A kind of nanometer cesium tungsten oxide and its preparation process and application
By reacting with a reducing surfactant in aqueous ethanol solution and insulated in organic solvents, the problem of long reaction time and insufficient size in the preparation of cesium tungsten bronze powder was solved, and a nanotungsten oxide with fine particle size and uniform particle size was prepared. Cesium, improves its performance in thermal insulation coatings, especially in terms of aging resistance and light shielding effects.
Patent Information
- Application Number
- CN202411103382.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-13
AI Technical Summary
In the prior art, the preparation method of cesium tungsten bronze powder has problems such as long reaction time, insufficient utilization of organic matter, and insufficient powder size. It lacks test data on the performance of cesium tungsten bronze powder, and its comprehensive performance cannot be effectively evaluated. .
The tungsten source and cesium source react with a reducing surfactant in an aqueous ethanol solution to form a precursor, and then insulated in an organic solvent to control the temperature and time to generate nanotungsten cesium oxide with fine particle size and uniform particle size to improve its Aging resistance and light shielding effect in thermal insulation coatings.
It realizes the efficient preparation of nanotungsten cesium oxide, has good aging resistance and light shielding effect, improves raw material utilization, and provides detailed performance test data to evaluate its comprehensive performance.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal compounds, and in particular relates to nano cesium tungsten oxide and a preparation process and application thereof. Background Art
[0002] With the rapid development of my country's economy and society, people have more and more requirements for glass windows. The thermal insulation performance of large-area ordinary glass is very poor and cannot meet people's demand for glass. At present, building energy-saving glass mainly includes the following types: (1) low-radiation energy-saving glass; (2) low-conductivity energy-saving glass; (3) transparent thermal insulation coating glass; and the nano-oxide materials used in transparent thermal insulation coatings are mostly conductive oxides, such as the commonly used antimony tin oxide and indium tin oxide. At present, tungsten bronze nanomaterials are emerging and widely used high-performance transparent thermal insulation materials because of their good ability to transmit visible light, shield infrared rays and absorb ultraviolet rays. They have important research significance in the field of building energy-saving glass.
[0003] In addition, the currently disclosed patents mainly use high-temperature solid-phase reaction, hydrothermal synthesis and other methods to prepare cesium tungsten bronze powder. In the hydrothermal synthesis method, the size of cesium tungsten bronze powder can be adjusted by adding organic matter, but because the entire reaction process is mainly carried out in an aqueous solution, there will be problems such as long reaction time, insufficient utilization of organic matter, and insufficient size of cesium tungsten bronze powder. The patent application with patent announcement number CN117566797A discloses a method for preparing ultrafine cesium tungsten bronze powder. The invention mixes tungsten source, cesium source and organic solvent, and keeps them warm at 80-150°C to form a uniform solution, and then reacts at 100-300°C to obtain cesium tungsten bronze powder with a particle size range or thickness range of 5-10nm and uniform size. The patent application with patent announcement number CN117049600A discloses a method for preparing nano-cesium tungsten bronze, which includes the following steps: preparation of tungsten source solution, preparation of cesium source solution, coprecipitation, sand milling to obtain cesium tungsten bronze precursor solution; spray drying the precursor solution to obtain cesium tungsten bronze precursor powder; and heat treatment to obtain cesium tungsten bronze nanopowder. Although these two invention patents disclose the preparation of cesium tungsten bronze powder, there is a lack of performance test data for cesium tungsten bronze powder, and it is impossible to evaluate the comprehensive performance of cesium tungsten bronze powder, which has no reference significance for the practical application of cesium tungsten bronze powder in life.
