Negative electrode sheet and preparation method thereof and lithium ion battery

By designing a multi-channel carbon nanofiber layer and a transition layer with gradient distribution of tin in lithium-ion batteries, and using electrospinning technology to prepare negative electrode sheets, the tin volume expansion problem in lithium-ion batteries is solved, and the cycling performance of the battery is improved. Energy density.

CN118610375BActive Publication Date: 2024-12-03JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411074007.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-12-03
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The volume expansion of elemental tin in lithium-ion batteries causes the electrode material to pulverize and peel off, affecting the circulation performance, and the prior art is difficult to effectively alleviate this problem.

Method used

A negative electrode sheet is designed, which includes a multi-channel carbon nanofiber layer and a transition layer with gradient distribution of tin elemental mass. It is prepared by electrospinning technology to form a multi-channel nanofiber structure to alleviate the volume expansion of tin and improve the mechanics of the material. Structural performance.

Benefits of technology

It effectively alleviates the volume expansion of tin, improves the circulation performance and capacity retention rate of lithium-ion batteries, reduces the possibility of pole chip cracking, and improves the overall energy density of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118610375B_ABST
    Figure CN118610375B_ABST
Patent Text Reader

Abstract

The present application relates to the field of battery technology, and specifically to a negative electrode plate and a method for preparing the same, and a lithium-ion battery. The negative electrode plate comprises: a first multi-channel carbon nanofiber layer; a second multi-channel carbon nanofiber layer; a third transition layer disposed between the first multi-channel carbon nanofiber layer and the second multi-channel carbon nanofiber layer, the third transition layer comprising tin and multi-channel carbon nanofibers, and the content of tin in the third transition layer gradually decreases as it moves away from the first multi-channel carbon nanofiber layer. The negative electrode plate of the present invention has good mechanical structural properties, can effectively alleviate the volume expansion of tin during charging and discharging, and enables the manufactured lithium-ion battery to have a higher capacity and stable cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a negative electrode plate and a preparation method thereof, and a lithium-ion battery. Background Art

[0002] Currently, lithium-ion batteries (LIBs) are widely used in portable devices and electronic products. However, there are still some problems in the application of electric vehicles and renewable energy storage grids, including energy density, material cost and safety of use. Therefore, improving the energy density and cycle life of lithium-ion batteries is a very important aspect.

[0003] Elemental tin (Sn) has a high theoretical specific capacity of 994 mAh / g and is a very promising negative electrode material. However, during the charge and discharge process, Sn will undergo an alloying reaction with lithium, resulting in a large volume expansion. The internal stress generated by the volume expansion will cause the electrode material to pulverize and peel off, resulting in a decrease in capacity and rapid decay of cycle performance. Therefore, the volume expansion of elemental tin is an important issue that needs to be solved at this stage.

[0004] Research has found that combining Sn with carbon materials can significantly alleviate this phenomenon and increase the electron conduction rate. However, there is still a certain volume expansion, which affects the cycle performance of lithium-ion batteries. Summary of the invention

[0005] In view of this, the present invention provides a negative electrode sheet and a preparation method thereof and a lithium ion battery. The negative electrode sheet has good mechanical structural properties, can effectively alleviate the volume expansion of tin during charging and discharging, so that the manufactured lithium ion battery has a higher capacity and stable cycle performance.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] In a first aspect, the present invention provides a negative electrode plate, the negative electrode plate comprising:

[0008] a first multi-channel carbon nanofiber layer;

[0009] a second multi-channel carbon nanofiber layer;

[0010] A third transition layer is arranged between the first multi-channel carbon nanofiber layer and the second multi-channel carbon nanofiber layer. The third transition layer includes tin and multi-channel carbon nanofibers. The content of tin in the third transition layer gradually decreases in a direction gradually away from the first multi-channel carbon nanofiber layer.

[0011] In an embodiment of the present invention, the third transition layer has a first surface close to the first multi-channel carbon nanofiber layer and a second surface arranged opposite to the first surface; the thickness of the negative electrode plate is denoted as H, the area from the first surface of the third transition layer to the thickness range of 0.6H to 0.7H is recorded as the first area of ​​the third transition layer, and the area from the second surface of the third transition layer to the thickness range of 0.04H to 0.06H is recorded as the second area of ​​the third transition layer.

[0012] Preferably, the thickness of the first multi-channel carbon nanofiber layer is 0.02H-0.04H.

[0013] Preferably, the thickness of the second multi-channel carbon nanofiber layer is 0.02H-0.04H.

[0014] In an embodiment of the present invention, the first region includes a first tin element and a first multi-channel carbon nanofiber, and the first tin element is uniformly distributed in the first multi-channel carbon nanofiber; the second region includes a second tin element and a second multi-channel carbon nanofiber, and the second tin element is uniformly distributed in the second multi-channel carbon nanofiber.

[0015] Preferably, the molar ratio of the first tin element to the first multi-channel carbon nanofibers in the first region is 1:(8-15).

[0016] Preferably, the molar ratio of the first tin element to the first multi-channel carbon nanofibers in the first region is 1:(10-12).

[0017] Preferably, the molar ratio of the second tin element to the second multi-channel carbon nanofibers in the second region is 1:(35-40).

[0018] Preferably, the molar ratio of the second tin element to the second multi-channel carbon nanofibers in the second region is 1:(37-39).

[0019] Preferably, the porosity of the fiber skeleton in the first region is 22% to 23%.

[0020] Preferably, the porosity of the fiber skeleton in the second region is 19% to 21%.

[0021] Preferably, the porosity of the fiber skeleton of the first multi-channel carbon nanofiber layer or the second multi-channel carbon nanofiber layer is 23% to 24%.

[0022] Preferably, the fiber diameter of the fiber skeleton in the first multi-channel carbon nanofiber layer, the second multi-channel carbon nanofiber layer or the third transition layer is 300-400 nm.

[0023] In the implementation manner of the present invention, the area between the first area and the second area is recorded as an intermediate area, and the intermediate area includes m intermediate areas, where m≥1.

[0024] In the embodiment of the present invention, the middle region includes a third tin element and third multi-channel carbon nanofibers, and the third tin element is uniformly distributed in the third multi-channel carbon nanofibers in each middle region.

[0025] In an embodiment of the present invention, when m≥2, the content of the tin element in the m middle regions gradually decreases along the direction gradually away from the first multi-channel carbon nanofiber layer, the thickness of the m middle regions gradually decreases, and the porosity of the m middle regions gradually decreases.

[0026] In the embodiment of the present invention, when m≥2, the middle region adjacent to the first region is recorded as the first middle region, and the middle region adjacent to the second region is recorded as the mth middle region.

[0027] In an embodiment of the present invention, the content of the tin element in the first intermediate region is less than that in the first region, and the content of the tin element in the mth intermediate region is greater than that in the second region.

[0028] In an embodiment of the present invention, the thickness of the first intermediate region is smaller than the thickness of the first region, and the thickness of the mth intermediate region is larger than the thickness of the second region.

[0029] In an embodiment of the present invention, the porosity of the fiber skeleton in the first intermediate region is smaller than that in the first region, and the porosity of the fiber skeleton in the mth intermediate region is larger than that in the second region.

[0030] In a second aspect, the present invention provides a method for preparing the above-mentioned negative electrode sheet, comprising the following steps:

[0031] S1, mixing the carbon source and the solvent, performing a first stirring, and obtaining a carbon source solution after stirring evenly; mixing the tin source, the pore-forming agent and the carbon source solution, and performing a second stirring to obtain solutions with different tin source concentrations, and the solutions with different tin source concentrations are respectively recorded as A and B according to the tin source concentration from high to low. 1 , A 2 ...A n-1 , A n ; n ≥ 3;

[0032] The carbon source and the solvent are mixed and stirred for the third time to obtain a carbon source solution after being stirred evenly; the pore-forming agent and the carbon source solution are mixed and stirred for the fourth time to obtain a first solution and a second solution without a tin source, and the first solution is recorded as B 1 , the second solution is denoted as B 2 ;

[0033] S2, B 1 , A 1 , A 2 ...An-1 , A n , B 2 Electrospinning is performed sequentially to prepare a fiber membrane;

[0034] S3, heating the fiber membrane in an oxygen-containing atmosphere, and then calcining it in an inert gas atmosphere to obtain a negative electrode sheet.

