Environmentally friendly casting release agent for metal casting and preparation method thereof
By combining modified nanomontmorillonite with recovered oil and other components, an environmentally friendly casting release agent with high heat resistance and stability was prepared, which solved the decline in performance and high cost of traditional release agents at high temperatures. The problem of this has realized a green and environmentally friendly casting process.
Patent Information
- Application Number
- CN202411118436.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-15
AI Technical Summary
The existing casting release agents are prone to decomposition at high temperatures, resulting in a decrease in mold release performance, high production costs, and some raw materials are not renewable, which is not conducive to green and environmental protection.
Modified nanomontmorillonite is combined with recovered oil, polycarboxylic acid and other components to prepare an environmentally friendly casting release agent. Through the preparation process of modified nanomontmorillonite, it can improve its heat resistance and stability, and use it Recycling of oil reduces costs.
The casting release agent is achieved with high heat resistance, stability and multiple uses, which reduces production costs, improves the demolding efficiency and surface quality of the castings, and realizes a green and environmentally friendly casting process.
Smart Images

Figure CN118616645B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of casting release agents, and in particular relates to an environmentally friendly casting release agent for metal casting and a preparation method thereof. Background Art
[0002] Demolding is a critical step in the metal casting process. It ensures that the casting can be separated from the mold smoothly and plays a decisive role in the integrity and quality of the casting. In aluminum casting, demoulding technology is particularly important due to the low melting point and high fluidity of aluminum and its alloys. Traditional demoulding methods rely on the use of release agents, which need to have good thermal stability, chemical stability and lubricity to reduce friction between the casting and the mold and prevent adhesion. Therefore, the release agent is directly related to the quality of the casting.
[0003] However, the existing release agents have some defects: for example, unreasonable ratios result in the release agent being unable to form an effective isolation layer on the mold surface, causing problems such as sticking to the board, flash and burrs; during high-temperature casting, the release agent needs to have good thermal stability, while traditional release agents are prone to decomposition or performance degradation at high temperatures, affecting their demolding performance and reducing the number of repeated demolding times; the production cost of traditional release agents is high, and some raw materials are non-renewable, which is not conducive to the concept of green environmental protection. Summary of the invention
[0004] In view of the above situation, in order to overcome the defects of the prior art, the present invention modifies nano-montmorillonite to produce an environmentally friendly casting release agent for metal casting. The agent has good heat resistance and high stability, good dispersibility and wettability on the mold, good demolding effect on the casting, short casting time, high demolding times, and uses recycled oil as raw material, which reduces costs and achieves green environmental protection.
[0005] In order to achieve the above-mentioned purpose, the following technical scheme is adopted: the present invention provides an environmentally friendly casting release agent for metal casting, comprising the following components in weight percentage: 5-10% of recovered oil, 5-10% of dispersant, 3-8% of preservative, 5-15% of silicon nitride powder, 20-30% of polycarboxylic acid, 20-30% of modified nano-montmorillonite, and the balance is water.
[0006] Furthermore, the modified nano-montmorillonite is prepared by the following steps:
[0007] (1) Add diphenyl sulfone compounds and potassium iodide to anhydrous ethanol, heat to reflux, add allyl bromide under stirring, and continue to reflux for 5-10 hours. After the product is washed with deionized water, it is dried, and the obtained product is dissolved in toluene. Then, a hydroxyl-terminated polysiloxane is added, and 0.05 mol / L chloroplatinic acid isopropanol solution is added dropwise. The reaction is heated to 60-80°C and reacted for 8-12 hours. After the reaction is completed, the reaction solution is added to methanol to precipitate, filtered, and the solid is washed with methanol and dried to obtain a polysiloxane containing a sulfone group on the side chain;
[0008] (2) adding the polysiloxane containing sulfone groups on the side chains and ethyl bromodifluoroacetate obtained in step (1) to acetic acid, adding sodium persulfate, reacting for 5-12 hours, and after the reaction is completed, adding 1 mol / L NaOH to adjust the pH to neutral, filtering, washing the solid with deionized water, and drying to obtain a polysiloxane containing sulfone groups and geminal difluoro groups on the side chains;
[0009] (3) dispersing the nano-montmorillonite in an ethanol / water mixed solution with a volume ratio of ethanol to water of 2:1, then adding the polysiloxane containing a sulfone group and a geminal difluoro group in the side chain prepared in step (2), adding sodium hydroxide, stirring for 12-24 hours, centrifuging the solution to separate the solid, and drying to obtain the modified nano-montmorillonite.