[0004] Based on the problems existing in the prior art, developing a method for efficiently preparing cesium tungsten bronze nanopowder is of great significance to people's lives and actual industrial production. Summary of the invention
[0005] In order to solve the above-mentioned technical problems, the present invention provides a nano-cesium tungsten oxide and its preparation process and application. The nano-cesium tungsten oxide obtained by the preparation process has a small and uniform particle size. When used in coatings, the coatings can have better aging resistance and better shielding effects on 550nm and 950nm light.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0007] The first aspect of the present invention provides a preparation process of nano-cesium tungsten oxide, comprising the following preparation steps:
[0008] (1) placing a tungsten source and a cesium source in an ethanol aqueous solution, adding a reducing surfactant thereto, reacting in a sealed container at 75-85°C for 2-3 hours, and drying to obtain a precursor;
[0009] (2) The precursor obtained in step (1) is placed in a mixed solvent, stirred for 1-2 hours, then kept warm in a reactor, cooled to room temperature, washed, and dried to obtain nano-cesium tungsten oxide.
[0010] The preparation steps of the reducing surfactant are:
[0011] Dispersing 2,3-dihydroxypropylamine and dodecyltrimethylammonium bromide in anhydrous ethanol at a molar ratio of 1:(2-2.3), stirring and reacting at 75-85° C. for 6-9 hours, rotary evaporating, separating, and drying to obtain a reducing surfactant;
[0012] The amount of the reducing surfactant is 5-25wt% of the tungsten source;
[0013] The mixed solvent comprises oleic acid and isobutanol in a mass ratio of (48-53):1; the ratio of the mass of the precursor in step (2) to the volume of the mixed solvent is 1 g:(4.5-5.5) mL;
[0014] The tungsten source is one or more of tungsten chloride, sodium tungstate and ammonium tungstate;
[0015] The cesium source is one or more of cesium carbonate, cesium hydroxide, cesium sulfate and cesium nitrate.
[0016] In some embodiments, the concentration of the ethanol aqueous solution is 90-95 wt %.
[0017] In some embodiments, the molar ratio of tungsten element to cesium element in the tungsten source and the cesium source is (2-4):1.
[0018] Preferably, the molar ratio of tungsten element to cesium element in the tungsten source and the cesium source is (3-4):1.
[0019] In some embodiments, the reducing surfactant is used in an amount of 15 wt % of the tungsten source.
[0020] In some embodiments, the mixed solvent comprises oleic acid and isobutanol in a mass ratio of 51:1; and the ratio of the mass of the precursor to the volume of the mixed solvent in step (2) is 1 g:5 mL.
[0021] In some embodiments, the insulation temperature is 210-250° C., and the insulation time is 2-4 hours.
[0022] Preferably, the insulation temperature is 220-240° C., and the insulation time is 3-4 hours.
[0023] The second aspect of the present invention provides a nano-cesium tungsten oxide obtained by the above-mentioned preparation process, wherein the average particle size of the nano-cesium tungsten oxide is 10-30nm.
[0024] The second aspect of the present invention provides an application of the above-mentioned nano-cesium tungsten oxide in the field of thermal insulation coatings.
[0025] The invention adopts an ethanol aqueous solution with a certain mass fraction as a reaction solvent, and adds a tungsten source, a cesium source and a certain amount of reducing surfactant therein, so that the tungsten source and the cesium source form a precursor with uniform texture in the solvent, and then the precursor is subjected to heat preservation reaction in an organic solvent to obtain nano-tungsten cesium oxide with fine and uniform particle size. The nano-tungsten cesium oxide has high comprehensive performance and extremely high raw material utilization rate in the preparation process.