[0035] In an embodiment of the present invention, the carbon source includes but is not limited to at least one of polyacrylonitrile, polyvinyl pyrrolidone, polyvinyl alcohol, and polyvinylidene fluoride.

[0036] In an embodiment of the present invention, the solvent includes but is not limited to at least one of N,N-dimethylformamide, N,N-dimethylacetamide, anhydrous ethanol, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, and ethylene carbonate.

[0037] In an embodiment of the present invention, the tin source includes but is not limited to stannous chloride (SnCl 2 ), at least one of stannous isooctanoate.

[0038] In an embodiment of the present invention, the pore-forming agent includes but is not limited to at least one of polystyrene, polyvinyl pyrrolidone, and polymethyl methacrylate.

[0039] In the embodiment of the present invention, A 1 , A 2 ...A n-1 , A n The content of tin source in the medium gradually decreases.

[0040] As a preference, A 1 The content of tin source is 9 wt% to 10 wt%.

[0041] As a preference, A 2 To A n-1 The content of tin source in one of the catalysts is 3 wt% to 9 wt%.

[0042] As a preference, A n The content of tin source is 1 wt% to 3wt%.

[0043] As a preference, A 1 , A 2 ...A n-1 , A n , B 1 , B 2 The content of the pore-forming agent in the mixture is 5 wt% to 8 wt%.

[0044] Preferably, in step S1, the first stirring, the second stirring, the third stirring or the fourth stirring is stirring under oil bath conditions, the temperature of the oil bath is 60-80° C.; the second stirring time is 8-14 h; the fourth stirring time is 4-6 h.

[0045] Preferably, in step S2, the conditions for electrospinning are: the distance between the spinneret and the receiver roller is 10-18 cm, the voltage is 10-25 kV, the flow rate is 0.5-1.0 mL / h, the humidity is less than 20%, the receiver is made of aluminum foil, and the spinneret width is 10-12 cm.

[0046] In an embodiment of the present invention, in step S3, before the heating treatment, a step of fixing the fiber membrane with a clamp is also included.

[0047] Preferably, the heating rate of the heating treatment is 2-5°C / min, the holding temperature is 250-300°C, and the holding time is 100-150 min.

[0048] Preferably, the heating rate of the calcination treatment is 2-5°C / min, the holding temperature is 600-900°C, and the holding time is 100-150 min.

[0049] In a third aspect, the present invention provides a lithium-ion battery, which includes a positive electrode plate, a negative electrode plate, a separator and an electrolyte, wherein the negative electrode plate is the above-mentioned negative electrode plate and / or the negative electrode plate prepared by the above-mentioned preparation method.

[0050] Compared with the prior art, the present invention has the following beneficial effects:

[0051] The negative electrode plate of the present invention is a tin-carbon material with a multi-channel nanofiber structure and a metal tin concentration gradient. The metal tin is evenly distributed inside the nanofiber. The multi-channel structure of the first region (high tin region) of the third transition layer is relatively small, while the multi-channel structure of the second region (low tin region) of the third transition layer is relatively loose, and the pores of the multi-channel structure are relatively large. The metal tin in the high tin region undergoes a large volume expansion during the charge and discharge process, but the middle region (transition region) and the second region (low tin region) in contact with it can act as a buffer. The multi-channel carbon nanofiber can effectively alleviate the volume expansion of tin during the charge and discharge process, stabilize the material structure, and reduce the volume expansion caused by Li +The mechanical stress caused by embedding / ejection makes the negative electrode have good mechanical structural properties and can maintain excellent structural stability. At the same time, it provides more channels for ion / electron transmission, reduces the shedding of active materials into the electrolyte, reduces the possibility of electrode cracking, and improves the cycle life. Multi-channel carbon nanofibers are cross-linked to form a 3D conductive network, which can not only disperse the current density, but also accommodate metallic lithium deposition. In addition, the multi-channel nanofiber structure is conducive to full contact between the electrode and the electrolyte, which helps the embedding and extraction of ions / electrons, thereby obtaining higher capacity and improving the first coulomb efficiency and capacity retention rate.

[0052] The negative electrode plate of the present invention can completely avoid using inactive materials such as rigid current collectors, binders and conductive agents, and can be directly used as an electrode of a lithium ion battery, avoiding the introduction of binders that lead to a decrease in the conductivity of active materials, and greatly improving the overall energy density of the battery.

[0053] The present invention utilizes electrostatic spinning technology to design and prepare the negative electrode sheet. The preparation method is simple to operate, the morphology is easy to control, the cost is low, and it is conducive to industrial production.

[0054] The lithium ion battery assembled from the negative electrode sheet of the present invention has a higher capacity and a stable cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] Figure 1 Schematic diagram of the structure of the negative electrode plate of Example 1.

[0056] Figure 2 This is an XRD image of carbon nanofibers (Sn@MCNF) containing tin in the first region of the third transition layer of the negative electrode sheet of Example 1.

[0057] Figure 3 This is a SEM image of the cross section of the fiber skeleton in the first region of the third transition layer of the negative electrode plate of Example 1.

[0058] Figure 4 This is a TEM image of the fiber skeleton in the first region of the third transition layer of the negative electrode plate of Example 1, with a scale of 200 nm.

[0059] Figure 5 This is a TEM image of the fiber skeleton in the first region of the third transition layer of the negative electrode plate of Example 1, with a scale of 10 nm.

[0060] Figure 6 This is the C element mapping image of the fiber skeleton in the first region of the third transition layer of the negative electrode plate of Example 1.

[0061] Figure 7 This is the Sn element mapping image of the fiber skeleton in the first region of the third transition layer of the negative electrode sheet of Example 1.

[0062] Figure 8 Schematic diagram of the structure of the negative electrode plate of Example 4.

[0063] The reference numerals are as follows:

[0064] 11, a first multi-channel carbon nanofiber layer;

[0065] 12, a second multi-channel carbon nanofiber layer;

[0066] 21, first area;

[0067] 22, 1st intermediate area;

[0068] 23, 2nd middle area;

[0069] 24, second area. DETAILED DESCRIPTION

[0070] The present invention discloses a negative electrode plate and a method for preparing the same, and a lithium-ion battery. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the same. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

[0071] In the description of the present invention, it should be noted that the terms "first", "second", etc. are only used for descriptive purposes, and do not indicate or imply relative importance.

[0072] In the description of the present invention, a list of items connected by the term "at least one of" or other similar terms may mean any combination of the listed items. For example, if items A, B are listed, the phrase "at least one of A, B" means only A; only B; or A and B. In another example, if items A, B, C are listed, the phrase "at least one of A, B, C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.

[0073] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range or the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0074] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0075] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0076] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or included, or may only include or include the listed components.

[0077] Electrospinning is a special fiber manufacturing process in which a solution or melt is jet-spun in a strong electric field. Under the action of the electric field, the droplet at the needle tip changes from a sphere to a cone (i.e., a "Taylor cone"), and fiber filaments are extended from the tip of the cone. This method can produce filaments with nanometer diameters. The present invention uses this technology to design a self-supporting negative electrode with a concentration gradient. The material has a multi-channel nanofiber structure, which can stabilize the volume expansion of Sn while allowing the material to be more fully in contact with the electrolyte, allowing lithium ions to be quickly transmitted. In addition, carbon-based materials also have good electrical conductivity, and combining with Sn can improve the conductivity of the material to a certain extent.

[0078] Specifically, the present invention adopts the following technical solutions:

[0079] In a first aspect, the present invention provides a negative electrode plate, the negative electrode plate comprising:

[0080] a first multi-channel carbon nanofiber layer;

[0081] a second multi-channel carbon nanofiber layer;

[0082] A third transition layer is arranged between the first multi-channel carbon nanofiber layer and the second multi-channel carbon nanofiber layer. The third transition layer includes tin and multi-channel carbon nanofibers. The content of tin in the third transition layer gradually decreases in a direction gradually away from the first multi-channel carbon nanofiber layer.

