Lithium metal negative electrode material and preparation method thereof, lithium metal composite negative electrode, lithium ion battery
By using three-dimensional skeleton materials, gradient-distributed inorganic solid electrolytes and surface-distributed high-dielectric materials in lithium metal negative electrode materials, the problem of volume changes and dendrites during charging and discharging of lithium metal negative electrodes is solved, and the ion transmission of batteries is improved Speed and stability optimize the charging and discharging performance of the battery.
Patent Information
- Application Number
- CN202411083260.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-08
AI Technical Summary
The lithium metal negative electrode is prone to volume changes and dendrites during charging and discharging, resulting in a short circuit or thermal runaway from the battery, and the side reaction with the electrolyte affects the stability of the battery, and the prior art affects the ion mobility rate and conductivity, and affects the energy density of the battery.
Using three-dimensional framework materials as carriers, doped with inorganic solid electrolytes and high dielectric materials. By designing the gradient distribution of inorganic solid electrolytes from the inside to the outside, high dielectric materials are distributed on the surface, enhancing the compatibility of electrodes/electrolyte interfaces and improving ionic conductance rate and charge and discharge performance.
The electrode/electrolyte interface compatibility of lithium metal negative electrode material is enhanced, the transmission speed of lithium ions is improved, polarization is reduced, dendrite growth is suppressed, and the charging and discharge performance and stability of the battery is improved.
Smart Images

Figure CN118610467B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of new energy technology, and in particular to a lithium metal negative electrode material and a preparation method thereof, a lithium metal composite negative electrode, and a lithium ion battery. Background Art
[0002] As a battery technology with high energy density potential, lithium metal anode batteries are currently in a rapid development stage. Its theoretical specific capacity is about 3860mAh / g, which is much higher than the commonly used graphite anode, which allows it to match high-voltage positive electrode materials and increase the battery energy density to more than 400Wh / kg. However, there are many problems with lithium metal anodes in practical applications. For example, significant volume changes are likely to occur during the charging and discharging process, and dendrites are easily formed, causing battery short circuits or thermal runaway; side reactions with the electrolyte may lead to the formation of unstable solid electrolyte interface films, affecting battery cycles, etc.
[0003] In the existing technology, the problems of lithium metal negative electrodes are overcome by improving the electrolyte formula, developing artificial SEI layer, designing new host materials and using solid or polymer electrolytes. However, these methods have problems such as affecting the ion migration rate, poor conductivity, and affecting the battery energy density. Summary of the invention
[0004] The purpose of this application is to provide a lithium metal negative electrode material and a preparation method thereof, a lithium metal composite negative electrode, and a lithium ion battery, aiming to solve the problems existing in the prior art.
[0005] To achieve the above objectives, the present application provides a lithium metal negative electrode material, comprising: a three-dimensional skeleton material and an inorganic solid electrolyte and a high dielectric material doped in the three-dimensional skeleton material;
[0006] The doping amount of the inorganic solid electrolyte is distributed in a gradient from more to less in the direction from the inside to the outside of the three-dimensional skeleton material, and the inorganic solid electrolyte includes a first inorganic solid electrolyte doped inside the three-dimensional skeleton material and a second inorganic solid electrolyte doped on the surface of the three-dimensional skeleton material, and the doping amount of the first inorganic solid electrolyte is higher than the doping amount of the second inorganic solid electrolyte;
[0007] The high dielectric material is distributed on the surface of the three-dimensional skeleton material.
[0008] Among them, the three-dimensional skeleton material is a porous structure, the direction from the inside to the outside of the three-dimensional skeleton material refers to the direction from the center of the three-dimensional skeleton material to its outer surface, the surface of the three-dimensional skeleton material refers to the outer surface of the three-dimensional skeleton material, and the inside of the three-dimensional skeleton material refers to the part from the center of the three-dimensional skeleton material to the outer surface, that is, everything except the outer surface is inside the three-dimensional skeleton material.
[0009] It is understandable that the first inorganic solid electrolyte refers to all inorganic solid electrolytes doped in the internal pores of the three-dimensional skeleton material. The first inorganic solid electrolyte can be a doping amount, so that the first inorganic solid electrolyte is evenly distributed inside the three-dimensional skeleton material. The first inorganic solid electrolyte can also be a plurality of doping amounts, for example, it can be two, three, four, five or more kinds, and the first inorganic solid electrolyte with a plurality of doping amounts is also distributed in a gradient from more to less in the direction from the inside to the outside in the three-dimensional skeleton material. The second inorganic solid electrolyte and the high dielectric material are both distributed in the surface pores of the three-dimensional skeleton material. The second inorganic solid electrolyte and the high dielectric material can be distributed in the same surface pores or in different surface pores.
[0010] In some embodiments, the inorganic solid electrolyte satisfies at least one of the following conditions:
[0011] A. The inorganic solid electrolyte includes one or two of LATP and LLTO;
[0012] B. The particle size D50 of the inorganic solid electrolyte is 100nm~2μm;
[0013] C. The specific surface area of the inorganic solid electrolyte is 10 m 2 / g ~50m 2 / g;
[0014] D. The doping amount of the inorganic solid electrolyte is 6%-30% of the mass of the three-dimensional skeleton material, for example, it can be 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30% or any value between 6% and 30%;
[0015] E. The doping amount of the first inorganic solid electrolyte is 5%-20% of the mass of the three-dimensional skeleton material, for example, it can be 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20% or any value between 5% and 20%;
[0016] F. The doping amount of the second inorganic solid electrolyte is 1%-10% of the mass of the three-dimensional skeleton material, for example, it can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or any value between 1% and 10%.