[0026] The present invention first fully mixes the tungsten source, the cesium source and the reducing surfactant in a closed container at 75-85°C to form a uniform solution, which can ensure that an easily soluble precursor is obtained after drying, and adds a synthetic reducing surfactant thereto, which is obtained by reacting 2,3-dihydroxypropylamine and dodecyltrimethylammonium bromide. It can significantly reduce the aggregation force between particles, promote the dispersion of the tungsten source and the cesium source in the solvent, regulate the structure of the precursor, and is conducive to the subsequent generation of nano-tungsten cesium oxide. The liquid solvent is then removed by drying to avoid the generation of some impurities in the subsequent reaction process. The obtained precursor is then dissolved in an organic solvent composed of isobutanol and oleic acid, and the precursor can be well dispersed in the organic solvent. Isobutanol and oleic acid can produce a synergistic effect to prevent the precursor from excessively agglomerating and causing the nano-tungsten cesium oxide particle size to be too large, and further regulate the size and dispersion of the tungsten cesium oxide. This is because cesium ions can be evenly dispersed in the tungsten source in the organic solvent system. In the process of tungsten source forming a crystal lattice, the cesium ions dispersed therein can be in-situ filled in the tungsten oxide lattice to form grains with stable structure, small interaction force and easy dispersion. The crystal nucleation rate and crystal particle size can be controlled by controlling the insulation temperature and duration, thereby improving the aging resistance and light shielding effect of nano-tungsten oxide cesium.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] 1. The present invention selects a specific tungsten source and a cesium source, and fully mixes the tungsten source, the cesium source and the synthesized reducing surfactant in an ethanol aqueous solution in a closed container at a certain temperature, and then dries to form a precursor with uniform texture, which is conducive to the subsequent generation of nano-tungsten cesium oxide. The precursor is then dissolved in an organic solvent composed of isobutanol and oleic acid, and the crystal nucleation rate and crystal particle size are controlled by controlling the insulation temperature and duration to generate nano-tungsten cesium oxide with fine particle size and uniform texture. The preparation method of the present invention has a higher raw material utilization rate, and the prepared nano-tungsten cesium oxide has good aging resistance and light shielding effect.
[0029] 2. The present invention prepares a reducing surfactant, which is used in the preparation process of nano-cesium tungsten oxide, and can significantly improve the aging resistance and light shielding effect of nano-cesium tungsten oxide. DETAILED DESCRIPTION
[0030] Now, various exemplary embodiments of the present invention are described in detail, which should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not used to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges may be independently included or excluded in the range. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as commonly understood by conventional technicians in the field of the present invention. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. Without departing from the scope or spirit of the present invention, various modifications and changes can be made to the specific embodiments of the present invention specification, which will be obvious to those skilled in the art. Other embodiments obtained from the description of the present invention will be obvious to technicians. The present application description and examples are exemplary only.
[0031] The words “include,” “including,” “have,” or “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0032] The tungsten source used in the present invention is ammonium tungstate; the cesium source used is cesium nitrate.
[0033] The steps for preparing the reducing surfactant used in Examples 1-9 and Comparative Examples 1 and 2 are as follows:
[0034] Disperse 0.1 mol of 2,3-dihydroxypropylamine and 0.22 mol of dodecyltrimethylammonium bromide in 250 mL of anhydrous ethanol, stir and react at 80°C for 8 h, remove the anhydrous ethanol by rotary evaporation at 40°C, add 100 mL of deionized water for extraction, shake well and let stand for 15 min, take the supernatant, pass it through a chromatography column, and freeze-dry to obtain a reducing surfactant.
[0035] Example 1
[0036] A preparation process of nano-cesium tungsten oxide comprises the following preparation steps:
[0037] (1) 20 g of tungsten source and 5.91 g of cesium source were placed in 100 mL of 90 wt% ethanol aqueous solution, 1 g of reducing surfactant was added thereto, and the mixture was reacted at 75 °C for 3 h in a sealed container at a stirring speed of 500 r / min, and then dried at 60 °C for 10 h to obtain a precursor;
[0038] (2) 10 g of the precursor obtained in step (1) was placed in 45 mL of a mixed solvent, stirred at 500 r / min for 2 h, then kept at 220 ° C for 4 h in a polytetrafluoroethylene reactor, cooled to room temperature, washed with cyclohexane and anhydrous ethanol for 3 times, and dried at 60 ° C for 10 h to obtain nano-cesium tungsten oxide.
[0039] The mixed solvent used was composed of oleic acid and isobutanol in a mass ratio of 48:1;
[0040] The particle size of the nano-cesium tungsten oxide in this embodiment ranges from 24 to 30 nm.
