Application of a metal-organic framework material in liquid phase separation of hexane isomers

Through the application of TJE-4 ultramicroporous metal organic frame material, the high-efficiency liquid phase separation of hexane isomers is achieved through the application of TJE-4 ultramicroporous metal organic frame material, and the high energy consumption and cost in the prior art are solved. The problem of weak selectivity has high adsorption selectivity and thermal stability, which is suitable for industrial applications.

CN118616022BActive Publication Date: 2024-11-12TONGJI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410722449.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-11-12
Estimated Expiration
2044-06-05

AI Technical Summary

Technical Problem

The prior art has problems of high energy consumption, high cost and weak selectivity when separating hexane isomers in liquid phase, making it difficult to achieve efficient and low-cost separation methods, and material stability is also a major challenge.

Method used

Using an ultramicroporous metal organic frame material called TJE-4, the synergistic effect of its periodic three-dimensional pores and electronegative oxygen atoms and trifluoromethyl functional groups can achieve high adsorption and Adsorption of single-branched isomers at the same time, and the dibranched isomers are not adsorbed at all, and separation is carried out in combination with a liquid phase adsorption column and an elution step.

Benefits of technology

It has achieved efficient separation of five hexane isomers, with high adsorption selectivity, low cost and high thermal stability, easy operation, low energy consumption, small equipment investment, and suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118616022B_ABST
    Figure CN118616022B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of new liquid phase adsorption separation materials, and particularly proposes an application of a metal organic framework material in liquid phase separation of hexane isomers. The chemical formula of the metal organic framework material is [Zn4O(tfpc)3] n , wherein Zn represents metal center zinc, TFPC represents organic ligand 3-(trifluoromethyl)-1H-pyrazole-4-carboxylic acid, and the TFPC structural formula is #imgabs0# The metal organic framework material has symmetrical periodic three-dimensional channels, and the surface of the three-dimensional channels is distributed with oxygen atoms and trifluoromethyl functional groups. The present invention aims to efficiently separate hexane isomers with different branching degrees by liquid phase adsorption. The metal organic framework material obtained by the present invention exhibits extremely high adsorption capacity for linear isomers, moderate adsorption for single-branched isomers, and no adsorption for dibranched isomers, and excels in both selectivity and scalability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of new liquid phase adsorption separation materials, in particular to the application of a metal organic framework material in liquid phase separation of hexane isomers. Background Art

[0002] Hexane is an alkane with five isomers, which is widely used in various industrial applications, but is often produced as a mixture. Generally speaking, after catalytic isomerization, the linear isomers [n-hexane (nHEX)] and the monobranched isomers [2-methylpentane (2MP), 3-methylpentane (3MP)] can be used as raw materials for steam cracking to produce important chemicals such as ethylene and propylene. At the same time, n-hexane is also an important solvent in organic synthesis and is used for extraction in the food industry. On the other hand, the two di-branched isomers, 2,3-dimethylbutane (23DMB) and 2,2-dimethylbutane (22DMB), have higher octane numbers (101.7 and 91.8, respectively), and can be used to improve the anti-knock ability of gasoline. Therefore, it is crucial to effectively separate linear / branched isomers and mono-branched / di-branched isomers, as this directly affects the use of these isomers in various industrial applications. At present, the main method for separating hexane isomers is distillation, which is widely used but has high energy consumption and high installation costs. However, efficient adsorptive separation of hexane isomers is a complex challenge due to their chemical inertness and similar physicochemical properties.

[0003] The five isomers of hexane are very similar in physical properties and have molecular sizes ranging from The boiling point is between 49.65 and 68.65°C. Traditional distillation separation methods require high equipment construction costs and energy consumption. At present, direct liquid-phase physical adsorption separation based on porous materials is an emerging technology to reduce the energy consumption of hexane isomer separation. Metal-organic frameworks (MOFs) are a new type of microporous material formed by self-assembly of metal centers and organic ligands. Due to the controllable pore size and pore chemistry, they have good application prospects as an adsorption material in the separation of hexane isomers. At present, MOFs have made certain research progress in this field, but current separation technology still faces a series of problems and challenges. A significant problem is how to maintain good selectivity while achieving high adsorption capacity. For example, the MOF material HIAM-202 reported by Wang et al. The pore size can adsorb a relatively high amount, especially at 30 °C, the adsorption amount of n-hexane reached about 375 mg g -1However, its selectivity for adsorbing the monobranched isomer (2-methylpentane) and dibranched isomer (2,2-dimethylbutane) is relatively weak, with adsorption ratios to n-hexane of only 1.06 and 2.54. On the other hand, the NU-2005 material with stronger sieving ability reported by Omar K. Farha et al. showed extremely low adsorption of dibranched isomer (2,2-dimethylbutane), but was limited by its limited pore volume, and the adsorption capacity for n-hexane was only 104 mg g -1 In addition to the trade-off between adsorption capacity and selectivity, stability is also a key factor that must be considered when designing materials. This is because stability is not only related to the long-term performance of the material, but also plays a decisive role in its production, transportation and performance in practical applications.