[0017] In some embodiments, the high dielectric material satisfies at least one of the following conditions:
[0018] G. The high dielectric material includes one or more of barium titanate, titanium dioxide, silicon dioxide, magnesium titanate, calcium titanate, aluminum oxide, lithium niobate, and hexagonal boron nitride;
[0019] Preferably, the high dielectric material is barium titanate;
[0020] H. The particle size D50 of the high dielectric material is 100nm~1μm;
[0021] I. The doping amount of the high dielectric material is 1% to 30% of the sum of the mass of the inorganic solid electrolyte and the three-dimensional skeleton material, for example, it can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30% or any value between 1% and 30%. Preferably, the doping amount of the high dielectric material is 3% to 8% of the sum of the mass of the inorganic solid electrolyte and the three-dimensional skeleton material.
[0022] In some embodiments, the three-dimensional skeleton material satisfies at least one of the following conditions:
[0023] J. The three-dimensional skeleton material is in the form of microspheres, and its surface has a porous structure assembled from nanosheets;
[0024] K. The particle size D50 of the three-dimensional skeleton material is 10 μm to 60 μm;
[0025] L. The specific surface area of the three-dimensional skeleton material is 30m 2 / g~200m 2 / g;
[0026] M. The tap density of the three-dimensional skeleton material is 0.2~1g / cm 3 .
[0027] In some embodiments, the lithium metal negative electrode material satisfies at least one of the following conditions:
[0028] N. The particle size D50 of the lithium metal negative electrode material is 20 μm to 60 μm;
[0029] O. The specific surface area of the lithium metal negative electrode material is 40m 2 / g~100m 2 / g;
[0030] P. The ionic conductivity of the lithium metal negative electrode material is 10 -4 S / cm ~10 -3 S / cm.
[0031] The present application also provides a method for preparing the above-mentioned lithium metal negative electrode material, comprising:
[0032] The first polymerized monomer, the second polymerized monomer, the first inorganic solid electrolyte and the dispersant are stirred and mixed in the first water, a catalyst is added to adjust the pH, the mixture is allowed to stand for a first time after stirring, and finally the second inorganic solid electrolyte is added, the mixture is allowed to stand for a second time after stirring, and the mixture is dried to obtain a three-dimensional skeleton material doped with an inorganic solid electrolyte, wherein the mass of the first inorganic solid electrolyte is greater than the mass of the second inorganic solid electrolyte;
[0033] The three-dimensional skeleton material doped with an inorganic solid electrolyte, a high dielectric material and a surfactant or a dispersant are stirred and mixed in the second water to obtain the lithium metal negative electrode material.
[0034] First, the first inorganic solid electrolyte is added to ensure that the three-dimensional skeleton material has a solid electrolyte during the nucleation process. As the three-dimensional skeleton material continues to grow, the first inorganic solid electrolyte is gradually inside the three-dimensional skeleton material. The second inorganic solid electrolyte is added when the morphology of the three-dimensional skeleton material has grown to a relatively fixed state, thereby ensuring that the second inorganic solid electrolyte exists on the surface of the three-dimensional skeleton material.
[0035] If the first inorganic solid electrolyte has a single doping amount, the first inorganic solid electrolyte only needs to be added once; if the first inorganic solid electrolyte has multiple doping amounts, the first inorganic solid electrolyte needs to be added multiple times accordingly.
[0036] By controlling the pH of the solution, the precipitation time of the product can be ensured to be relatively consistent. Under this premise, adding the first inorganic solid electrolyte in multiple times can be, for example, as follows: first add part of the first inorganic solid electrolyte, let it stand for a period of time after stirring evenly, separate, wash with water, collect the first product, and terminate the reaction by washing with water (increasing the pH) so that the three-dimensional skeleton material can no longer grow; disperse the first product in the filtrate, add different amounts of the first inorganic solid electrolyte again, and ensure that the pH is within the range, so as to activate the reaction and allow the three-dimensional skeleton material to continue to grow; as the three-dimensional skeleton material grows, the first inorganic solid electrolyte can be distributed in the skeleton by adding more materials until the first inorganic solid electrolyte is added. Adding the first inorganic solid electrolyte in multiple times can also be as follows: add a catalyst to adjust the pH, stir, let it stand for the first time, and then directly add different amounts of the first inorganic solid electrolyte without separation and washing.
[0037] By controlling the time of each doping reaction of the first inorganic solid electrolyte to be shorter, all the polymerized monomers will not be consumed in each reaction, so that the doping reaction can continue when the subsequent first inorganic solid electrolyte is added.