[0010] Furthermore, in step (1), the mass ratio of the diphenyl sulfone compound, potassium iodide, anhydrous ethanol, propylene bromide, hydroxyl-terminated polysiloxane, and chloroplatinic acid isopropanol solution is 70-100: 5-8: 180-250: 25-40: 9-18: 2-5.
[0011] Furthermore, in the step (2), the mass ratio of the polysiloxane containing a sulfone group on the side chain, ethyl bromodifluoroacetate, acetic acid, and sodium persulfate is 50-80:30-50:150-200:5-8.
[0012] Furthermore, in step (3), the mass ratio of nano-montmorillonite, ethanol / water mixed solution, polysiloxane containing sulfone group and geminal difluoro group in the side chain, and sodium hydroxide is 35-60:300-600:40-80:2-8.
[0013] Furthermore, the diphenyl sulfone compound is one of 4-hydroxy-4-isopropoxy diphenyl sulfone, 4,4'-dihydroxy diphenyl sulfone, 4-allyloxy-4'-chloro diphenyl sulfone, and 4,4'-bis(4-chloroformylphenoxy) diphenyl sulfone.
[0014] Furthermore, the hydroxyl-terminated polysiloxane is one of hydroxyl-terminated polydimethylsiloxane, polymethylphenylsiloxane, polymethylethylsiloxane and polydiethylsiloxane.
[0015] Furthermore, the preservative is at least one of 1,2-hexanediol, 1,2-cyclopentanediol, and 2,4-pentanediol.
[0016] Furthermore, the recycled oil is at least one of waste engine oil, waste lubricating oil, and waste silicone oil.
[0017] Furthermore, the dispersant is at least one of polyvinyl alcohol, sodium carboxymethyl cellulose, sodium lignin sulfonate and fatty alcohol polyoxyethylene ether.
[0018] On the other hand, the present invention also provides a method for preparing an environmentally friendly casting release agent for metal casting, the preparation method comprising the following steps: mixing the recovered oil, dispersant, and polycarboxylic acid to obtain a mixed liquid, then adding 1 / 3 of water to the mixed liquid, stirring until it becomes a colloid, and then adding the remaining water and preservatives, silicon nitride powder, and modified nano-montmorillonite, and continuing to stir to obtain the environmentally friendly casting release agent.
[0019] The beneficial effects of the present invention are:
[0020] (1) The casting release agent prepared by the present invention has good heat resistance and high stability, good dispersibility and wettability to the mold, good demoulding effect on the casting, short casting time, many demoulding times, and uses recycled oil as raw material, which reduces costs and achieves green environmental protection;
[0021] (2) The present invention introduces sulfone groups and geminal difluoro groups on the side chains of hydroxyl-terminated polysiloxane. The sulfone groups provide polar interactions. The hydrophilicity and polar interactions of the sulfone groups help the release agent to spread evenly on the mold surface and enhance the adhesion between the release agent and the mold surface. The sulfone groups also enhance the lubricity of the release agent and reduce the friction between the mold and the casting, thereby improving the demolding efficiency and the integrity of the casting. The introduction of geminal difluoro groups improves the thermal stability and chemical stability of the release agent, allowing it to maintain good performance under high temperature and chemical environment, thereby increasing the demolding times of the release agent. The geminal difluoro groups have high electronegativity, and their hydrophobicity promotes the rapid evaporation of water, thereby promoting the rapid evaporation of water from the release agent at high temperature, thereby allowing the release agent to form a dense isolation layer, shortening the casting time, reducing the pores, flash and burrs on the surface of the casting, and greatly improving the surface quality and mechanical properties of the casting. Therefore, the combination of the two provides excellent lubricity and demolding performance;
[0022] (3) The hydroxyl groups terminated by polysiloxane are combined with the silanol groups on the nano-montmorillonite to form a cross-linked structure of the nano-montmorillonite, thereby improving the mechanical strength and heat resistance of the release agent, improving the thermal conductivity of the release agent, making the heat more evenly distributed between the mold and the casting, reducing the occurrence of cracking of the isolation layer formed by the release agent, and making the surface of the release agent smoother. The cross-linked structure of montmorillonite also reduces the adsorption of pollutants, helps to keep the mold clean, and affects the rheological properties of the release agent, making it easier to apply evenly during the application process, thereby improving the coverage effect of the release agent.