[0004] In the prior art, most hexane isomers are separated by gas phase separation, that is, nitrogen is bubbled in a liquid mixture to produce a gaseous mixture, and then the hexane isomers are separated. However, this method has high requirements on equipment, complex operation and high cost.

[0005] Therefore, there is an urgent need to develop a simple, efficient, and low-cost method for separating hexane isomers in the liquid phase, as well as a physical adsorption material that achieves an ideal balance between high stability and separation performance. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides an application of a metal organic framework material in liquid phase separation of hexane isomers, in particular a method for liquid phase separation of hexane isomers. The ultra-microporous metal organic framework material prepared by the present invention exhibits extremely high adsorption of linear isomers, moderate adsorption of single-branched isomers, and no adsorption of dibranched isomers, and has good selectivity and scalability, and can achieve lower-cost separation of hexane isomers.

[0007] The object of the present invention is to provide an application of a metal organic framework material in liquid phase adsorption separation of hexane isomers; the metal organic framework material is named TJE-4, and the chemical formula is [Zn4O(tfpc)3] n , wherein Zn represents metal center zinc, tfpc represents organic ligand 3-(trifluoromethyl)-1H-pyrazole-4-carboxylic acid, and the structural formula of tfpc is n indicates that the metal organic framework material is a polymer.

[0008] In some embodiments of the present invention, the method of application comprises the following steps:

[0009] A1: The metal organic framework material is loaded into the adsorption column and compacted, and a solution containing hexane isomers is passed into the adsorption column at 0-25°C;

[0010] A2: After the metal organic framework material is saturated with adsorption, it is eluted with an organic solvent, and the effluent phases at different time periods are collected to obtain the components of hexane isomers;

[0011] A3: The metal organic framework material used in step A2 is heated and purged with an inert gas to achieve the recycling of the metal organic framework material.

[0012] In some embodiments of the present invention, the hexane isomer is selected from n-hexane, 2-methylpentane, 3-methylpentane, 2,2-dimethylbutane and 2,3-dimethylbutane;

[0013] In some embodiments of the present invention, in step A1, the inner diameter of the adsorption column is 6-10 mm;

[0014] And / or, the total concentration of the solution containing hexane isomers is 0.1 to 5 mol / L.

[0015] and / or, after loading, using mesitylene solution to flow through the adsorption column at a pressure of >0.5 MPa to fully compact the material;

[0016] And / or, the solution containing hexane isomers is pumped into the adsorption column by means of a liquid phase pump, the pumping pressure is greater than 0.5 MPa, and the pumping speed is 0.1 to 0.5 mL·min -1 In this way, the hexane isomers can be fully contacted with the metal organic framework material.

[0017] In some embodiments of the present invention, in steps A2 and A3, the organic solvent is selected from one or more of methanol, ethanol, acetone, and dichloromethane;

[0018] and / or, elution time > 5 minutes;

[0019] And / or, the inert gas is selected from nitrogen and / or helium, and the heating and purging temperature is 100° C. and the time is >5 minutes.

[0020] In some embodiments of the present invention, in step A2, the metal organic framework material preferentially adsorbs and captures linear n-hexane in the mixed gas, and then adsorbs a small amount of single-branched isomers 2-methylpentane and 3-methylpentane, while completely does not adsorb the di-branched isomers 2,2-dimethylbutane and 2,3-dimethylbutane, thereby achieving the separation of hexane isomers with different branching degrees. The 2,2-dimethylbutane and 2,3-dimethylbutane components in the solution containing hexane isomers preferentially penetrate the bed, followed by the single-branched isomers 2-methylpentane and 3-methylpentane, and finally n-hexane.

[0021] In the present invention, the metal organic framework material has symmetrical periodic three-dimensional channels, and electronegative oxygen atoms and trifluoromethyl functional groups are distributed on the surface of the channels.