[0083] In an embodiment of the present invention, the third transition layer has a first surface close to the first multi-channel carbon nanofiber layer and a second surface arranged opposite to the first surface; the thickness of the negative electrode plate is denoted as H, the area from the first surface of the third transition layer to the thickness range of 0.6H to 0.7H is recorded as the first area of ​​the third transition layer, and the area from the second surface of the third transition layer to the thickness range of 0.04H to 0.06H is recorded as the second area of ​​the third transition layer. Exemplarily, the thickness of the first region is any value among 0.6H, 0.61H, 0.62H, 0.63H, 0.64H, 0.65H, 0.66H, 0.67H, 0.68H, 0.69H, 0.7H, or any value within the range consisting of any two of the above values, and the thickness of the second region is any value among 0.04H, 0.042H, 0.044H, 0.046H, 0.048H, 0.05H, 0.052H, 0.054H, 0.056H, 0.058H, 0.06H, or any value within the range consisting of any two of the above values.

[0084] Preferably, the thickness of the first multi-channel carbon nanofiber layer is 0.02H to 0.04H. Exemplarily, the thickness of the first multi-channel carbon nanofiber layer is any value among 0.02H, 0.022H, 0.024H, 0.026H, 0.028H, 0.03H, 0.032H, 0.034H, 0.036H, 0.038H, 0.04H or any value within the range consisting of any two of the above values.

[0085] Preferably, the thickness of the second multi-channel carbon nanofiber layer is 0.02H to 0.04H. Exemplarily, the thickness of the second multi-channel carbon nanofiber layer is any value among 0.02H, 0.022H, 0.024H, 0.026H, 0.028H, 0.03H, 0.032H, 0.034H, 0.036H, 0.038H, 0.04H or any value within the range consisting of any two of the above values.

[0086] In an embodiment of the present invention, the first region includes a first tin element and a first multi-channel carbon nanofiber, and the first tin element is uniformly distributed in the first multi-channel carbon nanofiber; the second region includes a second tin element and a second multi-channel carbon nanofiber, and the second tin element is uniformly distributed in the second multi-channel carbon nanofiber.

[0087] Preferably, the molar ratio of the first tin element to the first multi-channel carbon nanofiber in the first region is 1:(8-15). Exemplarily, the molar ratio of the first tin element to the first multi-channel carbon nanofiber in the first region is any value among 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, or any value within the range of any two of the above values.

[0088] Preferably, the molar ratio of the first tin element to the first multi-channel carbon nanofibers in the first region is 1:(10-12).

[0089] Preferably, the molar ratio of the second tin element to the second multi-channel carbon nanofiber in the second region is 1:(35-40). Exemplarily, the molar ratio of the second tin element to the second multi-channel carbon nanofiber in the second region is any one of 1:35, 1:36, 1:37, 1:38, 1:39, 1:40 or any value within the range of any two of the above values.

[0090] Preferably, the molar ratio of the second tin element to the second multi-channel carbon nanofibers in the second region is 1:(37-39).

[0091] Preferably, the porosity of the fiber skeleton in the first region is 22% to 23%. Exemplarily, the porosity of the fiber skeleton in the first region is any value among 22%, 22.1%, 22.2%, 22.3%, 22.4%, 22.5%, 22.6%, 22.7%, 22.8%, 22.9%, 23%, or any value within the range consisting of any two of the above values.

[0092] Preferably, the porosity of the fiber skeleton in the second region is 19% to 21%. Exemplarily, the porosity of the fiber skeleton in the second region is any value among 19%, 19.2%, 19.4%, 19.6%, 19.8%, 20%, 20.2%, 20.4%, 20.6%, 20.8%, 21%, or any value within the range of any two of the above values.

[0093] Preferably, the porosity of the fiber skeleton of the first multi-channel carbon nanofiber layer or the second multi-channel carbon nanofiber layer is 23% to 24%. Exemplarily, the porosity of the fiber skeleton of the first multi-channel carbon nanofiber layer or the second multi-channel carbon nanofiber layer is any value among 23%, 23.1%, 23.2%, 23.3%, 23.4%, 23.5%, 23.6%, 23.7%, 23.8%, 23.9%, 24%, or any value within the range consisting of any two of the above values.

[0094] The porosity of each layer is related to the concentration of the preparation solution and the amount of pore-forming agent added. On the one hand, the higher the concentration of the preparation solution of each layer, the greater the porosity inside the fiber, because high-concentration solutions are more likely to form pore structures during the stretching process, thereby increasing the porosity of the fiber. On the other hand, the more pore-forming agent is added, the greater the porosity.

[0095] Preferably, the fiber diameter of the fiber skeleton in the first multi-channel carbon nanofiber layer, the second multi-channel carbon nanofiber layer or the third transition layer is 300 to 400 nm. Exemplarily, the fiber diameter of the fiber skeleton in the first multi-channel carbon nanofiber layer, the second multi-channel carbon nanofiber layer or the third transition layer is any value in 300 nm, 310 nm, 320 nm, 330 nm, 340 nm, 350 nm, 360 nm, 370 nm, 380 nm, 390 nm, 400 nm or any value in the range of any two of the above values.

[0096] In the embodiment of the present invention, the area between the first area and the second area is recorded as the intermediate area, and the intermediate area includes m intermediate areas, where m≥1. Exemplarily, m is any value among 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 or any value within the range of any two of the above values. Preferably, m is 1-3.

[0097] In the embodiment of the present invention, the middle region includes a third tin element and third multi-channel carbon nanofibers, and the third tin element is uniformly distributed in the third multi-channel carbon nanofibers in each middle region.

[0098] In an embodiment of the present invention, when m≥2, the content of the tin element in the m middle regions gradually decreases along the direction gradually away from the first multi-channel carbon nanofiber layer, the thickness of the m middle regions gradually decreases, and the porosity of the m middle regions gradually decreases.

[0099] In the embodiment of the present invention, when m≥2, the middle region adjacent to the first region is recorded as the first middle region, and the middle region adjacent to the second region is recorded as the mth middle region.

[0100] In an embodiment of the present invention, the content of the tin element in the first intermediate region is less than that in the first region, and the content of the tin element in the mth intermediate region is greater than that in the second region.

[0101] Preferably, the molar ratio of the third tin element to the third multi-channel carbon nanofiber in an intermediate region is 1: (12-38). Exemplarily, the molar ratio of the third tin element to the third multi-channel carbon nanofiber in an intermediate region may be any of 1:12, 1:14, 1:16, 1:18, 1:20, 1:22, 1:24, 1:26, 1:28, 1:30, 1:32, 1:34, 1:36, 1:38 or any value within the range of any two of the above values. As long as the above-mentioned tin content gradually decreases from the first intermediate region to the mth intermediate region, and the tin content in the first intermediate region is less than the tin content in the first region, the tin content in the mth intermediate region is greater than the tin content in the second region.

[0102] In an embodiment of the present invention, the thickness of the first intermediate region is smaller than the thickness of the first region, and the thickness of the mth intermediate region is larger than the thickness of the second region.

[0103] Preferably, the thickness of an intermediate region is 0.06H to 0.6H. Exemplarily, the thickness of an intermediate region may be any value among 0.06H, 0.1H, 0.15H, 0.16H, 0.18H, 0.19H, 0.2H, 0.25H, 0.28H, 0.3H, 0.35H, 0.4H, 0.45H, 0.5H, 0.55H, 0.6H, or any value within the range of any two of the above values. As long as the thickness of the first intermediate region to the mth intermediate region gradually decreases, the thickness of the first intermediate region is less than the thickness of the first region, and the thickness of the mth intermediate region is greater than the thickness of the second region, the rule is satisfied.

[0104] In an embodiment of the present invention, the porosity of the fiber skeleton in the first intermediate region is smaller than that in the first region, and the porosity of the fiber skeleton in the mth intermediate region is larger than that in the second region.

[0105] Preferably, the porosity of the fiber skeleton in an intermediate region is 20% to 22.5%. Exemplarily, the porosity of the fiber skeleton in an intermediate region may be any value among 20%, 20.5%, 21%, 21.5%, 22%, 22.5%, or any value within the range of any two of the above values. As long as the porosity of the fiber skeleton from the first intermediate region to the mth intermediate region gradually decreases, and the porosity of the fiber skeleton in the first intermediate region is less than the porosity of the fiber skeleton in the first region, and the porosity of the fiber skeleton in the mth intermediate region is greater than the porosity of the fiber skeleton in the second region, the rule is satisfied.