[0023] (4) The present invention provides basic lubricating properties through the recovery oil, combined with the high wettability, lubricity and good demoulding effect of the modified nano-montmorillonite, so that the demoulding agent can achieve efficient demoulding at a lower dosage, reducing the amount of material used and improving economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The demoulding time and smoothness test results of the demoulding agents prepared in various embodiments and comparative examples of the present invention;
[0025] Figure 2 The adhesion test results of the release agents prepared in various embodiments and comparative examples of the present invention are shown;
[0026] Figure 3 The demoulding resistance test results of the demoulding agents prepared in various embodiments and comparative examples of the present invention are shown;
[0027] Figure 4 The following are the test results of the continuous demoulding times of aluminum solution on the demoulding agents prepared in various embodiments and comparative examples of the present invention.
[0028] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION
[0029] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0030] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.
[0031] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified. Example
[0032] Environmentally friendly casting release agent for metal casting and preparation method thereof
[0033] The environmentally friendly casting release agent comprises the following components in percentage by weight: 5% recycled oil, 5% dispersant, 3% preservative, 5% silicon nitride powder, 20% polycarboxylic acid, 20% modified nano-montmorillonite, and the balance is water.
[0034] The modified nano-montmorillonite is prepared by the following steps:
[0035] (1) Add diphenyl sulfone compounds and potassium iodide to anhydrous ethanol, heat to reflux, add allyl bromide under stirring, and continue to reflux for 5 hours. Wash the product with deionized water and dry it. Dissolve the product in toluene, add hydroxyl-terminated polysiloxane, add 0.05 mol / L chloroplatinic acid isopropanol solution dropwise, heat to 60°C and react for 8 hours. After the reaction is completed, add the reaction solution to methanol to precipitate, filter, wash the solid with methanol, and dry it to obtain polysiloxane containing sulfone groups on the side chain;
[0036] (2) adding the polysiloxane containing sulfone groups on the side chains and ethyl bromodifluoroacetate obtained in step (1) to acetic acid, adding sodium persulfate, reacting for 5 hours, and after the reaction is completed, adding 1 mol / L NaOH to adjust the pH to neutral, filtering, washing the solid with deionized water, and drying to obtain a polysiloxane containing sulfone groups and geminal difluoro groups on the side chains;
[0037] (3) dispersing the nano-montmorillonite in an ethanol / water mixed solution with a volume ratio of ethanol to water of 2:1, then adding the polysiloxane containing a sulfone group and a geminal difluoro group in the side chain prepared in step (2), adding sodium hydroxide, stirring for 12 hours, centrifuging the solution to separate the solid, and drying to obtain the modified nano-montmorillonite.
[0038] In the step (1), the mass ratio of the diphenyl sulfone compound, potassium iodide, anhydrous ethanol, propylene bromide, hydroxyl-terminated polysiloxane, and chloroplatinic acid isopropanol solution is 70:5:180:25:9:2.
[0039] In the step (2), the mass ratio of the polysiloxane containing a sulfone group on the side chain, ethyl bromodifluoroacetate, acetic acid and sodium persulfate is 50:30:150:5.
[0040] In the step (3), the mass ratio of nano-montmorillonite, ethanol / water mixed solution, polysiloxane containing sulfone groups and geminal difluoro groups in the side chain, and sodium hydroxide is 35:300:40:2.