[0022] In some embodiments of the present invention, the cross-sectional aperture of the three-dimensional channel is The pore size belongs to the ultra-micropore level.

[0023] In the present invention, the metal organic framework material has symmetrical microporous periodic three-dimensional channels, and the narrowest pore size of the channel cross section is The zinc in TJE-4 is 4-coordinated, and the four zinc atoms are coordinated with the central oxygen bridge to form a Zn4O atomic cluster. Subsequently, each zinc forms a coordination bond with one pyrazole N or one carboxylate O from three 3-(trifluoromethyl)-1H-pyrazole-4-carboxylic acid ligands in three perpendicular directions, and no open metal site is formed.

[0024] In some embodiments of the present invention, the method for preparing the metal organic framework material comprises the following steps:

[0025] S1: dissolving an organic ligand 3-(trifluoromethyl)-1H-pyrazole-4-carboxylic acid in an organic solvent, then adding a zinc source and dissolving to obtain a mixed solution;

[0026] S2: transferring the mixed solution obtained in step S1 to a pressure-resistant sealed container and heating the container for reaction. After the reaction is completed, cooling and solid-liquid separation are performed to obtain a homogeneous powder material, and a low-boiling point solvent is used for solvent exchange treatment;

[0027] S3: separating the mixed liquid obtained in step S2 after the low boiling point solvent exchange by solid-liquid separation, and removing the solvent by vacuum drying and heating to obtain the metal organic framework material.

[0028] In some embodiments of the present invention, in step S1, the organic solvent includes methanol and N,N-dimethylacetamide, and the volume ratio of methanol to N,N-dimethylacetamide is 1:0.5-2;

[0029] And / or, the zinc source is selected from Zn(NO3)2; the above zinc sources may be Zn(NO3)2 containing hydrate or not containing hydrate, such as Zn(NO3)2 without crystal water, Zn(NO3)2·4H2O containing crystal water, and Zn(NO3)2·6H2O.

[0030] The molar ratio of the organic ligand 3-(trifluoromethyl)-1H-pyrazole-4-carboxylic acid to the zinc source is 1:1-5.

[0031] In some embodiments of the present invention, in step S1, the dissolution method is a conventional method in the art, and any method can be used as long as it can achieve complete dissolution of the substance referred to in the present invention. Stirring and / or ultrasonic oscillation may be preferred.

[0032] In some embodiments of the present invention, in step S2, the pressure-resistant sealed container is a sealed glass reaction bottle with a polytetrafluoroethylene gasket or a polytetrafluoroethylene-lined reaction kettle;

[0033] And / or, the low boiling point solvent is one or more of methanol, ethanol, dichloromethane or acetone;

[0034] And / or, the exchange treatment lasts for no less than 3 days, and the low boiling point solvent is replaced no less than 4 times during the exchange treatment.

[0035] In some embodiments of the present invention, in step S2, the temperature of the heating reaction is 100-140° C., and the reaction time is 24-48 hours.

[0036] In some embodiments of the present invention, in step S3, the vacuum drying temperature is 70-100° C. and the time is 12-24 hours. The vacuum drying method is used to remove the solvent molecules in the pores of the metal organic framework material as much as possible to achieve activation of the metal organic framework material.

[0037] In some embodiments of the present invention, in steps S2 and S3, the solid-liquid separation is performed by suction filtration, and an organic phase filter membrane or filter paper with a pore size of 0.2 to 5 μm is used in the suction filtration. Furthermore, a suction filtration device such as a Buchner funnel or a sand core filter device is used.

[0038] The above technical solution of the present invention has the following advantages compared with the prior art:

[0039] (1) The metal organic framework material TJE-4 obtained by the present invention has periodic three-dimensional channels, and the pore cross-section diameter of the channel is The pore size is at the ultra-micropore level, and oxygen atom action sites and trifluoromethyl functional groups are distributed on the pore surface. Oxygen atoms and trifluoromethyl groups can form hydrogen bond interactions with n-hexane molecules, and the presence of trifluoromethyl groups can further control the pore size within the kinetic diameter of the dibranched isomer. The synergistic effect of these functional groups leads to the selective adsorption and separation effect of TJE-4 on n-hexane.

[0040] (2) The present invention provides a new method for separating hexane isomers based on liquid phase adsorption of metal organic framework materials. The new ultra-microporous metal organic framework material used in the method has a special pore structure, and the adsorption capacity for linear n-hexane is higher than that for single-branched hexane isomers, while the di-branched isomers are not adsorbed at all. Due to the different molecular configurations of the five isomers, the strength of the hydrogen bonding they are subjected to in the pores is different. Thus, the five isomers with different branching degrees can be efficiently separated.