[0106] In a second aspect, the present invention provides a method for preparing the above-mentioned negative electrode sheet, comprising the following steps:

[0107] S1, mixing the carbon source and the solvent, performing a first stirring, and obtaining a carbon source solution after stirring evenly; mixing the tin source, the pore-forming agent and the carbon source solution, and performing a second stirring to obtain solutions with different tin source concentrations, and the solutions with different tin source concentrations are respectively recorded as A and B according to the tin source concentration from high to low. 1 , A 2 ...A n-1 , A n ; n ≥ 3;

[0108] The carbon source and the solvent are mixed and stirred for the third time to obtain a carbon source solution after being stirred evenly; the pore-forming agent and the carbon source solution are mixed and stirred for the fourth time to obtain a first solution and a second solution without a tin source, and the first solution is recorded as B 1 , the second solution is denoted as B 2 ;

[0109] S2, B 1 , A 1 , A 2 ...A n-1 , A n , B 2 Electrospinning is performed sequentially to prepare a fiber membrane;

[0110] S3, heating the fiber membrane in an oxygen-containing atmosphere, and then calcining it in an inert gas atmosphere to obtain a negative electrode sheet.

[0111] In the embodiment of the present invention, the carbon source includes but is not limited to at least one of polyacrylonitrile, polyvinyl pyrrolidone, polyvinyl alcohol and polyvinylidene fluoride. Polyacrylonitrile is preferred, which provides a carbon source and is doped with N atoms to increase the capacity.

[0112] In an embodiment of the present invention, the solvent includes but is not limited to at least one of N,N-dimethylformamide, N,N-dimethylacetamide, anhydrous ethanol, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, and ethylene carbonate, preferably N,N-dimethylformamide.

[0113] In an embodiment of the present invention, the tin source includes but is not limited to stannous chloride (SnCl 2 ), at least one of stannous isooctanoate.

[0114] In an embodiment of the present invention, the pore-forming agent includes but is not limited to at least one of polystyrene, polyvinyl pyrrolidone, and polymethyl methacrylate.

[0115] In the embodiment of the present invention, A 1 , A 2 ...A n-1 , An The content of tin source in the medium gradually decreases.

[0116] As a preference, A 1 The content of tin source in the catalyst is 9 wt% to 10 wt%. 1 The content of the tin source in the tin source is any value among 9wt%, 9.2wt%, 9.4wt%, 9.6wt%, 9.8wt%, 10wt% or any value within the range formed by any two of the above values. When the concentration is higher than this range, it is not conducive to spinning.

[0117] As a preference, A 2 To A n-1 In one embodiment, the content of the tin source is 3 wt% to 9 wt%. 2 To A n-1 The content of tin source in one of the above is any value among 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt% or any value within the range composed of any two of the above values.

[0118] As a preference, A n The content of tin source in the catalyst is 1 wt% to 3 wt%. n The content of the tin source is any value among 1wt%, 1.2wt%, 1.4wt%, 1.6wt%, 1.8wt%, 2wt%, 2.2wt%, 2.4wt%, 2.6wt%, 2.8wt%, 3wt% or any value within the range formed by any two of the above values.

[0119] As a preference, A 1 , A 2 ...A n-1 , A n , B 1 , B 2 In one embodiment, the content of the pore former is 5 wt% to 8 wt%. For example, the content of the pore former is any one of 5 wt%, 5.5 wt%, 6 wt%, 6.5 wt%, 7 wt%, 7.5 wt%, 8 wt%, or any value within the range consisting of any two of the above values.

[0120] Preferably, in step S1, the first stirring, the second stirring, the third stirring or the fourth stirring is stirring under oil bath conditions, the temperature of the oil bath is 60-80°C; the second stirring time is 8-14 h; the fourth stirring time is 4-6 h. Exemplarily, the temperature of the oil bath is any value among 60°C, 62°C, 64°C, 66°C, 68°C, 70°C, 72°C, 74°C, 76°C, 78°C, 80°C or any value within the range of any two of the above values, the second stirring time is any value among 8 h, 9 h, 10 h, 11 h, 12 h, 13 h, 14 h or any value within the range of any two of the above values, and the fourth stirring time is any value among 4 h, 4.5 h, 5 h, 5.5 h, 6 h or any value within the range of any two of the above values. Solutions with different tin source concentrations require longer heating time to fully dissolve due to the presence of tin source; in solutions without tin source, the carbon source and pore former are easier to dissolve, so the heating time can be reduced.

[0121] Preferably, in step S2, the conditions for electrospinning are: the distance between the spinneret and the receiver roller is 10-18 cm, the voltage is 10-25 kV, the flow rate is 0.5-1.0 mL / h, the humidity is less than 20%, the receiver is an aluminum foil material, and the spinneret width is 10-12 cm. The above-mentioned technical parameters of electrospinning are conventional parameters in the spinning field, and those skilled in the art can adjust them according to their needs.

[0122] In an embodiment of the present invention, in step S3, before the heating treatment, a step of fixing the fiber membrane with a clamp is also included.

[0123] Preferably, the heating rate of the heat treatment is 2-5°C / min, the holding temperature is 250-300°C, and the holding time is 100-150 min. Exemplarily, the heating rate of the heat treatment is any value among 2°C / min, 3°C / min, 4°C / min, 5°C / min, or any value within the range of any two of the above values, the holding temperature of the heat treatment is any value among 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, or any value within the range of any two of the above values, and the holding time of the heat treatment is any value among 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, or any value within the range of any two of the above values. The purpose of the heat treatment is to accelerate the curing of the fiber membrane and stabilize the structure of the material.

[0124] Preferably, the heating rate of the calcination treatment is 2-5°C / min, the holding temperature is 600-900°C, and the holding time is 100-150 min. Exemplarily, the heating rate of the calcination treatment is any of 2°C / min, 3°C / min, 4°C / min, 5°C / min or any of the ranges of any two of the above values, the holding temperature of the calcination treatment is any of 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C or any of the ranges of any two of the above values, and the holding time of the calcination treatment is any of 100 min, 110 min, 120 min, 130 min, 140 min, 150 min or any of the ranges of any two of the above values. The purpose of the calcination treatment is, first, carbonization of the carbon source, second, reduction of the tin source to a single substance of tin, and third, removal of the pore-forming agent in the fiber membrane.

[0125] In a third aspect, the present invention provides a lithium-ion battery, which includes a positive electrode plate, a negative electrode plate, a separator and an electrolyte, wherein the negative electrode plate is the above-mentioned negative electrode plate and / or the negative electrode plate prepared by the above-mentioned preparation method.

[0126] In the embodiment of the present invention, the battery structure includes but is not limited to button batteries, soft-pack batteries, cylindrical batteries, etc.

[0127] The present application has no particular restrictions on the negative electrode sheet, separator, and electrolyte in the battery, and those skilled in the art can select them according to actual needs as long as the purpose of the present application can be achieved.

[0128] The reagents, instruments or materials used in the present invention can be obtained through commercial channels.

[0129] The present invention will be further described below in conjunction with embodiments:

[0130] Example 1: B 1 , A 1 , A 2 , A 3 , A 4 , B 2

[0131] 1. Negative electrode sheet structure and preparation method thereof

[0132] (1) Negative electrode structure

[0133] like Figure 1 As shown, the negative electrode sheet (thickness 120μm) includes from bottom to top:

[0134] The first multi-channel carbon nanofiber layer (3% thickness, 24% porosity),

[0135] The first area of ​​the third transition layer (i.e., the high tin area, with a thickness of 65%, a porosity of 23%, and a Sn / C molar ratio of 1:11.3),

[0136] The first middle area of ​​the third transition layer (i.e., transition zone, thickness accounts for 16%, porosity is 22%, Sn / C molar ratio is 1:13.6),

[0137] The second middle region of the third transition layer (i.e., transition zone, thickness accounts for 8%, porosity is 20%, Sn / C molar ratio is 1:22.6),

[0138] The second region of the third transition layer (i.e., the low tin region, with a thickness of 5%, a porosity of 19%, and a Sn / C molar ratio of 1:37.7)

[0139] The second multi-channel carbon nanofiber layer (3% thickness, 24% porosity).