[0038] In some embodiments, at least one of the following conditions is met:
[0039] a. The mass of the first inorganic solid electrolyte is 1% to 5% of the total mass of the first polymerized monomer and the second polymerized monomer;
[0040] b. The mass of the second inorganic solid electrolyte is 0.1% to 3% of the total mass of the first polymerized monomer and the second polymerized monomer;
[0041] c. The mass of the high dielectric material is 1% to 30% of the mass of the three-dimensional skeleton material doped with the inorganic solid electrolyte.
[0042] In some embodiments, at least one of the following conditions is met:
[0043] (1) The first polymerizable monomer includes one or more of cresol, nonylphenol, urea, melamine, phenol, aralkylphenol, furfuryl alcohol, acrylic acid, phthalic acid, and aniline;
[0044] (2) the second polymerizable monomer includes one or more of formaldehyde, pentamethylenediamine, propylene, acrylonitrile, methacrylic acid, acetaldehyde, and vinyl alcohol;
[0045] (3) the molar ratio of the second polymerizable monomer to the first polymerizable monomer is 1 to 4;
[0046] (4) the mass ratio of the first water to the first polymerizable monomer is 5 to 500;
[0047] (5) The dispersant includes any one of polyacrylate, polyvinyl ester, sodium tripolyphosphate, sodium pyrophosphate, sodium citrate, cellulose, polyvinyl pyrrolidone, polyvinyl alcohol, polycarboxylic acid, and ethanol;
[0048] (6) The catalyst is selected from one or more of hydrochloric acid, formic acid, ammonia water, sulfuric acid, oxalic acid, carbonic acid, citric acid, acetic acid, and sodium hydroxide;
[0049] (7) The pH range is 3 to 5;
[0050] (8) The stirring time is 10-60 min;
[0051] (9) The first standing time is 10-30 minutes;
[0052] (10) The second standing time is 12-24 hours;
[0053] (11) The surfactant includes any one of sodium dodecylbenzene sulfonate, Tween 80, hexadecyltrimethylammonium bromide, ethylene oxide, and sodium hydroxyethyl cellulose;
[0054] (12) The drying temperature is 80°C to 110°C, and the drying time is 12h to 24h.
[0055] This application also provides a lithium metal composite negative electrode, see Figure 1 , wherein the multi-component three-dimensional skeleton material is the lithium metal negative electrode material of the present application, including:
[0056] current collector;
[0057] The above-mentioned lithium metal negative electrode material coated on the surface of the current collector;
[0058] Lithium metal is composited on the surface of the lithium metal negative electrode material.
[0059] The present application also provides a lithium-ion battery, comprising the above-mentioned lithium metal composite negative electrode.
[0060] Compared with the prior art, the beneficial effects of this application include:
[0061] The lithium metal negative electrode material provided in the present application uses a three-dimensional skeleton material as a carrier, and is doped with an inorganic solid electrolyte and a high dielectric material as an ion-conducting material. The inorganic solid electrolyte is designed to be distributed in a gradient from the inside to the outside, with more inside and less outside, and the high dielectric material is distributed on the surface of the three-dimensional skeleton material. The electrode / electrolyte interface compatibility of the lithium metal negative electrode material is enhanced, the material has high ionic conductivity, and the charge and discharge performance of the battery is optimized.
[0062] First, the inorganic solid electrolyte is distributed in a gradient from the inside to the outside of the three-dimensional skeleton material, so that the three-dimensional skeleton material can induce lithium ions to deposit inside the skeleton material during the charge and discharge process, avoiding the accumulation on the outside that causes the growth of dendrites. At the same time, it can increase the transmission speed of lithium ions, reduce polarization, and help the battery charge and discharge at high rates.
[0063] Secondly, the high dielectric material is distributed on the surface of the three-dimensional skeleton material, and polarization will occur under the action of the external electric field, forming a built-in reverse electric field, which helps the dissociation of lithium salts, thereby increasing the concentration of freely moving lithium ions. In addition, the high dielectric material will couple with the electrolyte, providing more lithium ion transmission channels and achieving efficient ion transmission.
[0064] Therefore, under the synergistic effect of the gradient-distributed inorganic solid electrolyte and high dielectric material, the side reaction between lithium metal and electrolyte can be reduced, the growth of dendrites can be inhibited, the stability of the electrode material interface can be improved, and the charge and discharge performance of the battery can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0065] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.
[0066] Figure 1 This is a schematic diagram of the structure of the lithium metal composite negative electrode of the present application;
[0067] Figure 2 This is a surface SEM image of the multi-component three-dimensional skeleton pole piece of Example 1;
[0068] Figure 3 This is a surface SEM image of the multi-component three-dimensional skeleton pole piece of Example 3;
[0069] Figure 4 This is a surface SEM image of the single-component three-dimensional skeleton pole piece of Comparative Example 4;
[0070] Figure 5 The cycle performance results of the full battery assembled in Example 1 and Example 2 are shown;
[0071] Figure 6 The full battery cycle performance result diagram assembled for Example 3, Example 4, Comparative Example 4 and Comparative Example 5;
[0072] Figure 7 This is a graph showing the cycle performance results of the full battery assembled in Example 5;
[0073] Figure 8 This is a graph showing the cycle performance results of the full battery assembled in comparative example 3. DETAILED DESCRIPTION
[0074] As used herein:
[0075] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0076] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0077] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0078] In these examples, parts and percentages are by mass unless otherwise indicated.