[0041] (3) In the metal organic framework material obtained by the present invention, Zn coordination is saturated, so there is no open metal site, and the structure can remain stable even in boiling water. In addition, the thermal decomposition temperature of TJE-4 is as high as 450°C, and it has good thermal stability.

[0042] (4) Compared with conventional porous adsorbents, the metal organic framework material used in the present invention has the advantages of high adsorption capacity, excellent desorption performance, repeated regeneration, high adsorption selectivity and low material cost. The material used is simple and safe in preparation, with high yield and basically no by-products.

[0043] (5) Compared with the traditional distillation method or gas phase adsorption separation method, the separation method provided by the present invention has the advantages of mild operating conditions, low energy consumption, and small equipment investment. Therefore, the present invention is expected to bring about an improvement in economic benefits for related petrochemical enterprises. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:

[0045] Figure 1 Schematic diagram of the spatial structure of TJE-4 (view observed along the c-axis of the unit cell);

[0046] Figure 2 The X-ray powder diffraction experimental results of TJE-4 obtained in Examples 1, 2, and 3;

[0047] Figure 3 Thermogravimetric curve of TJE-4 obtained in Example 1;

[0048] Figure 4 The saturated vapor adsorption isotherms of TJE-4 synthesized and activated in Example 1 for five isomers at 30°C;

[0049] Figure 5 The breakthrough curves of TJE-4 synthesized and activated in Example 1 for five equimolar hexane isomers at 25°C;

[0050] Figure 6The breakthrough curves of TJE-4 synthesized and activated in Example 2 for four equimolar hexane isomers at 25°C;

[0051] Figure 7 The breakthrough curves of TJE-4 synthesized and activated in Example 2 at 25°C for five hexane isomers in a molar ratio of 4:1:1:4:4;

[0052] Figure 8 The X-ray powder diffraction experimental results of TJE-4 synthesized in Example 3 and after being treated under various conditions are shown. DETAILED DESCRIPTION

[0053] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0054] Embodiment 1:

[0055] Weigh 810 mg (4.5 mmol) of 3-(trifluoromethyl)-1H-pyrazole-4-carboxylic acid (tfpc) and dissolve it in 30 mL of a mixed solvent of methanol and N,N-dimethylacetamide in a volume ratio of 1:1, and fully dissolve it under ultrasonic vibration. Then, add 1785 mg (6.0 mmol) of Zn(NO3)2·6H2O to the above solution and stir to dissolve. Then transfer the clarified solution to a 50 mL sealed bottle, heat it at 100 ° C for 36 hours, and after cooling, filter it using a glass sand core suction filtration device equipped with an organic phase filter membrane with a pore size of 0.22 μm to obtain a colorless newly synthesized TJE-4 single crystal. In order to obtain TJE-4 with complete solvent removal, the synthesized sample was washed 6 times with 30 mL of fresh methanol within 3 days. Finally, the sample was filtered and dried, and then heated to 150 ° C under vacuum conditions and dried for 12 hours to obtain the activated TJE-4. The spatial structure of the prepared TJE-4 is as follows Figure 1 As shown; TJE-4 was analyzed by X-ray powder diffraction, and the results were consistent with the powder diffraction obtained by analytical structure simulation ( Figure 2 ). Thermogravimetric curves of materials before and after vacuum drying ( Figure 3 ) shows that the material is fully activated and that the thermal stability of the material reaches above 450°C.

[0056] The saturated vapor adsorption isotherms of five hexane isomers were measured on activated TJE-4 at 30°C. Figure 4 As shown in Figure 2, the saturated adsorption capacity of TJE-4 for n-hexane reached 223 mg·g -1 , which is significantly higher than the saturated adsorption capacity (49 mg g) of the single-branched isomers (2-methylpentane and 3-methylpentane). -1 and 37 mg g-1 ), while there was almost no adsorption on the di-branched isomers (2,3-dimethylbutane and 2,2-dimethylbutane), showing extremely high adsorption selectivity.