[0041] Example 2
[0042] A preparation process of nano-cesium tungsten oxide comprises the following preparation steps:
[0043] (1) 20 g of tungsten source and 4.43 g of cesium source were placed in 100 mL of 95 wt% ethanol aqueous solution, 5 g of reducing surfactant was added thereto, and the mixture was reacted at 85 °C for 2 h in a sealed container at a stirring speed of 700 r / min, and then dried at 60 °C for 10 h to obtain a precursor;
[0044] (2) 10 g of the precursor obtained in step (1) was placed in 55 mL of a mixed solvent, stirred at 700 r / min for 1 h, then kept at 250 ° C for 3 h in a polytetrafluoroethylene reactor, cooled to room temperature, washed with cyclohexane and anhydrous ethanol for 3 times, and dried at 60 ° C for 10 h to obtain nano-cesium tungsten oxide.
[0045] The mixed solvent used was composed of oleic acid and isobutanol in a mass ratio of 53:1.
[0046] The particle size of the nano-cesium tungsten oxide in this embodiment ranges from 14 to 20 nm.
[0047] Example 3
[0048] A preparation process of nano-cesium tungsten oxide comprises the following preparation steps:
[0049] (1) 20 g of tungsten source and 5.07 g of cesium source were placed in 100 mL of 93 wt% ethanol aqueous solution, 3 g of reducing surfactant was added thereto, and the mixture was reacted at 80 °C for 2.5 h in a sealed container at a stirring speed of 600 r / min, and then dried at 60 °C for 10 h to obtain a precursor;
[0050] (2) 10 g of the precursor obtained in step (1) was placed in 50 mL of a mixed solvent, stirred at 600 r / min for 1.5 h, then kept warm at 235 ° C for 3.5 h in a polytetrafluoroethylene reactor, cooled to room temperature, washed with cyclohexane and anhydrous ethanol for 3 times, and dried at 60 ° C for 10 h to obtain nano-cesium tungsten oxide.
[0051] The mixed solvent used was composed of oleic acid and isobutanol in a mass ratio of 51:1.
[0052] The particle size of the nano-cesium tungsten oxide in this embodiment is in the range of 10-15 nm.
[0053] Example 4
[0054] A preparation process of nano-cesium tungsten oxide comprises the following preparation steps:
[0055] (1) 20 g of tungsten source and 5.07 g of cesium source were placed in 100 mL of 85 wt% ethanol aqueous solution, 3 g of reducing surfactant was added thereto, and the mixture was reacted at 80 °C for 2.5 h in a sealed container at a stirring speed of 600 r / min, and then dried at 60 °C for 10 h to obtain a precursor;
[0056] (2) 10 g of the precursor obtained in step (1) was placed in 50 mL of a mixed solvent, stirred at 600 r / min for 1.5 h, then kept warm at 235 ° C for 3.5 h in a polytetrafluoroethylene reactor, cooled to room temperature, washed with cyclohexane and anhydrous ethanol for 3 times, and dried at 60 ° C for 10 h to obtain nano-cesium tungsten oxide.
[0057] The mixed solvent used was composed of oleic acid and isobutanol in a mass ratio of 51:1.
[0058] Example 5
[0059] A preparation process of nano-cesium tungsten oxide comprises the following preparation steps:
[0060] (1) 20 g of tungsten source and 5.07 g of cesium source were placed in 100 mL of anhydrous ethanol, 3 g of reducing surfactant was added thereto, the mixture was reacted at 80°C for 2.5 h in a sealed container at a stirring speed of 600 r / min, and then dried at 60°C for 10 h to obtain a precursor;
[0061] (2) 10 g of the precursor obtained in step (1) was placed in 50 mL of a mixed solvent, stirred at 600 r / min for 1.5 h, then kept warm at 235 ° C for 3.5 h in a polytetrafluoroethylene reactor, cooled to room temperature, washed with cyclohexane and anhydrous ethanol for 3 times, and dried at 60 ° C for 10 h to obtain nano-cesium tungsten oxide.
[0062] The mixed solvent used was composed of oleic acid and isobutanol in a mass ratio of 51:1.