[0041] The diphenyl sulfone compound is 4-hydroxy-4-isopropoxydiphenyl sulfone; the hydroxyl-terminated polysiloxane is hydroxyl-terminated polydimethylsiloxane; the preservative is 1,2-hexanediol; the recovered oil is a mixture of waste engine oil and waste lubricating oil in a mass ratio of 4:1; and the dispersant is polyvinyl alcohol.
[0042] The preparation method of the environmentally friendly casting release agent comprises the following steps: mixing the recovered oil, dispersant and polycarboxylic acid to obtain a mixed liquid, then adding 1 / 3 of water to the mixed liquid, stirring until it becomes a colloid, then adding the remaining water and preservative, silicon nitride powder and modified nano-montmorillonite, and continuing to stir to obtain the environmentally friendly casting release agent. Example
[0043] Environmentally friendly casting release agent for metal casting and preparation method thereof
[0044] The environmentally friendly casting release agent comprises the following components in percentage by weight: 10% of recycled oil, 10% of dispersant, 8% of preservative, 15% of silicon nitride powder, 30% of polycarboxylic acid, 30% of modified nano-montmorillonite, and the balance is water.
[0045] The modified nano-montmorillonite is prepared by the following steps:
[0046] (1) Add diphenyl sulfone compounds and potassium iodide to anhydrous ethanol, heat to reflux, add allyl bromide under stirring, and continue to reflux for 10 hours. After the product is washed with deionized water, it is dried, and the obtained product is dissolved in toluene. Then, a hydroxyl-terminated polysiloxane is added, and 0.05 mol / L chloroplatinic acid isopropanol solution is added dropwise. The reaction is heated to 80°C for 12 hours. After the reaction is completed, the reaction solution is added to methanol to precipitate, filtered, and the solid is washed with methanol and dried to obtain a polysiloxane containing a sulfone group on the side chain.
[0047] (2) adding the polysiloxane containing sulfone groups on the side chains and ethyl bromodifluoroacetate obtained in step (1) to acetic acid, adding sodium persulfate, reacting for 12 hours, and after the reaction is completed, adding 1 mol / L NaOH to adjust the pH to neutral, filtering, washing the solid with deionized water, and drying to obtain a polysiloxane containing sulfone groups and geminal difluoro groups on the side chains;
[0048] (3) dispersing the nano-montmorillonite in an ethanol / water mixed solution with a volume ratio of ethanol to water of 2:1, then adding the polysiloxane containing a sulfone group and a geminal difluoro group in the side chain prepared in step (2), adding sodium hydroxide, stirring for 12-24 hours, centrifuging the solution to separate the solid, and drying to obtain the modified nano-montmorillonite.
[0049] In the step (1), the mass ratio of the diphenyl sulfone compound, potassium iodide, anhydrous ethanol, propylene bromide, hydroxyl-terminated polysiloxane, and chloroplatinic acid isopropanol solution is 100:8:250:40:18:5.
[0050] In the step (2), the mass ratio of the polysiloxane containing a sulfone group on the side chain, ethyl bromodifluoroacetate, acetic acid and sodium persulfate is 80:50:200:8.
[0051] In the step (3), the mass ratio of nano-montmorillonite, ethanol / water mixed solution, polysiloxane containing sulfone groups and geminal difluoro groups in the side chain, and sodium hydroxide is 60:600:80:8.
[0052] The diphenyl sulfone compound is 4,4'-dihydroxydiphenyl sulfone; the hydroxyl-terminated polysiloxane is hydroxyl-terminated polymethylphenylsiloxane; the preservative is 1,2-cyclopentanediol; the recovered oil is a mixture of waste engine oil, waste lubricating oil and waste silicone oil in a mass ratio of 2:1:1; and the dispersant is sodium carboxymethyl cellulose.