[0057] 1.8 g of activated TJE-4 was loaded into an 8 mm fixed bed adsorption column for fixed bed penetration experiment. An equimolar solution of five hexane isomers was introduced at room temperature and 4 bar pressure, with a total flow rate of 0.2 mL min -1 The effluent phase was collected from the outlet at different times, and the concentration of each isomer at the outlet was quantitatively analyzed by gas chromatography equipped with a flame ionization detector. The results are shown in Figure 5 After the n-hexane component has completely penetrated, methanol is used to elute the packed column at the same pressure for 5 minutes, and helium is purged at 100°C for 5 minutes to achieve the desorption of the n-hexane component and the regeneration of the adsorbent material.

[0058] Embodiment 2:

[0059] Weigh 180 mg (1 mmol) of 3-(trifluoromethyl)-1H-pyrazole-4-carboxylic acid (tfpc) and dissolve it in 30 mL of a mixed solvent of methanol and N,N-dimethylacetamide in a volume ratio of 1:0.5, and dissolve it fully under ultrasonic vibration. Then, add 1487 mg (5.0 mmol) of Zn(NO3)2·6H2O to the above solution and stir to dissolve. Then transfer the clarified solution to a 50 mL polytetrafluoroethylene-lined reactor, heat it at 140 ° C for 36 hours, and after cooling, filter it using a Buchner funnel equipped with filter paper with a pore size of 5 μm, and then wash it 4 times with 50 mL of fresh ethanol within 3 days. Finally, filter the sample and dry it, then heat it to 70 ° C under vacuum conditions and dry it for 24 hours to obtain the activated TJE-4. The X-ray powder diffraction pattern of the prepared TJE-4 is as shown Figure 2 shown.

[0060] 2 g of activated TJE-4 was loaded into an 8 mm fixed bed adsorption column for a fixed bed penetration experiment. A mesitylene solution of four hexane isomers, 2-methylpentane: 3-methylpentane: 2,2-dimethylbutane: 2,3-dimethylbutane, was introduced at room temperature and 4 bar pressure, where the molar ratio of 2-methylpentane: 3-methylpentane: 2,2-dimethylbutane: 2,3-dimethylbutane was 1:1:1:1, and the total flow rate of the solution was 0.2 mL min -1 The effluent phase was collected from the outlet at different times, and the concentration of each isomer at the outlet was quantitatively analyzed by gas chromatography equipped with a flame ionization detector. The results are shown in Figure 6 shown.

[0061] Example 3

[0062] This example is a set of gram-scale amplified synthesis, as follows: Weigh 18g (0.1mol) 3-(trifluoromethyl)-1H-pyrazole-4-carboxylic acid (tfpc) and dissolve it in 30mL of a mixed solvent of methanol and N,N-dimethylacetamide in a volume ratio of 1:2, and fully dissolve it under ultrasonic vibration. Then, add 29.7g (0.1mol) Zn(NO3)2·6H2O to the above solution and dissolve it by ultrasonic vibration. Then transfer the clarified solution to a 50mL sealed bottle, heat it at 120°C for 3 days, and after cooling, filter it using a Buchner funnel equipped with filter paper with a pore size of 5μm, and then wash it 6 times with 100mL of fresh methanol within 3 days. Finally, filter and dry the sample, heat it to 100°C under vacuum conditions and dry it for 24 hours to obtain the activated TJE-4. The X-ray powder diffraction pattern of the prepared TJE-4 is as follows Figure 2 The weight of TJE-4 after activation was 18.5 g, and the yield (based on ligand tfpc) was 68.4%. TJE-4 was analyzed by X-ray powder diffraction, and the results were consistent with the powder diffraction obtained by analytical structure simulation ( Figure 2 ), proving that the amplified synthesis was successful.

[0063] 2 g of activated TJE-4 was loaded into an 8 mm fixed bed adsorption column for a fixed bed penetration experiment. At room temperature and 4 bar pressure, a mesitylene solution of five hexane isomers, n-hexane: 2-methylpentane: 3-methylpentane: 2,2-dimethylbutane: 2,3-dimethylbutane, was introduced, where the molar ratio of n-hexane: 2-methylpentane: 3-methylpentane: 2,2-dimethylbutane: 2,3-dimethylbutane was 4:1:1:4:4, and the total flow rate of the solution was 0.2 mL min -1 The effluent phase was collected from the outlet at different times, and the concentration of each isomer at the outlet was quantitatively analyzed by gas chromatography equipped with a flame ionization detector. The results are shown in Figure 7 shown.