[0079] "Mass parts" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass parts of component A are a parts and the mass parts of component B are b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass parts of all components is not limited to 100 parts.
[0080] “And / or” is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0081] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0082] Example 1
[0083] Dissolve 112g urea, 200g formaldehyde, 8.112g 300nm LATP and an appropriate amount of polyvinylpyrrolidone in 500mL water, where LATP accounts for 2.6% of the total mass of monomer one and monomer two. After stirring until completely dissolved, add a certain amount of hydrochloric acid to adjust the pH to 3 and stir evenly, then let it stand for 10 minutes. Finally, add 4g 300nm LATP inorganic solid electrolyte, stir for 30 minutes, let the mixed solution stand for 24h, separate the solid and liquid, wash with water, and dry to obtain a single-component three-dimensional skeleton material, where the yield of the three-dimensional skeleton material is 26%, and LATP accounts for 15% of the mass of the three-dimensional skeleton material. The specific surface area of the material measured by BET is 54m 2 / g, and the particle size D50 measured by Malvern laser particle size analyzer is 24μm.
[0084] Take 4.6975g of a single-component three-dimensional framework material and stir it evenly in water, then add 0.3125g of barium titanate and an appropriate amount of sodium dodecylbenzene sulfonate, stir the mixed solution at room temperature for a certain period of time, filter it, wash it with water, wash it with ethanol, and then dry it to obtain a multi-component mixed three-dimensional framework material, whose ionic conductivity is 3.6×10 -4 S / cm.
[0085] The multi-component mixed three-dimensional skeleton material, SP, CMC, and SBR were mixed in a mass ratio of 80:10:5:5, and a proper amount of water was added to prepare a slurry in a degassing machine. The slurry was then coated on the copper foil with a scraper, and after it was dried, a lithium foil with a thickness of 20 μm was rolled onto the electrode. The total thickness of the electrode was measured by a micrometer and was 52 μm. The surface SEM image of the electrode is as follows: Figure 2 The electrode was cut into discs with a diameter of 12 mm as the negative electrode, and NCM with a diameter of 8.4 mm was used as the positive electrode. 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 was used as the electrolyte to assemble a button-type full battery, and the charge and discharge test was performed on it.
[0086] Example 2
[0087] Dissolve 120.12g urea, 324g formaldehyde, 11.1g 300nm LLTO and appropriate amount of polyvinyl pyrrolidone in 1L water, stir until completely dissolved, add a certain amount of hydrochloric acid to adjust the pH to 3 and stir evenly, then let stand for 10min. Finally, add 2.22g 300nm LLTO inorganic solid electrolyte, stir for 30 minutes, let the mixed solution stand for 24h, separate the solid and liquid, wash with water, and dry to obtain a single-component three-dimensional framework material, in which the doping amount of LLTO accounts for 12% of the mass of the three-dimensional framework material.
[0088] Take 5g of single-component three-dimensional framework material and stir it evenly in water, then add 0.25g of barium titanate and an appropriate amount of ethanol. After stirring the mixed solution at room temperature for a certain period of time, filter it, wash it with water, wash it with ethanol, and then dry it to obtain a multi-component mixed three-dimensional framework material with an ionic conductivity of 6.41×10 -4 S / cm.
[0089] The multi-component mixed three-dimensional skeleton material, SP, CMC, and SBR were mixed in a mass ratio of 80:10:5:5, and a proper amount of water was added to prepare a slurry in a degassing machine. The slurry was then coated on the copper foil with a scraper, and after it was dried, a lithium foil with a thickness of 20 μm was rolled onto the electrode. The total thickness of the electrode was measured by a micrometer and was 52 μm. The surface SEM image of the electrode is as follows: Figure 3 The electrode was cut into discs with a diameter of 12 mm as the negative electrode, and NCM with a diameter of 8.4 mm was used as the positive electrode. 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 was used as the electrolyte to assemble a button-type full battery, and the charge and discharge test was performed on it.
[0090] Example 3
[0091] Dissolve 120.12g urea, 81g formaldehyde, 5.2g 600nm LATP and appropriate amount of sodium citrate in 500mL water, stir until completely dissolved, add a certain amount of hydrochloric acid to adjust the pH to 4 and stir evenly, then let stand for 10min. Finally, add 2.6g 600nm LATP inorganic solid electrolyte, stir for 30 minutes, let the mixed solution stand for 24h, separate the solid and liquid, wash with water, and dry to obtain a single-component three-dimensional framework material. At this time, LATP accounts for 13% of the mass of the three-dimensional framework material, the amount of LATP doped inside the three-dimensional framework material accounts for 10% of the mass of the three-dimensional framework material, and the LATP on the surface accounts for 5% of the mass of the three-dimensional framework material.
[0092] Take 10g of a single-component three-dimensional framework material and stir it evenly in water, then add 0.3g of barium titanate and an appropriate amount of sodium dodecylbenzene sulfonate, stir the mixed solution at room temperature for a certain period of time, filter it, wash it with water, wash it with ethanol, and then dry it to obtain a multi-component mixed three-dimensional framework material.