[0053] The preparation method of the environmentally friendly casting release agent includes the same steps as those in Example 1. Example
[0054] Environmentally friendly casting release agent for metal casting and preparation method thereof
[0055] The environmentally friendly casting release agent comprises the following components in percentage by weight: 7.5% of recycled oil, 8% of dispersant, 4.5% of preservative, 13% of silicon nitride powder, 24% of polycarboxylic acid, 28% of modified nano-montmorillonite, and the balance is water.
[0056] The modified nano-montmorillonite is prepared by the following steps: (1) adding a diphenyl sulfone compound and potassium iodide to anhydrous ethanol, heating to reflux, adding propylene bromide under stirring, and continuing the reflux reaction for 7 hours after the addition is complete. The product is washed with deionized water and dried. The obtained product is dissolved in toluene, and then a hydroxyl-terminated polysiloxane is added. A 0.05 mol / L chloroplatinic acid isopropanol solution is added dropwise, and the reaction is heated to 70° C. for 10 hours. After the reaction is completed, the reaction solution is added to methanol to precipitate, filtered, and the solid is washed with methanol. After drying, a polysiloxane containing a sulfone group on the side chain is obtained.
[0057] (2) adding the polysiloxane containing sulfone groups on the side chains and ethyl bromodifluoroacetate obtained in step (1) to acetic acid, adding sodium persulfate, reacting for 7 hours, and after the reaction is completed, adding 1 mol / L NaOH to adjust the pH to neutral, filtering, washing the solid with deionized water, and drying to obtain a polysiloxane containing sulfone groups and geminal difluoro groups on the side chains;
[0058] (3) dispersing the nano-montmorillonite in an ethanol / water mixed solution with a volume ratio of ethanol to water of 2:1, then adding the polysiloxane containing a sulfone group and a geminal difluoro group in the side chain prepared in step (2), adding sodium hydroxide, stirring for 12-24 hours, centrifuging the solution to separate the solid, and drying to obtain the modified nano-montmorillonite.
[0059] In the step (1), the mass ratio of the diphenyl sulfone compound, potassium iodide, anhydrous ethanol, propylene bromide, hydroxyl-terminated polysiloxane, and chloroplatinic acid isopropanol solution is 850:6.5:220:35:14:3.5.
[0060] In the step (2), the mass ratio of the polysiloxane containing a sulfone group on the side chain, ethyl bromodifluoroacetate, acetic acid and sodium persulfate is 70:42:165:7.5.
[0061] In the step (3), the mass ratio of nano-montmorillonite, ethanol / water mixed solution, polysiloxane containing sulfone group and geminal difluoro group in the side chain, and sodium hydroxide is 45:450:65:4.5.
[0062] The diphenyl sulfone compound is 4-allyloxy-4'-chlorodiphenyl sulfone; the hydroxyl-terminated polysiloxane is hydroxyl-terminated polymethylethylsiloxane; the preservative is obtained by mixing 1,2-hexanediol, 1,2-cyclopentanediol and 2,4-pentanediol in a mass ratio of 2:1:2; the recovered oil is obtained by mixing waste engine oil, waste lubricating oil and waste silicone oil in a mass ratio of 3:1:2; the dispersant is obtained by mixing polyvinyl alcohol, sodium lignin sulfonate and fatty alcohol polyoxyethylene ether in a mass ratio of 1:1:2.
[0063] The preparation method of the environmentally friendly casting release agent includes the same steps as those in Example 1.
[0064] Comparative Example 1
[0065] The difference between this comparative example and Example 3 is that an equal amount of nano-montmorillonite is used to replace modified nano-montmorillonite in the components of the environmentally friendly casting release agent, and the remaining components, component contents, and preparation process are the same as those in Example 3.
[0066] Comparative Example 2
[0067] The difference between this comparative example and Example 3 is that an equal amount of polysiloxane containing sulfone groups in the side chain is used to replace the polysiloxane containing sulfone groups and geminal difluoro groups in the components of the environmentally friendly casting release agent, and reacts with nano-montmorillonite to obtain modified nano-montmorillonite. The remaining components, component contents, and preparation process are the same as those in Example 3.