[0063] Example 6
[0064] A preparation process of nano-cesium tungsten oxide comprises the following preparation steps:
[0065] (1) 20 g of tungsten source and 6.87 g of cesium source were placed in 100 mL of 93 wt% ethanol aqueous solution, 3 g of reducing surfactant was added thereto, and the mixture was reacted at 80 °C for 2.5 h in a sealed container at a stirring speed of 600 r / min, and then dried at 60 °C for 10 h to obtain a precursor;
[0066] (2) 10 g of the precursor obtained in step (1) was placed in 50 mL of a mixed solvent, stirred at 600 r / min for 1.5 h, then kept warm at 235 ° C for 3.5 h in a polytetrafluoroethylene reactor, cooled to room temperature, washed with cyclohexane and anhydrous ethanol for 3 times, and dried at 60 ° C for 10 h to obtain nano-cesium tungsten oxide.
[0067] The mixed solvent used was composed of oleic acid and isobutanol in a mass ratio of 51:1.
[0068] Example 7
[0069] A preparation process of nano-cesium tungsten oxide comprises the following preparation steps:
[0070] (1) 20 g of tungsten source and 1.96 g of cesium source were placed in 100 mL of 93 wt% ethanol aqueous solution, 3 g of reducing surfactant was added thereto, and the mixture was reacted at 80 °C for 2.5 h in a sealed container at a stirring speed of 600 r / min, and then dried at 60 °C for 10 h to obtain a precursor;
[0071] (2) 10 g of the precursor obtained in step (1) was placed in 50 mL of a mixed solvent, stirred at 600 r / min for 1.5 h, then kept warm at 235 ° C for 3.5 h in a polytetrafluoroethylene reactor, cooled to room temperature, washed with cyclohexane and anhydrous ethanol for 3 times, and dried at 60 ° C for 10 h to obtain nano-cesium tungsten oxide.
[0072] The mixed solvent used was composed of oleic acid and isobutanol in a mass ratio of 51:1.
[0073] Example 8
[0074] A preparation process of nano-cesium tungsten oxide comprises the following preparation steps:
[0075] (1) 20 g of tungsten source and 5.07 g of cesium source were placed in 100 mL of 93 wt% ethanol aqueous solution, 6 g of reducing surfactant was added thereto, and the mixture was reacted at 80 °C for 2.5 h in a sealed container at a stirring speed of 600 r / min, and then dried at 60 °C for 10 h to obtain a precursor;
[0076] (2) 10 g of the precursor obtained in step (1) was placed in 50 mL of a mixed solvent, stirred at 600 r / min for 1.5 h, then kept warm at 235 ° C for 3.5 h in a polytetrafluoroethylene reactor, cooled to room temperature, washed with cyclohexane and anhydrous ethanol for 3 times, and dried at 60 ° C for 10 h to obtain nano-cesium tungsten oxide.
[0077] The mixed solvent used was composed of oleic acid and isobutanol in a mass ratio of 51:1.
[0078] Example 9
[0079] A preparation process of nano-cesium tungsten oxide comprises the following preparation steps:
[0080] (1) 20 g of tungsten source and 5.07 g of cesium source were placed in 100 mL of 93 wt% ethanol aqueous solution, 3 g of reducing surfactant was added thereto, and the mixture was reacted at 80 °C for 2.5 h in a sealed container at a stirring speed of 600 r / min, and then dried at 60 °C for 10 h to obtain a precursor;
[0081] (2) 10 g of the precursor obtained in step (1) was placed in 50 mL of a mixed solvent, stirred at 600 r / min for 1.5 h, then kept at 200 ° C for 3.5 h in a polytetrafluoroethylene reactor, cooled to room temperature, washed with cyclohexane and anhydrous ethanol for 3 times, and dried at 60 ° C for 10 h to obtain nano-cesium tungsten oxide.
[0082] The mixed solvent used was composed of oleic acid and isobutanol in a mass ratio of 51:1.