[0093] The multi-component mixed three-dimensional skeleton material, SP, and LA133 were mixed in a mass ratio of 90:5:5, and an appropriate amount of water was added to prepare a slurry in a degassing machine. The slurry was then coated on a copper foil with a scraper, and after it dried, a lithium foil with a thickness of 20μm was rolled onto the pole piece. The total thickness of the pole piece measured by a micrometer was 52μm. The pole piece was cut into a disc with a diameter of 12mm as the negative electrode, and a button-type full battery was assembled with an NCM with a diameter of 8.4mm as the positive electrode, and 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte, and the charge and discharge test was performed on it.
[0094] Example 4
[0095] The same scheme as in Example 3 was adopted to prepare a single-component three-dimensional skeleton material.
[0096] Take 10g of a single-component three-dimensional framework material and stir it evenly in water, then add 1g of barium titanate and an appropriate amount of polyvinyl pyrrolidone, stir the mixed solution at room temperature for a certain period of time, filter it, wash it with water, wash it with ethanol, and then dry it to obtain a multi-component mixed three-dimensional framework material.
[0097] The multi-component mixed three-dimensional skeleton material, SP, and LA133 were mixed in a mass ratio of 80:10:10, and an appropriate amount of water was added to prepare a slurry in a degassing machine. The slurry was then coated on a copper foil with a scraper, and after it dried, a lithium foil with a thickness of 20μm was rolled onto the pole piece. The total thickness of the pole piece measured by a micrometer was 52μm. The pole piece was cut into a disc with a diameter of 12mm as the negative electrode, and a button-type full battery was assembled with an NCM with a diameter of 8.4mm as the positive electrode, and 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte, and the charge and discharge test was performed on it.
[0098] Example 5
[0099] Dissolve 200g urea, 360g formaldehyde, 16.8g 300nm LATP and appropriate amount of polyvinyl pyrrolidone in 1L water, stir until completely dissolved, add a certain amount of hydrochloric acid to adjust the pH to 3 and stir evenly, then stand for 10min, separate the solid and liquid, collect the filtrate and wash with water. The washed material is dispersed in the above filtrate again, and the solution pH is ensured to be 3, then add 11.2g 300nm LATP, stir evenly and stand for 30min, then add 7g 300nm LATP, stir evenly and stand for 24h, separate the solid and liquid, wash with water, and dry to obtain a single-component three-dimensional framework material, wherein the LATP inside the three-dimensional framework material accounts for 19.2% of the mass of the three-dimensional framework material, and the LATP on the surface of the three-dimensional framework material accounts for 4.8% of the mass of the three-dimensional framework material.
[0100] Take 5g of a single-component three-dimensional framework material and stir it evenly in water, then add 0.25g of barium titanate and an appropriate amount of ethanol. After stirring the mixed solution at room temperature for a certain period of time, filter it, wash it with water, wash it with ethanol, and then dry it to obtain a multi-component mixed three-dimensional framework material.
[0101] The multi-component mixed three-dimensional skeleton material, SP, CMC, and SBR were mixed in a mass ratio of 80:10:5:5, and an appropriate amount of water was added to prepare a slurry in a degassing machine. The slurry was then coated on a copper foil with a scraper, and after it dried, a lithium foil with a thickness of 20 μm was rolled onto the pole piece. The total thickness of the pole piece measured by a micrometer was 52 μm. The pole piece was cut into a disc with a diameter of 12 mm as the negative electrode, and a button-type full battery was assembled with an NCM with a diameter of 8.4 mm as the positive electrode, and 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte, and the charge and discharge test was performed on it.
[0102] Example 6
[0103] Dissolve 200g urea, 360g formaldehyde, 14g 300nm LATP and an appropriate amount of sodium citrate in 1L water, where LATP accounts for 2.5% of the total mass of monomer 1 and monomer 2. After stirring until completely dissolved, add a certain amount of hydrochloric acid to adjust the pH to 3 and stir evenly, then let stand for 10 minutes, separate the solid and liquid, collect the filtrate, and wash with water. Disperse the washed material in the above filtrate again, and ensure that the solution pH is 3, then add 9.8g 300nm LATP, stir evenly and let stand for 10 minutes, separate the solid and liquid again, collect the filtrate, and wash with water. Finally, the above steps were repeated once, and 4.2 g of 300 nm LATP was added, stirred evenly and allowed to stand for 30 min, and then 2.8 g of 300 nm LATP was added, stirred evenly and allowed to stand for 24 h. The solid-liquid separation, water washing and drying were performed to obtain a single-component three-dimensional framework material, wherein the LATP inside the three-dimensional framework material accounted for 19.2% of the mass of the three-dimensional framework material, and the LATP on the surface accounted for 2% of the mass of the three-dimensional framework material.
[0104] Take 5g of a single-component three-dimensional framework material and stir it evenly in water, then add 0.2g of barium titanate and an appropriate amount of ethanol. After stirring the mixed solution at room temperature for a certain period of time, filter it, wash it with water, wash it with ethanol, and then dry it to obtain a multi-component mixed three-dimensional framework material.