[0068] Results Analysis
[0069] Experimental Example 1
[0070] Demolding time and smoothness test of release agent
[0071] The release agents prepared in each embodiment and comparative example were subjected to 30 demoulding tests respectively, and were classified into three types according to the results: smooth demoulding with short time, smooth demoulding with long time, and demoulding with stuck phenomenon and long time. The test results are shown in Figure 1 .
[0072] From the test results, it can be seen that the demolding of the release agents prepared in Examples 1-3 of the present invention is smooth and the demolding is short, and there is no jamming phenomenon or long demolding time, which proves that the demolding time is short and the demolding is smooth. The release agents of Examples 1-3 are better than those of Comparative Examples 1-2 in terms of smooth demolding and short time, indicating that the release agents of the present invention have better demolding performance, and that the heat resistance, stability, dispersibility and wettability of the release agents prepared by the present invention are better than those of the comparative examples.
[0073] Experimental Example 2
[0074] Release agent adhesion test
[0075] A test piece (8407 alloy steel) with a size of 20mm×20mm was air-fired at 200℃ for 30min, then a release agent was applied to the test piece, and it was baked at 350℃ for 30min, and then air-cooled. The mass of the test piece was measured, and the adhesion amount was calculated from the difference in mass before and after the test. The adhesion amount was used as the evaluation standard for evaluating the adhesion of the release agent. The results are shown in Figure 2 .
[0076] It can be seen from the test results that the amount of release agent attached to the present invention is small, which indicates that no excessive release agent will remain during the demolding process. Combined with the test results of Experimental Example 1, it can be seen that the release agent prepared by the present invention can achieve better demolding effect with a small amount.
[0077] Experimental Example 3
[0078] Release agent demoulding resistance test
[0079] Heat the 8407 alloy steel test plate to 450℃, apply the release agent to the test plate using a vertically set spray device in front of the test plate, place the test plate on the test machine stand and ensure that it is placed horizontally, place a ring mold in the center of the test plate, inject aluminum melt (ADC-12, temperature 650℃) into the mold, continue to cool the test plate for 40s after cooling and solidifying, then slowly place weights on the solidified aluminum melt, use the Imada SVZ-200NB-50R3 tensile testing machine, stretch the test plate together with the aluminum melt and the weights in the X direction, and measure the demoulding resistance through the tensiometer of the tensile testing machine during the stretching process. The test results are shown in Figure 3 .
[0080] The test results show that the demolding resistance of Examples 1-3 is relatively small, indicating that the present invention reduces the friction between the mold and the casting by introducing sulfone groups and geminal difluoro groups on the side chains of the hydroxyl-terminated polysiloxane, thereby improving the demolding efficiency of the aluminum casting process.
[0081] Experimental Example 4
[0082] Test on the number of continuous demoulding of aluminum solution on the release agent
[0083] Apply the release agent to the cleaned mold, then inject aluminum melt (ADC-12, temperature 650℃) into the mold, let it cool and solidify for 45s, and continuously mold on the mold. When the casting sticks to the mold or cannot be easily removed from the mold, the process ends. Record the number of continuous demolding of the aluminum solution on the release agent. The test results are shown in Figure 4 .
[0084] It can be seen from the test results that Examples 1-3 have more demolding times, which indicates that the release agent prepared by the present invention has excellent reusability. This is related to the improved mechanical strength and heat resistance formed by the cross-linking structure formed by the combination of the hydroxyl groups terminated by polysiloxane and the silanol groups on the nano-montmorillonite, and is also related to the high lubricity and thermal stability of the release agent.
[0085] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
[0086] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.