[0064] Weigh 0.2g of activated TJE-4 and soak it in 20mL of water. Heat it to 100℃ for 3 days in a sealed state, and then place TJE-4 in a vacuum oven at 100℃ for 24h. The X-ray powder diffraction results of TJE-4 did not change during the whole process, and were consistent with the powder diffraction obtained by analytical structure simulation, indicating that TJE-4 has excellent water stability ( Figure 8 ). At the same time, when TJE-4 was heated in air at 100°C for 3 days, or immersed in solvents such as chloroform, dichloromethane, ethanol, methanol, n-hexane, and xylene for 7 days, the X-ray powder diffraction results did not change ( Figure 8 ), which shows that TJE-4 has good thermal stability and good stability in solvents such as chloroform, dichloromethane, ethanol, methanol, n-hexane, and xylene.

[0065] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from them are still within the protection scope of the invention.

Claims

1. Application of a metal organic framework material in liquid phase adsorption separation of hexane isomers; The metal organic framework material is named TJE-4, and its chemical formula is [Zn4O(tfpc)3] n ,in, Zn represents metal center zinc, tfpc represents organic ligand 3-(trifluoromethyl)-1H-pyrazole-4-carboxylic acid, and the structural formula of tfpc is The metal organic framework material has symmetrical and periodic three-dimensional pores, and oxygen atoms and trifluoromethyl functional groups are distributed on the surface of the three-dimensional pores.

2. The use according to claim 1, characterized in that: The cross-sectional aperture of the three-dimensional channel is 3. The use according to claim 1, characterized in that: The method for preparing the metal organic framework material comprises the following steps: S1: dissolving an organic ligand 3-(trifluoromethyl)-1H-pyrazole-4-carboxylic acid in an organic solvent, then adding a zinc source and dissolving to obtain a mixed solution; S2: transferring the mixed solution obtained in step S1 to a pressure-resistant sealed container and heating the container for reaction. After the reaction is completed, cooling and solid-liquid separation are performed to obtain a homogeneous powder material, and a low-boiling point solvent is used for solvent exchange treatment; S3: separating the solid-liquid mixture obtained in step S2 after the low boiling point solvent exchange, and removing the solvent by vacuum drying and heating to obtain the metal organic framework material.

4. The use according to claim 3, characterized in that: In step S1, the organic solvent includes methanol and N,N-dimethylacetamide, and the volume ratio of methanol to N,N-dimethylacetamide is 1:0.5-2; And / or, the zinc source is selected from Zn(NO3)2 or Zn(NO3)2 hydrate; And / or, the molar ratio of the organic ligand 3-(trifluoromethyl)-1H-pyrazole-4-carboxylic acid to the zinc source is 1:1-5.

5. The use according to claim 3, characterized in that: In step S2, the pressure-resistant sealed container is a sealed glass reaction bottle with a polytetrafluoroethylene gasket or a polytetrafluoroethylene-lined reactor; And / or, the low boiling point solvent is one or more of methanol, ethanol, dichloromethane or acetone; And / or, the exchange treatment lasts for no less than 3 days, and the low boiling point solvent is replaced no less than 4 times during the exchange treatment; And / or, the temperature of the heating reaction is 100-140° C., and the reaction time is 24-48 hours.

6. The use according to claim 3, characterized in that: In step S3, the vacuum drying heating temperature is 70-100° C., and the drying time is 12-24 hours.

7. The use according to claim 1, characterized in that: The method of application includes the following steps: A1: The metal organic framework material is loaded into the adsorption column and compacted, and the solution containing hexane isomers is passed into the adsorption column; A2: After the metal organic framework material is saturated with adsorption, it is eluted with an organic solvent, and the effluent phases at different time periods are collected to obtain the components of hexane isomers; A3: The metal organic framework material used in step A2 is heated and purged with an inert gas to achieve the recycling of the metal organic framework material.

8. The use according to claim 7, characterized in that: The hexane isomers include n-hexane, 2-methylpentane, 3-methylpentane, 2,2-dimethylbutane and 2,3-dimethylbutane.

9. The use according to claim 7, characterized in that: In step A1, the inner diameter of the adsorption column is 6-10 mm; and / or, after loading, using mesitylene solution to flow through the adsorption column at a pressure of >0.5 MPa to fully compact the material; and / or, the addition rate of the solution containing hexane isomers is 0.1-0.5 mL·min -1 .

10. The use according to claim 7, characterized in that: In steps A2 and A3, the organic solvent is selected from one or more of methanol, ethanol, acetone and dichloromethane; and / or, elution time > 5 minutes; And / or, the inert gas is selected from nitrogen and / or helium, and the heating and purging temperature is 100-150° C. and the time is >5 minutes.