based film is placed in a hydrothermal container, and hydrothermal reactants are added into the hydrothermal container to carry out a hydrothermal reaction, wherein the hydrothermal reactants include water, hydrochloric acid and isopropyl titanate; the reaction temperature during the hydrothermal reaction is controlled to be 150°C to 200°C, and the reaction time is 1h to 5h.

7. The method for preparing a copper indium sulfur thin film solar cell according to claim 5, characterized in that: The step of depositing the cadmium sulfide layer comprises: The titanium dioxide nanorods are immersed in a first precursor solution containing cadmium ions and alkaline solution, and thiourea is added to perform a first heating reaction to form the cadmium sulfide layer. The reaction temperature during the first heating reaction is controlled to be 40° C. to 60° C., and the reaction time is 5 min to 15 min.

8. The method for preparing a copper indium sulfur thin film solar cell according to any one of claims 5 to 7, characterized in that: The second precursor solution includes indium ions, copper ions and thiourea, and the molar ratio of the indium ions, copper ions and thiourea is 1:(1.1-1.9):(6-10).

9. The method for preparing a copper indium sulfur thin film solar cell according to claim 8, characterized in that: The step of depositing the copper indium sulfide layer also includes: after depositing the copper indium sulfide material, placing the substrate and thiourea in a heating chamber, controlling the temperature in the heating chamber to 120° C. to 200° C. to perform a sulfurization treatment on the deposited copper indium sulfide material.

10. The method for preparing a copper indium sulfur thin film solar cell according to claim 8, characterized in that: Before preparing the second electrode, the step of preparing a hole transport layer is also included, which includes: spin coating a third precursor solution on the side of the stacked structure away from the first electrode, and annealing to form a hole transport layer; the third precursor solution includes Spiro-OMeTAD, LiTFSI and TBP, wherein the amount ratio of Spiro-OMeTAD, LiTFSI and TBP is 1: (0.4~0.6): (2~4).

Citation Information

Patent Citations

  • Photovoltaic cell based on zinc oxide nanorods and method for making the same

    CN101861654A

  • Thin-film photovoltaic devices and related manufacturing methods

    CN101990713A

  • CIGS nanostructure thin-film photovoltaic battery and preparation method thereof

    CN102629632A

  • TiO2-CuInS2 core-shell nanorod array-based organic / inorganic hybrid solar battery and manufacturing method thereof

    CN102842676A

  • CIGS-based thin-film solar cell and preparation method thereof

    CN106024937A