Claims
1. An environmentally friendly casting release agent for metal casting, characterized in that: The invention comprises the following components in weight percentage: 5-10% of recovered oil, 5-10% of dispersant, 3-8% of preservative, 5-15% of silicon nitride powder, 20-30% of polycarboxylic acid, 20-30% of modified nano-montmorillonite, and the balance of water; The modified nano-montmorillonite is prepared by the following steps: (1) Add diphenyl sulfone compounds and potassium iodide to anhydrous ethanol, heat to reflux, add allyl bromide under stirring, and continue to reflux for 5-10 hours. After the product is washed with deionized water, it is dried, and the obtained product is dissolved in toluene. Then, a hydroxyl-terminated polysiloxane is added, and 0.05 mol / L chloroplatinic acid isopropanol solution is added dropwise. The reaction is heated to 60-80°C and reacted for 8-12 hours. After the reaction is completed, the reaction solution is added to methanol to precipitate, filtered, and the solid is washed with methanol and dried to obtain a polysiloxane containing a sulfone group on the side chain; (2) adding the polysiloxane containing sulfone groups on the side chains and ethyl bromodifluoroacetate obtained in step (1) to acetic acid, adding sodium persulfate, reacting for 5-12 hours, and after the reaction is completed, adding 1 mol / L NaOH to adjust the pH to neutral, filtering, washing the solid with deionized water, and drying to obtain a polysiloxane containing sulfone groups and geminal difluoro groups on the side chains; (3) dispersing the nano-montmorillonite in an ethanol / water mixed solution with a volume ratio of ethanol to water of 2:1, then adding the polysiloxane containing a sulfone group and a geminal difluoro group in the side chain prepared in step (2), adding sodium hydroxide, stirring for 12-24 hours, centrifuging the solution to separate the solid, and drying to obtain the modified nano-montmorillonite.
2. The environmentally friendly casting release agent for metal casting according to claim 1, characterized in that: In the step (1), the mass ratio of the diphenyl sulfone compound, potassium iodide, anhydrous ethanol, propylene bromide, hydroxyl-terminated polysiloxane, and chloroplatinic acid isopropanol solution is 70-100: 5-8: 180-250: 25-40: 9-18: 2-5.
3. The environmentally friendly casting release agent for metal casting according to claim 2, characterized in that: In the step (2), the mass ratio of the polysiloxane containing a sulfone group on the side chain, ethyl bromodifluoroacetate, acetic acid and sodium persulfate is 50-80:30-50:150-200:5-8.
4. The environmentally friendly casting release agent for metal casting according to claim 3, characterized in that: In the step (3), the mass ratio of nano-montmorillonite, ethanol / water mixed solution, polysiloxane containing sulfone group and geminal difluoro group in the side chain, and sodium hydroxide is 35-60:300-600:40-80:2-8.
5. The environmentally friendly casting release agent for metal casting according to claim 4, characterized in that: The diphenyl sulfone compound is one of 4-hydroxy-4-isopropoxy diphenyl sulfone, 4,4'-dihydroxy diphenyl sulfone, 4-allyloxy-4'-chloro diphenyl sulfone and 4,4'-bis(4-chloroformylphenoxy) diphenyl sulfone.
6. The environmentally friendly casting release agent for metal casting according to claim 5, characterized in that: The hydroxyl-terminated polysiloxane is one of hydroxyl-terminated polydimethylsiloxane, polymethylphenylsiloxane, polymethylethylsiloxane and polydiethylsiloxane.
7. The environmentally friendly casting release agent for metal casting according to claim 6, characterized in that: The preservative is at least one of 1,2-hexanediol, 1,2-cyclopentanediol and 2,4-pentanediol.
8. The environmentally friendly casting release agent for metal casting according to claim 7, characterized in that: The recycled oil is at least one of waste engine oil, waste lubricating oil and waste silicone oil.
9. The environmentally friendly casting release agent for metal casting according to claim 8, characterized in that: The dispersant is at least one of polyvinyl alcohol, sodium carboxymethyl cellulose, sodium lignin sulfonate and fatty alcohol polyoxyethylene ether.
10. A method for preparing an environmentally friendly casting release agent for metal casting according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: mixing the recovered oil, dispersant and polycarboxylic acid to obtain a mixed liquid, then adding 1 / 3 of water to the mixed liquid, stirring until it becomes a colloid, then adding the remaining water and a preservative, silicon nitride powder and modified nano-montmorillonite, and continuing to stir to obtain the environmentally friendly casting release agent.