[0105] The multi-component mixed three-dimensional skeleton material, SP, CMC, and SBR were mixed in a mass ratio of 80:10:5:5, and an appropriate amount of water was added to prepare a slurry in a degassing machine. The slurry was then coated on a copper foil with a scraper, and after it dried, a lithium foil with a thickness of 20 μm was rolled onto the pole piece. The total thickness of the pole piece measured by a micrometer was 52 μm. The pole piece was cut into a disc with a diameter of 12 mm as the negative electrode, and a button-type full battery was assembled with an NCM with a diameter of 8.4 mm as the positive electrode, and 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte, and the charge and discharge test was performed on it.
[0106] Comparative Example 1
[0107] Dissolve 10g PVDF-HFP in an appropriate amount of NMP solution, stir until completely dispersed, then add 0.5g LATP, 0.5g barium titanate and 1.1g SP, stir in a degassing machine until completely dispersed to prepare a slurry. Then use a scraper to coat the slurry on the copper foil, wait for it to dry, and then roll a 20μm thick lithium foil onto the pole piece. The total thickness of the pole piece measured by a micrometer is 52μm. Cut the pole piece into a 12mm diameter disc as the negative electrode, and use an 8.4mm diameter NCM as the positive electrode, 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte to assemble a button-type full battery, and perform charge and discharge tests on it.
[0108] Comparative Example 2
[0109] Dissolve 112g urea and 200g formaldehyde in 500mL water, stir until completely dissolved, add a certain amount of hydrochloric acid to adjust the pH to 3 and stir evenly, then stand for 24h, separate the solid and liquid, wash with water, and dry to obtain a three-dimensional skeleton material. The tap density of the material is measured to be 0.3g / cm 3 .
[0110] 0.4375g of three-dimensional skeleton material, 0.03125g of 300nm LATP and 0.03125g of barium titanate were physically mixed into a multi-component three-dimensional skeleton material. Then the multi-component mixed three-dimensional skeleton material, SP, CMC, and SBR were mixed in a mass ratio of 83.7:10:1.3:5, and an appropriate amount of water was added to prepare a slurry in a degassing machine. Then the slurry was coated on the copper foil with a scraper, and after it was dried, a lithium foil with a thickness of 20μm was rolled onto the pole piece. The total thickness of the pole piece measured by a micrometer was 52μm. The pole piece was cut into a disc with a diameter of 12mm as the negative electrode, and a button-type full battery was assembled with an NCM with a diameter of 8.4mm as the positive electrode, 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte, and the charge and discharge test was performed on it.
[0111] Comparative Example 3
[0112] Dissolve 120.12g urea, 81g formaldehyde and 10.45g 300nm LLZTO in 500mL water, stir until completely dissolved, add a certain amount of hydrochloric acid to adjust the pH to 4 and stir evenly, then let stand for 10min. Finally, add 2.6g 300nm LLZTO inorganic solid electrolyte, stir for 30 minutes, let the mixed solution stand for 24h, separate the solid and liquid, wash with water, and dry to obtain a single-component three-dimensional framework material.
[0113] Take 10g of a single-component three-dimensional framework material and stir it evenly in water, then add 0.3g of barium titanate and an appropriate amount of sodium dodecylbenzene sulfonate, stir the mixed solution at room temperature for a certain period of time, filter it, wash it with water, wash it with ethanol, and then dry it to obtain a multi-component mixed three-dimensional framework material.
[0114] The multi-component mixed three-dimensional skeleton material, SP, and LA133 were mixed in a mass ratio of 90:5:5, and an appropriate amount of water was added to prepare a slurry in a degassing machine. The slurry was then coated on a copper foil with a scraper, and after it dried, a lithium foil with a thickness of 20μm was rolled onto the pole piece. The total thickness of the pole piece measured by a micrometer was 52μm. The pole piece was cut into a disc with a diameter of 12mm as the negative electrode, and a button-type full battery was assembled with an NCM with a diameter of 8.4mm as the positive electrode, and 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte, and the charge and discharge test was performed on it.
[0115] Comparative Example 4
[0116] The single-component three-dimensional skeleton material was prepared in the same manner as in Example 1.
[0117] The single-component three-dimensional skeleton material, SP, CMC, and SBR were mixed in a mass ratio of 80:10:5:5, and a proper amount of water was added to prepare a slurry in a degassing machine. The slurry was then coated on a copper foil with a scraper, and after drying, a lithium foil with a thickness of 20 μm was rolled onto the electrode. The total thickness of the electrode was measured by a micrometer and was 52 μm. The SEM image of the electrode is shown in the figure below. Figure 4 The electrode was cut into discs with a diameter of 12 mm as the negative electrode, and NCM with a diameter of 8.4 mm was used as the positive electrode. 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 was used as the electrolyte to assemble a button-type full battery, and the charge and discharge test was performed on it.
[0118] Comparative Example 5
[0119] The same scheme as in Example 3 was adopted to prepare a single-component three-dimensional skeleton material.
[0120] Take 10g of a single-component three-dimensional framework material and stir it evenly in water, then add 5g of barium titanate and an appropriate amount of sodium dodecylbenzene sulfonate, stir the mixed solution at room temperature for a certain period of time, filter it, wash it with water, wash it with ethanol, and then dry it to obtain a multi-component mixed three-dimensional framework material.