[0140] Depend on Figure 2 From the XRD spectrum of the negative electrode sheet material of this embodiment, it can be seen that the peak of the X-ray diffraction peak of Sn is obvious, and the characteristic peaks at 30.6°, 32°, 43.9°, and 44.9° correspond to (200), (101), (220), and (211), respectively. There is an obvious carbon peak near 23°, which is determined to be the Sn@MCNF phase, that is, the mesoporous carbon nanofiber (MCNF) containing Sn.

[0141] Depend on Figure 3 SEM images and Figure 4 and Figure 5 It can be seen from the TEM image that on the cross-section of the fiber, the channel holes are evenly distributed and the fiber diameter is 300-400nm.

[0142] Depend on Figure 4 and Figure 6 It can be seen that the fiber skeleton in the first region of the third transition layer has a multi-channel structure.

[0143] Depend on Figure 7 From the mapping diagram, it can be seen that the Sn particles are dispersed in the carbon nanofibers.

[0144] (2) Preparation method of negative electrode sheet

[0145] S1. Dissolve 1.2 g polyacrylonitrile (the amount of substance of the C element is 0.0678 mol) in 10 mL N,N-dimethylformamide, stir evenly in an oil bath at 60°C, add 0.7 g polystyrene and 1.15 g stannous chloride (the amount of substance of the Sn element is 0.006 mol, and the concentration of stannous chloride is 9.2%) in sequence while stirring, and stir in the oil bath for 12 h to obtain solution A. 1.

[0146] 1.2 g of polyacrylonitrile was dissolved in 10 mL of N,N-dimethylformamide and stirred evenly in an oil bath at 60 °C. 0.8 g of polystyrene and 0.95 g of stannous chloride (the amount of Sn element was 0.005 mol and the concentration of stannous chloride was 7.7%) were added in turn under stirring. The solution A was obtained by stirring in an oil bath for 12 h. 2 .

[0147] 1.2 g of polyacrylonitrile was dissolved in 10 mL of N,N-dimethylformamide and stirred evenly in an oil bath at 60 °C. 0.9 g of polystyrene and 0.6 g of stannous chloride (the amount of Sn element was 0.003 mol and the concentration of stannous chloride was 4.9%) were added in turn under stirring. The solution A was obtained by stirring in an oil bath for 12 h. 3 .

[0148] 1.2 g of polyacrylonitrile was dissolved in 10 mL of N,N-dimethylformamide and stirred evenly in an oil bath at 60 °C. 0.9 g of polystyrene and 0.35 g of stannous chloride (the amount of Sn element was 0.0018 mol and the concentration of stannous chloride was 2.9%) were added in turn under stirring. The solution A was obtained by stirring in an oil bath for 12 h. 4 .

[0149] 1.2 g of polyacrylonitrile was dissolved in 10 mL of N,N-dimethylformamide and stirred evenly in an oil bath at 60°C. 0.9 g of polystyrene was added in sequence under stirring and stirred in the oil bath for 4 h to obtain solution B.

[0150] S2. B, A 1 , A 2 , A 3 , A 4 , B are electrospun in sequence to obtain B 1 , A 1 , A 2 , A 3 , A 4 , B 2 The fiber layer finally prepared the electrospun fiber containing tin. The distance between the electrospinning spinneret and the receiver roller was 15 cm; the voltage was 20 kV; the flow rate was 0.8 mL / h, and the humidity was 18%. The receiver was made of aluminum foil; the electrospinning spinneret width was 12 cm. The percentage of each layer solution was: B 1 3%, A 1 65%, A 2 16%, A 3 8%, A 4 5%, B 2 3%.

[0151] S3. The electrospun fibers collected in S2 were kept at 280°C in air for 2 h to stabilize the structure of the material, and then calcined at 700°C in an argon atmosphere for 2 h to remove the polystyrene in the fibers and obtain tin-containing multi-channel carbon nanofibers. The electrospun fibers need to be fixed with a splint when heated, and the heating rate is 2°C / min.

[0152] 2. Preparation of lithium-ion batteries

[0153] The lithium-ion battery of this embodiment includes a positive electrode, a negative electrode, a separator, and an electrolyte. The negative electrode is the self-supporting tin-carbon negative electrode sheet prepared as described above, which is cut into round pieces with a mass of 3 to 4 mg by a punching machine.

[0154] The button half-cell was assembled in an argon-filled glove box, with metallic lithium as the counter electrode and 1 mol L electrolyte. −1 LiPF 6 (The solvent was EC+DEC, and the volume ratio of EC: DEC=1:1), the separator was Celgard 2400 polymer separator, and the electrochemical test was carried out after standing for 16 h.

[0155] Embodiment 2:

[0156] Compared with Example 1, this example is different only in the calcination temperature in step S3 of the preparation method, which is 600° C., and other conditions are the same.

[0157] Embodiment 3:

[0158] Compared with Example 1, this embodiment is different only in the calcination temperature in step S3 of the preparation method, which is 800° C., and other conditions are the same.

[0159] Example 4: B 1 , A 1 , A 2 , A 3 , B 2

[0160] 1. Negative electrode sheet structure and preparation method thereof

[0161] (1) Negative electrode structure

[0162] Compared with Example 1, the third transition layer in this example includes an intermediate area.

[0163] like Figure 8 As shown, the negative electrode sheet (thickness 120μm) includes from bottom to top:

[0164] The first multi-channel carbon nanofiber layer (3% thickness, 24% porosity),

[0165] The first area of ​​the third transition layer (i.e., the high tin area, with a thickness of 70%, a porosity of 23%, and a Sn / C molar ratio of 1:11.3),

[0166] The middle area of ​​the third transition layer (i.e., transition zone, thickness accounts for 19%, porosity is 22%, Sn / C molar ratio is 1:18.3),

[0167] The second region of the third transition layer (i.e., the low tin region, with a thickness of 5%, a porosity of 19%, and a Sn / C molar ratio of 1:37.7)

[0168] The second multi-channel carbon nanofiber layer (3% thickness, 24% porosity).

[0169] (2) Preparation method of negative electrode sheet

[0170] S1. Dissolve 1.2 g of polyacrylonitrile in 10 mL of N,N-dimethylformamide and stir evenly in an oil bath at 60°C. Add 0.7 g of polystyrene and 1.15 g of stannous chloride in turn while stirring. Stir in the oil bath for 12 h to obtain solution A. 1 .

[0171] 1.2 g of polyacrylonitrile was dissolved in 10 mL of N,N-dimethylformamide and stirred evenly in an oil bath at 60 °C. 0.8 g of polystyrene and 0.7 g of stannous chloride (the amount of Sn element was 0.0037 mol and the concentration of stannous chloride was 5.7%) were added in sequence under stirring. The solution A was obtained by stirring in the oil bath for 12 h. 2 .

[0172] 1.2 g of polyacrylonitrile was dissolved in 10 mL of N,N-dimethylformamide and stirred evenly in an oil bath at 60 °C. 0.9 g of polystyrene and 0.35 g of stannous chloride were added in sequence under stirring and stirred in the oil bath for 12 h to obtain solution A. 3 .

[0173] 1.2 g of polyacrylonitrile was dissolved in 10 mL of N,N-dimethylformamide and stirred evenly in an oil bath at 60 °C. 0.9 g of polystyrene was added in sequence under stirring and stirred in the oil bath for 4 h to obtain solution B.

[0174] S2. B, A 1 , A 2 , A 3 , B are electrospun in sequence to obtain B 1 , A 1 , A 2 , A 3 , B 2The fiber layer is finally prepared to obtain tin-containing electrospun fibers. The electrospinning preparation parameters are the same as those in Example 1. The percentages of the solutions in each layer are: 1 3%, A 1 70%, A 2 19%, A 3 5%, B 2 3%.