[0121] The multi-component mixed three-dimensional skeleton material, SP, and LA133 were mixed in a mass ratio of 80:10:10, and an appropriate amount of water was added to prepare a slurry in a degassing machine. The slurry was then coated on a copper foil with a scraper, and after it dried, a lithium foil with a thickness of 20μm was rolled onto the pole piece. The total thickness of the pole piece measured by a micrometer was 52μm. The pole piece was cut into a disc with a diameter of 12mm as the negative electrode, and a button-type full battery was assembled with an NCM with a diameter of 8.4mm as the positive electrode, and 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte, and the charge and discharge test was performed on it.
[0122] The multi-component mixed three-dimensional skeleton materials obtained in the above embodiments and comparative examples were tested for specific surface area and pore size distribution using a Gaobo BK300C specific surface area meter and an American Mack TriStar-3030 pore size analyzer, the particle size range of the samples was tested using a Malvern 3000 laser particle size analyzer, the surface and cross-section SEM of the samples were tested using a Zeiss SEM 460 thermal field emission scanning electron microscope and an Oxford UltimMax170 energy spectrometer, the type and content of the elements doped in the samples were tested using EDS, the electrochemical properties of the samples were tested using a Blue Electric M340A test cabinet, and the battery assembly was carried out in a German Braun glove box.
[0123] The specific button-type full battery is prepared by a method known in the art: NCM polycrystalline is used as the positive electrode, and the pole piece design surface density is 14 mg / cm 2 The multi-component mixed three-dimensional skeleton material pole piece is the negative electrode, and the pole piece design surface density is 1.4mg / cm 2 ; 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 was used as the electrolyte, Celgard2400 was used as the separator, and the shell was a 2016 button battery shell, and the button full battery was assembled. The test conditions were: at room temperature, first using a 0.05C constant rate charge and discharge for two weeks, the voltage range was 2.75-4.2V, and then using a 1C / 5C charge and discharge system for cycling. In all embodiments and comparative examples, the designed gram capacity of the multi-component mixed three-dimensional skeleton material electrode was greater than 2000mAh / g.
[0124] The electrochemical performance test results of each embodiment and comparative example are shown in Table 1. Figures 5 to 8 shown.
[0125] Table 1 Capacity retention rate and pole piece expansion rate of full battery assembled in the embodiment and comparative example after 100 cycles
[0126]
[0127] The test results are shown in Table 1. It can be seen that the expansion rate of the electrode plates using three-dimensional skeleton materials in Example 1, Example 3, Example 4, etc. after cycling is lower than that of the electrode plates using high molecular polymer in Comparative Example 1, and the capacity retention rate after cycling is also higher than that of Comparative Example 1. This shows that the use of three-dimensional skeleton materials can, to a certain extent, avoid direct deposition of lithium metal on the electrode surface, reduce the occurrence of side reactions and the consumption of electrolyte, and thus the capacity retention rate is higher and the expansion is smaller.
[0128] From Table 1, Figure 2 , Figure 5 and Figure 7 It can be seen that the special distribution of inorganic solid electrolyte materials from inside to outside and from more to less in the three-dimensional skeleton material can prevent the agglomeration of inorganic solid electrolyte particles, and at the same time, its good ion conductivity provides a channel for efficient lithium ion transmission. The distribution of BTO on the surface of the three-dimensional skeleton material can, on the one hand, react with the electrolyte first, promote the dissociation of lithium salts, and increase the concentration of freely moving lithium ions; on the other hand, it helps to form a stable SEI on the electrode surface, improve the compatibility of the electrode material and electrolyte interface, and improve the safety of the battery.
[0129] Figure 6 The figure shows the cycle performance of the whole battery under different BTO addition amounts. It can be seen that when the BTO content is too much or too little, the battery cycle performance is not improved. This is because too much BTO will form a higher resistance layer inside the battery, increasing the internal resistance of the battery. At higher charge and discharge rates, too much BTO addition will affect the stability of the electrode and electrolyte interface and affect the migration rate of ions at the interface.
[0130] In addition, not all inorganic solid electrolyte materials and BTO will bring beneficial effects, such as Figure 8 When the inorganic solid electrolyte changes from LATP or LLTO to LLZTO, the battery's cycle performance decays rapidly. This is because LLZTO easily reacts with water and carbon dioxide in the air to generate LiCO3. When the multi-component mixed three-dimensional skeleton material is composited with lithium metal to form a lithium metal negative electrode, the electrode interface will further deteriorate, especially when it is infiltrated by the electrolyte for charging and discharging. It is easy to cause the growth and aggregation of lithium dendrites due to the uneven interface, causing the battery to fail quickly.
[0131] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
[0132] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.
Claims
1. A material for lithium metal negative electrode, characterized in that: include: Three-dimensional framework material and inorganic solid electrolyte and high dielectric material doped in the three-dimensional framework material; The three-dimensional skeleton material is in the form of microspheres, and its surface has a porous structure assembled from nanosheets; The doping amount of the inorganic solid electrolyte is distributed in a gradient from more to less in the direction from the center of the three-dimensional skeleton material to the outer surface thereof, and the inorganic solid electrolyte includes a first inorganic solid electrolyte doped inside the three-dimensional skeleton material and a second inorganic solid electrolyte doped on the outer surface of the three-dimensional skeleton material, and the doping amount of the first inorganic solid electrolyte is higher than the doping amount of the second inorganic solid electrolyte; The high dielectric material is distributed on the outer surface of the three-dimensional skeleton material; The high dielectric material includes barium titanate; The doping amount of the high dielectric material is 1% to 30% of the sum of the mass of the inorganic solid electrolyte and the three-dimensional skeleton material; The inorganic solid electrolyte includes one or two of LATP and LLTO.
2. The material for lithium metal negative electrode according to claim 1, characterized in that The inorganic solid electrolyte satisfies at least one of the following conditions: A. The particle size D50 of the inorganic solid electrolyte is 100nm~2μm; B. The specific surface area of the inorganic solid electrolyte is 10 m 2 / g ~50m 2 / g; C. The doping amount of the inorganic solid electrolyte is 6%-30% of the mass of the three-dimensional skeleton material; D. The doping amount of the first inorganic solid electrolyte is 5%-20% of the mass of the three-dimensional skeleton material; E. The doping amount of the second inorganic solid electrolyte is 1%-10% of the mass of the three-dimensional skeleton material.
3. The material for lithium metal negative electrode according to claim 1, characterized in that The particle size D50 of the high dielectric material is 100 nm to 1 μm.
4. The material for lithium metal negative electrode according to claim 1, characterized in that: The three-dimensional skeleton material satisfies at least one of the following conditions: F. The particle size D50 of the three-dimensional skeleton material is 10 μm to 60 μm; G. The specific surface area of the three-dimensional skeleton material is 30m 2 / g~200m 2 / g; H. The tap density of the three-dimensional skeleton material is 0.2~1g / cm 3 .
5. The material for lithium metal negative electrode according to any one of claims 1 to 4, characterized in that: At least one of the following conditions is met: I. The particle size D50 of the material for the lithium metal negative electrode is 20 μm to 60 μm; J. The specific surface area of the material used for the lithium metal negative electrode is 40m 2 / g~100m 2 / g; K. The ionic conductivity of the material for lithium metal negative electrode is 10 -4 S / cm ~10 -3 S / cm.
6. A method for preparing a material for a lithium metal negative electrode according to any one of claims 1 to 5, characterized in that: include: The first polymerized monomer, the second polymerized monomer, the first inorganic solid electrolyte and the dispersant are stirred and mixed in the first water, a catalyst is added to adjust the pH, the mixture is allowed to stand for a first time after stirring, and finally the second inorganic solid electrolyte is added, the mixture is allowed to stand for a second time after stirring, and the mixture is dried to obtain a three-dimensional skeleton material doped with an inorganic solid electrolyte, wherein the mass of the first inorganic solid electrolyte is greater than the mass of the second inorganic solid electrolyte; The three-dimensional skeleton material doped with an inorganic solid electrolyte, a high dielectric material and a surfactant or a dispersant are stirred and mixed in the second water to obtain the material for the lithium metal negative electrode.
7. The method for preparing a material for a lithium metal negative electrode according to claim 6, characterized in that: At least one of the following conditions is met: a. The mass of the first inorganic solid electrolyte is 1% to 5% of the total mass of the first polymerized monomer and the second polymerized monomer; b. The mass of the second inorganic solid electrolyte is 0.1% to 3% of the total mass of the first polymerized monomer and the second polymerized monomer; c. The mass of the high dielectric material is 1% to 30% of the mass of the three-dimensional skeleton material doped with the inorganic solid electrolyte.
8. The method for preparing a material for a lithium metal negative electrode according to claim 6, characterized in that: At least one of the following conditions is met: (1) The first polymerizable monomer includes one or more of cresol, nonylphenol, urea, melamine, phenol, aralkylphenol, furfuryl alcohol, acrylic acid, phthalic acid, and aniline; (2) the second polymerizable monomer includes one or more of formaldehyde, pentamethylenediamine, propylene, acrylonitrile, methacrylic acid, acetaldehyde, and vinyl alcohol; (3) the molar ratio of the second polymerizable monomer to the first polymerizable monomer is 1 to 4; (4) the mass ratio of the first water to the first polymerizable monomer is 5 to 500; (5) The dispersant includes any one of polyacrylate, polyvinyl ester, sodium tripolyphosphate, sodium pyrophosphate, sodium citrate, cellulose, polyvinyl pyrrolidone, polyvinyl alcohol, polycarboxylic acid, and ethanol; (6) The catalyst is selected from one or more of hydrochloric acid, formic acid, ammonia water, sulfuric acid, oxalic acid, carbonic acid, citric acid, acetic acid, and sodium hydroxide; (7) The pH range is 3 to 5; (8) The stirring time is 10-60 min; (9) The first standing time is 10-30 minutes; (10) The second standing time is 12-24 hours; (11) The surfactant includes any one of sodium dodecylbenzene sulfonate, Tween 80, hexadecyltrimethylammonium bromide, ethylene oxide, and sodium hydroxyethyl cellulose; (12) The drying temperature is 80°C to 110°C, and the drying time is 12h to 24h.
9. A lithium metal composite negative electrode, characterized in that: include: current collector; The material for lithium metal negative electrode according to any one of claims 1 to 5 coated on the surface of the current collector; The lithium metal is composited on the surface of the material for the lithium metal negative electrode.