[0175] S3. The electrospun fibers collected in S2 were kept at 280°C in air for 2 h to stabilize the structure of the material, and then calcined at 700°C in an argon atmosphere for 2 h to remove the polystyrene in the fibers and obtain tin-containing multi-channel carbon nanofibers. The electrospun fibers need to be fixed with a splint when heated, and the heating rate is 2°C / min.

[0176] 2. Preparation of lithium-ion batteries

[0177] Same as Example 1.

[0178] Example 5: B 1 , A 1 , A 2 , A 3 , B 2

[0179] 1. Negative electrode sheet structure and preparation method thereof

[0180] (1) Negative electrode structure

[0181] Compared with Example 1, the third transition layer in this example includes an intermediate area.

[0182] The negative electrode sheet (thickness 120μm) includes from bottom to top:

[0183] The first multi-channel carbon nanofiber layer (3% thickness, 24% porosity),

[0184] The first area of ​​the third transition layer (i.e., the high tin area, with a thickness of 60%, a porosity of 23%, and a Sn / C molar ratio of 1:11.3),

[0185] The middle area of ​​the third transition layer (i.e., transition zone, thickness accounts for 28%, porosity is 22%, Sn / C molar ratio is 1:18.3),

[0186] The second region of the third transition layer (i.e., the low tin region, with a thickness of 6%, a porosity of 19%, and a Sn / C molar ratio of 1:37.7)

[0187] The second multi-channel carbon nanofiber layer (3% thickness, 24% porosity).

[0188] (2) Preparation method of negative electrode sheet

[0189] S1. Dissolve 1.2 g of polyacrylonitrile in 10 mL of N,N-dimethylformamide and stir evenly in an oil bath at 60°C. Add 0.7 g of polystyrene and 1.15 g of stannous chloride in turn while stirring. Stir in the oil bath for 12 h to obtain solution A. 1 .

[0190] 1.2 g of polyacrylonitrile was dissolved in 10 mL of N,N-dimethylformamide and stirred evenly in an oil bath at 60 °C. 0.8 g of polystyrene and 0.7 g of stannous chloride (the amount of Sn element was 0.0037 mol and the concentration of stannous chloride was 5.7%) were added in sequence under stirring. The solution A was obtained by stirring in the oil bath for 12 h. 2 .

[0191] 1.2 g of polyacrylonitrile was dissolved in 10 mL of N,N-dimethylformamide and stirred evenly in an oil bath at 60 °C. 0.9 g of polystyrene and 0.35 g of stannous chloride were added in sequence under stirring and stirred in the oil bath for 12 h to obtain solution A. 3 .

[0192] 1.2 g of polyacrylonitrile was dissolved in 10 mL of N,N-dimethylformamide and stirred evenly in an oil bath at 60 °C. 0.9 g of polystyrene was added in sequence under stirring and stirred in the oil bath for 4 h to obtain solution B.

[0193] S2. B, A 1 , A 2 , A 3 , B are electrospun in sequence to obtain B 1 , A 1 , A 2 , A 3 , B 2 The fiber layer is finally prepared to obtain tin-containing electrospun fibers. The electrospinning preparation parameters are the same as those in Example 1. The percentages of the solutions in each layer are: 1 3%, A 1 60%, A 2 28%, A 3 6%, B 2 3%.

[0194] S3. The electrospun fibers collected in S2 were kept at 280°C in air for 2 h to stabilize the structure of the material, and then calcined at 700°C in an argon atmosphere for 2 h to remove the polystyrene in the fibers and obtain tin-containing multi-channel carbon nanofibers. The electrospun fibers need to be fixed with a splint when heated, and the heating rate is 2°C / min.

[0195] 2. Preparation of lithium-ion batteries

[0196] Same as Example 1.

[0197] Example 6: B 1 , A 1 , A 2 , A 3 , A 4 , A 5 , B 2

[0198] 1. Negative electrode sheet structure and preparation method thereof

[0199] (1) Negative electrode structure

[0200] Compared with Example 1, the third transition layer in this example includes three intermediate regions.

[0201] The negative electrode sheet (thickness 120μm) includes from bottom to top:

[0202] The first multi-channel carbon nanofiber layer (3% thickness, 24% porosity),

[0203] The first area of ​​the third transition layer (i.e., the high tin area, with a thickness of 60%, a porosity of 23%, and a Sn / C molar ratio of 1:11.3),

[0204] The first middle area of ​​the third transition layer (i.e., transition zone, thickness accounts for 16%, porosity is 22%, Sn / C molar ratio is 1:13.6),

[0205] The second middle region of the third transition layer (i.e., transition zone, thickness accounts for 8%, porosity is 21%, Sn / C molar ratio is 1:17.0),

[0206] The third middle region of the third transition layer (i.e., transition zone, thickness 6%, porosity 20%, Sn / C molar ratio 1:22.6),

[0207] The second region of the third transition layer (i.e., the low tin region, with a thickness of 4%, a porosity of 19%, and a Sn / C molar ratio of 1:37.7)

[0208] The second multi-channel carbon nanofiber layer (3% thickness, 24% porosity).

[0209] (2) Preparation method of negative electrode sheet

[0210] S1. Dissolve 1.2 g polyacrylonitrile (the amount of substance of the C element is 0.0678 mol) in 10 mL N,N-dimethylformamide, stir evenly in an oil bath at 60°C, add 0.7 g polystyrene and 1.15 g stannous chloride (the amount of substance of the Sn element is 0.006 mol, and the concentration of stannous chloride is 9.2%) in sequence while stirring, and stir in the oil bath for 12 h to obtain solution A. 1 .

[0211] 1.2 g of polyacrylonitrile was dissolved in 10 mL of N,N-dimethylformamide and stirred evenly in an oil bath at 60 °C. 0.8 g of polystyrene and 0.95 g of stannous chloride (the amount of Sn element was 0.005 mol and the concentration of stannous chloride was 7.7%) were added in turn under stirring. The solution A was obtained by stirring in an oil bath for 12 h. 2 .

[0212] 1.2 g of polyacrylonitrile was dissolved in 10 mL of N,N-dimethylformamide and stirred evenly in an oil bath at 60 °C. 0.85 g of polystyrene and 0.75 g of stannous chloride (the amount of Sn element was 0.004 mol and the concentration of stannous chloride was 6.1%) were added in sequence under stirring. The solution A was obtained by stirring in the oil bath for 12 h. 3 .

[0213] 1.2 g of polyacrylonitrile was dissolved in 10 mL of N,N-dimethylformamide and stirred evenly in an oil bath at 60 °C. 0.9 g of polystyrene and 0.6 g of stannous chloride (the amount of Sn element was 0.003 mol and the concentration of stannous chloride was 4.9%) were added in turn under stirring. The solution A was obtained by stirring in an oil bath for 12 h. 4 .

[0214] 1.2 g of polyacrylonitrile was dissolved in 10 mL of N,N-dimethylformamide and stirred evenly in an oil bath at 60 °C. 0.9 g of polystyrene and 0.35 g of stannous chloride (the amount of Sn element was 0.0018 mol and the concentration of stannous chloride was 2.9%) were added in turn under stirring. The solution A was obtained by stirring in an oil bath for 12 h. 5 .

[0215] 1.2 g of polyacrylonitrile was dissolved in 10 mL of N,N-dimethylformamide and stirred evenly in an oil bath at 60°C. 0.9 g of polystyrene was added in sequence under stirring and stirred in the oil bath for 4 h to obtain solution B.

[0216] S2. B, A 1 , A 2 , A 3 , A 4 , A5 , B are electrospun in sequence to obtain B 1 , A 1 , A 2 , A 3 , A 4 , A 5 , B 2 The fiber layer finally prepared the electrospun fiber containing tin. The distance between the electrospinning spinneret and the receiver roller was 15 cm; the voltage was 20 kV; the flow rate was 0.8 mL / h, and the humidity was 18%. The receiver was made of aluminum foil; the electrospinning spinneret width was 12 cm. The percentage of each layer solution was: B 1 3%, A 1 60%, A 2 16%, A 3 8%, A 4 6%, A 5 4%, B 2 3%.

[0217] S3. The electrospun fibers collected in S2 were kept at 280°C in air for 2 h to stabilize the structure of the material, and then calcined at 700°C in an argon atmosphere for 2 h to remove the polystyrene in the fibers and obtain tin-containing multi-channel carbon nanofibers. The electrospun fibers need to be fixed with a splint when heated, and the heating rate is 2°C / min.

[0218] 2. Preparation of lithium-ion batteries

[0219] Same as Example 1.

[0220] Comparative Example 1: A 1 , A 2 , A 3 , A 4 , B 2

[0221] The difference from Example 1 is that there is no first multi-channel carbon nanofiber layer at the bottom layer. Other conditions are the same.

[0222] Comparative Example 2: A 1 , A 2 , A 3 , A 4

[0223] The difference from Example 1 is that there is no first multi-channel carbon nanofiber layer and second multi-channel carbon nanofiber layer, and only the third transition zone. Other conditions are the same.

[0224] Comparative Example 3: A 1

[0225] The difference from Example 1 is that only solution A1 is used for electrospinning, and solution B and A are not used. 2, A 3 , A 4 The solution was electrospun with other conditions being the same.

[0226] Comparative Example 4: B 1 , A 1 , A 2 , B 2

[0227] 1. Negative electrode sheet structure and preparation method thereof

[0228] (1) Negative electrode structure

[0229] Compared with Example 1, this comparative example does not include the middle area.

[0230] The negative electrode sheet (thickness 100 μm) includes from bottom to top:

[0231] The first multi-channel carbon nanofiber layer (3% thickness, 24% porosity),

[0232] The first area of ​​the third transition layer (i.e., the high tin area, with a thickness of 75%, a porosity of 23%, and a Sn / C molar ratio of 1:11.3),

[0233] The second region of the third transition layer (i.e., the low tin region, with a thickness of 19%, a porosity of 19%, and a Sn / C molar ratio of 1:37.7)

[0234] The second multi-channel carbon nanofiber layer (3% thickness, 24% porosity).

[0235] (2) Preparation method of negative electrode sheet

[0236] S1. Dissolve 1.2 g of polyacrylonitrile in 10 mL of N,N-dimethylformamide and stir evenly in an oil bath at 60°C. Add 0.7 g of polystyrene and 1.15 g of stannous chloride in turn while stirring. Stir in the oil bath for 12 h to obtain solution A. 1 .

[0237] 1.2 g of polyacrylonitrile was dissolved in 10 mL of N,N-dimethylformamide and stirred evenly in an oil bath at 60 °C. 0.9 g of polystyrene and 0.35 g of stannous chloride were added in sequence under stirring and stirred in the oil bath for 12 h to obtain solution A. 2 .

[0238] 1.2 g of polyacrylonitrile was dissolved in 10 mL of N,N-dimethylformamide and stirred evenly in an oil bath at 60 °C. 0.9 g of polystyrene was added in sequence under stirring and stirred in the oil bath for 4 h to obtain solution B.

[0239] S2. B, A 1, A 2 , B are electrospun in sequence to obtain B 1 , A 1 , A 2 , B 2 The fiber layer is finally prepared to obtain tin-containing electrospun fibers. The electrospinning preparation parameters are the same as those in Example 1. The percentages of the solutions in each layer are: 1 3%, A 1 75%, A 2 19%, B 2 3%.

[0240] S3. The electrospun fibers collected in S2 were kept at 280°C in air for 2 h to stabilize the structure of the material, and then calcined at 700°C in an argon atmosphere for 2 h to remove the polystyrene in the fibers and obtain tin-containing multi-channel carbon nanofibers. The electrospun fibers need to be fixed with a splint when heated, and the heating rate is 2°C / min.

[0241] 2. Preparation of lithium-ion batteries

[0242] Same as Example 1.

[0243] Comparative Example 5: B 1 , A 1 , B 2

[0244] 1. Negative electrode sheet structure and preparation method thereof

[0245] (1) Negative electrode structure

[0246] Compared with Example 1, the third transition zone in this comparative example only includes the first area, but does not include the second area and the middle area.

[0247] The negative electrode sheet (thickness 96 μm) includes from bottom to top:

[0248] The first multi-channel carbon nanofiber layer (3% thickness, 24% porosity),

[0249] The third transition zone (i.e., high tin zone, thickness accounts for 94%, porosity is 23%, Sn / C molar ratio is 1:11.3),

[0250] The second multi-channel carbon nanofiber layer (3% thickness, 24% porosity).

[0251] (2) Preparation method of negative electrode sheet

[0252] S1. Dissolve 1.2 g of polyacrylonitrile in 10 mL of N,N-dimethylformamide and stir evenly in an oil bath at 60°C. Add 0.7 g of polystyrene and 1.15 g of stannous chloride in turn while stirring. Stir in the oil bath for 12 h to obtain solution A.1 .

[0253] 1.2 g of polyacrylonitrile was dissolved in 10 mL of N,N-dimethylformamide and stirred evenly in an oil bath at 60 °C. 0.9 g of polystyrene was added in sequence under stirring and stirred in the oil bath for 4 h to obtain solution B.

[0254] S2. B, A 1 , B are electrospun in sequence to obtain B 1 , A 1 , B 2 The fiber layer is finally prepared to obtain tin-containing electrospun fibers. The electrospinning preparation parameters are the same as those in Example 1. The percentages of the solutions in each layer are: 1 3%, A 1 94%, B 2 3%.

[0255] S3. The electrospun fibers collected in S2 were kept at 280°C in air for 2 h to stabilize the structure of the material, and then calcined at 700°C in an argon atmosphere for 2 h to remove the polystyrene in the fibers and obtain tin-containing multi-channel carbon nanofibers. The electrospun fibers need to be fixed with a splint when heated, and the heating rate is 2°C / min.

[0256] 2. Preparation of lithium-ion batteries

[0257] Same as Example 1.

[0258] Battery electrochemical performance test:

[0259] The lithium ion batteries prepared in the examples and comparative examples were heated at room temperature at 0.2 A g -1 The current density and the voltage range of 0.01~2.0 V are used for charge and discharge cycles, as follows:

[0260] 1. First Coulomb efficiency:

[0261] Using the Land battery test system, at a constant temperature of 25°C, discharge at a rate of 0.05C to 0.01V, and discharge at a constant current of 20μA to 0V, and record the rate discharge capacity + constant current discharge capacity = first discharge capacity at this time; continue to charge from 0V to 2V at a rate of 0.1C, and record the charging capacity at this time as the first charging capacity; first coulomb efficiency = first charging capacity / first discharge capacity × 100%.

[0262] 2. Capacity retention rate:

[0263] Using the Land battery test system, at a constant temperature of 25°C, discharge at a current density of 200mA / g to 0V, and then charge at a constant current of 200mA / g to 2V. This is a complete charge and discharge cycle, recorded as cycle 1. Repeat this process until the number of cycles is equal to 500, and then end the test.

[0264] The discharge capacity at the 200th cycle is the reversible specific capacity. The discharge specific capacity at the 200th cycle / the discharge specific capacity at the 1st cycle = the capacity retention rate after 200 cycles.

[0265] The discharge capacity at the 500th cycle is the reversible specific capacity. The discharge specific capacity at the 500th cycle / the discharge specific capacity at the 1st cycle = the capacity retention rate after 500 cycles.

[0266] The results are shown in Table 1.

[0267] Table 1 The first coulombic efficiency and capacity retention rate of each group

[0268]

[0269] From the experimental results in Table 1, it can be seen that the first coulombic efficiency of Examples 1 to 6 and Comparative Examples 1 to 5 is between 73% and 87%. This is because an irreversible reaction occurs during the first charge and discharge process to form a stable SEI film, which has a good capacity retention rate in subsequent cycles.

[0270] Examples 1 to 6 include a high tin region, a transition region, and a low tin region. The tin-carbon material with a concentration gradient has better cycle stability, and the multi-channel nanofiber structure can effectively alleviate the volume expansion of Sn during charging and discharging. The multi-channel carbon nanofibers are cross-linked to form a 3D conductive network, which can not only disperse the current density, but also accommodate the deposition of metallic lithium. At the same time, the carbon region and the low tin region can stabilize the structure of the overall self-supporting material, while improving the conductivity. Examples 1 to 6 comprehensively design and construct the concentration gradient region and carbon region of Sn content, which can improve the capacity retention rate and improve the battery cycle stability.

[0271] Compared with Example 1, Comparative Examples 1 and 2 lack one or two layers of multi-channel carbon nanofiber layers. The synergistic effect between the carbon nanofiber framework structure and the uniformly distributed tin in the carbon matrix can effectively accelerate the ion migration rate and reduce the Li + Mechanical stress caused by embedding / de-embedding. The pole piece lacking one or two multi-channel carbon nanofiber layers will expand more in the later stage of cycling and have poor structural stability.

[0272] Compared with Example 1, Comparative Example 3 does not have a tin-carbon material with a concentration gradient difference, nor does it have a multi-channel carbon nanofiber layer, which not only fails to reduce the +The mechanical stress caused by embedding / ejection, the poor flexibility of the material, the rapid capacity decay and the large volume expansion.

[0273] Although comparative examples 1 to 3 have higher capacities, the flexibility of the materials is reduced, the structures are unstable, and the cycle stability is poor.

[0274] Compared with Example 1, Comparative Example 4 has only a low-tin region and a high-tin region, and lacks a transition region between the low-tin region and the high-tin region. Although it has a concentration gradient, the concentration gradient is quite different, and the first coulombic efficiency is low.

[0275] Compared with Example 1, Comparative Example 5 has only a high-tin region, lacks a low-tin region and a transition region, cannot alleviate the volume expansion of Sn during the charge and discharge process, and has a low first coulombic efficiency.

[0276] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A negative electrode sheet, It is characterized in that The negative electrode plate comprises: a first multi-channel carbon nanofiber layer; a second multi-channel carbon nanofiber layer; A third transition layer is disposed between the first multi-channel carbon nanofiber layer and the second multi-channel carbon nanofiber layer, the third transition layer comprises tin and multi-channel carbon nanofibers, and the content of tin in the third transition layer gradually decreases in a direction gradually away from the first multi-channel carbon nanofiber layer; The third transition layer has a first surface close to the first multi-channel carbon nanofiber layer and a second surface disposed opposite to the first surface; The thickness of the negative electrode sheet is recorded as H, the area from the first surface of the third transition layer to the thickness range of 0.6H to 0.7H is recorded as the first area of ​​the third transition layer, and the area from the second surface of the third transition layer to the thickness range of 0.04H to 0.06H is recorded as the second area of ​​the third transition layer; The first region includes a first tin element and a first multi-channel carbon nanofiber, and the first tin element is uniformly distributed in the first multi-channel carbon nanofiber; the second region includes a second tin element and a second multi-channel carbon nanofiber, and the second tin element is uniformly distributed in the second multi-channel carbon nanofiber; the region between the first region and the second region is recorded as an intermediate region, and the intermediate region includes a third tin element and a third multi-channel carbon nanofiber, and the third tin element is uniformly distributed in the third multi-channel carbon nanofiber in the intermediate region; The molar ratio of the first tin element to the first multi-channel carbon nanofiber in the first region is 1:(8-15); The molar ratio of the second tin element to the second multi-channel carbon nanofibers in the second region is 1:(35-40).

2. The negative electrode sheet according to claim 1, It is characterized in that The thickness of the first multi-channel carbon nanofiber layer is 0.02H to 0.04H; The thickness of the second multi-channel carbon nanofiber layer is 0.02H to 0.04H.

3. The negative electrode sheet according to claim 1, It is characterized in that The porosity of the fiber skeleton in the first region is 22% to 23%; The porosity of the fiber skeleton in the second region is 19% to 21%; The porosity of the fiber skeleton of the first multi-channel carbon nanofiber layer or the second multi-channel carbon nanofiber layer is 23% to 24%; The fiber diameter of the fiber skeleton in the first multi-channel carbon nanofiber layer, the second multi-channel carbon nanofiber layer or the third transition layer is 300-400 nm.

4. The negative electrode sheet according to claim 1, It is characterized in that The intermediate region includes m intermediate regions, m≥1; When m≥2, along the direction gradually away from the first multi-channel carbon nanofiber layer, the content of the tin element in the m middle regions gradually decreases, the thickness of the m middle regions gradually decreases, and the porosity of the m middle regions gradually decreases; When m≥2, the intermediate region adjacent to the first region is recorded as the first intermediate region, and the intermediate region adjacent to the second region is recorded as the mth intermediate region; the content of tin element in the first intermediate region is less than the content of tin element in the first region, and the content of tin element in the mth intermediate region is greater than the content of tin element in the second region; the thickness of the first intermediate region is less than the thickness of the first region, and the thickness of the mth intermediate region is greater than the thickness of the second region; the porosity of the fiber skeleton of the first intermediate region is less than the porosity of the fiber skeleton of the first region, and the porosity of the fiber skeleton of the mth intermediate region is greater than the porosity of the fiber skeleton of the second region.

5. A method for preparing a negative electrode sheet according to any one of claims 1 to 4, It is characterized in that The steps include: S1, mixing the carbon source and the solvent, performing a first stirring, and obtaining a carbon source solution after stirring evenly; mixing the tin source, the pore-forming agent and the carbon source solution, and performing a second stirring to obtain solutions with different tin source concentrations, and the solutions with different tin source concentrations are respectively recorded as A and B according to the tin source concentration from high to low. 1 , A 2 ……A n-1 , A n ; n ≥ 3; The carbon source and the solvent are mixed and stirred for a third time to obtain a carbon source solution after being stirred evenly; the pore-forming agent and the carbon source solution are mixed and stirred for a fourth time to obtain a first solution and a second solution without a tin source, wherein the first solution is recorded as B 1 , the second solution is denoted as B 2 ; S2, B 1 , A 1 , A 2 ……A n-1 , A n , B 2 Electrospinning is performed sequentially to prepare a fiber membrane; S3, heating the fiber membrane in an oxygen-containing atmosphere, and then calcining it in an inert gas atmosphere to obtain the negative electrode sheet.

6. The preparation method according to claim 5, It is characterized in that The carbon source includes at least one of polyacrylonitrile, polyvinyl pyrrolidone, polyvinyl alcohol and polyvinylidene fluoride; The solvent includes at least one of N,N-dimethylformamide, N,N-dimethylacetamide, anhydrous ethanol, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, and ethylene carbonate; The tin source includes at least one of stannous chloride and stannous isooctanoate; The pore-forming agent includes at least one of polystyrene, polyvinyl pyrrolidone and polymethyl methacrylate.

7. The preparation method according to claim 5, It is characterized in that The A 1 , A 2 ...A n-1 , A n The content of tin source in the medium gradually decreases; The A 1 The content of tin source in the medium is 9 wt% to 10 wt%; The A 2 To A n-1 The content of tin source in one of the above is 3 wt% to 9 wt%; The A n The content of tin source in the medium is 1 wt% to 3 wt%; The A 1 , A 2 ...A n-1 , A n , B 1 , B 2 The content of the pore-forming agent in the mixture is 5 wt% to 8 wt%.

8. The preparation method according to claim 5, It is characterized in that In step S1, the first stirring, the second stirring, the third stirring or the fourth stirring is stirring under oil bath conditions, the temperature of the oil bath is 60-80° C.; the second stirring time is 8-14 h; the fourth stirring time is 4-6 h; In step S2, the electrospinning conditions are as follows: the distance between the spinneret and the receiver roller is 10-18 cm, the voltage is 10-25 kV, the flow rate is 0.5-1.0 mL / h, the humidity is less than 20%, the receiver is aluminum foil material, and the spinneret width is 10-12 cm.

9. The preparation method according to any one of claims 5 to 8, It is characterized in that In step S3, before the heating treatment, the fiber membrane is also fixed by using a clamping plate; The heating rate of the heating treatment is 2-5°C / min, the holding temperature is 250-300°C, and the holding time is 100-150min; The heating rate of the calcination treatment is 2-5°C / min, the insulation temperature is 600-900°C, and the insulation time is 100-150min.

10. A lithium ion battery, It is characterized in that The lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the negative electrode sheet is the negative electrode sheet described in any one of claims 1 to 4, and / or the negative electrode sheet prepared by the preparation method described in any one of claims 5 to 9.