[0083] Comparative Example 1
[0084] A preparation process of nano-cesium tungsten oxide comprises the following preparation steps:
[0085] (1) 20 g of tungsten source and 5.07 g of cesium source were placed in 100 mL of 93 wt% ethanol aqueous solution, 3 g of reducing surfactant was added thereto, and the mixture was reacted at 80 °C for 2.5 h in a sealed container at a stirring speed of 600 r / min, and then dried at 60 °C for 10 h to obtain a precursor;
[0086] (2) 10 g of the precursor obtained in step (1) was placed in 50 mL of oleic acid, stirred at 600 r / min for 1.5 h, then kept warm at 235 ° C for 3.5 h in a polytetrafluoroethylene reactor, cooled to room temperature, washed with cyclohexane and anhydrous ethanol for 3 times, and dried at 60 ° C for 10 h to obtain nano-cesium tungsten oxide.
[0087] Comparative Example 2
[0088] A preparation process of nano-cesium tungsten oxide comprises the following preparation steps:
[0089] (1) 20 g of tungsten source and 5.07 g of cesium source were placed in 100 mL of 93 wt% ethanol aqueous solution, stirred at 600 r / min in a sealed container, reacted at 80 ° C for 2.5 h, and then dried at 60 ° C for 10 h to obtain a precursor;
[0090] (2) 10 g of the precursor obtained in step (1) was placed in 50 mL of a mixed solvent, stirred at 600 r / min for 1.5 h, then kept warm at 235 ° C for 3.5 h in a polytetrafluoroethylene reactor, cooled to room temperature, washed with cyclohexane and anhydrous ethanol for 3 times, and dried at 60 ° C for 10 h to obtain nano-cesium tungsten oxide.
[0091] The mixed solvent used was composed of oleic acid and isobutanol in a mass ratio of 51:1.
[0092] Comparative Example 3
[0093] A preparation process of nano-cesium tungsten oxide, the specific implementation method is the same as that of Example 3, except that an equal mass of dodecyltrimethylammonium bromide is used instead of a reducing surfactant.
[0094] Performance Test of Nano-Cesium Tungsten Oxide
[0095] 5 g of the prepared nano-tungsten cesium oxide in each embodiment and comparative example was placed in a beaker, and 50 g of anhydrous ethanol and 4 g of sodium dodecyl sulfate were added. After ultrasonic treatment at 20 KHz for 15 min, the mixture was poured into a nano-grinder for ball milling dispersion treatment (ball milling medium: zirconium oxide beads, size: 0.1 mm, speed: 5000 r / min) for 30 min, and the zirconium oxide beads were filtered out with a 200-mesh sieve to obtain a tungsten cesium oxide dispersion;
[0096] 2.5 g of polyvinyl butyral powder was mixed with 15 g of anhydrous ethanol and sealed, and then placed in an oven and heated at 60 ° C for 3 h to obtain a uniformly mixed PVB colloid. The PVB colloid was placed in a degassing box, and 0.11 g of triethylene glycol diisooctanoate, 0.145 g of 2, 6-di-tert-butyl-4-methylphenol and 0.2 g of the tungsten cesium oxide dispersion of each embodiment and comparative example were added. The mixture was degassed for 10 minutes and the obtained mixture was coated with a coating amount of 1.3 g / m 2 Evenly coating on a glass substrate and drying at 60°C to obtain a cesium tungsten oxide transparent heat-insulating composite film;
[0097] The prepared cesium tungsten oxide transparent thermal insulation composite film was placed in a "double 85" test box (temperature 85°C, humidity 85%) to evaluate its resistance to moisture and heat and aging. The light transmittance (%) was calculated by measuring the absorbance values of each cesium tungsten oxide transparent thermal insulation composite film at different aging times (0d, 7d, 30d, 60d) and wavelengths of 950nm and 550nm. The specific test results are shown in Table 1.
[0098] Table 1
[0099]
[0100] As can be seen from Table 1, the nano-cesium tungsten oxide prepared in Examples 1-3 has good light-blocking performance and aging resistance. After 60 days of aging, the blocking rate for near-infrared light at 950nm can still reach 91.3%, and the blocking rate for light at 550nm can still reach 74.8%. Compared with Example 3, Examples 4 and 5 respectively change the solvent used in step (1), which affects the texture of the generated nano-cesium tungsten oxide, and thus affects its aging resistance and light-blocking effect; Examples 6 and 7 change the molar ratio of tungsten element and cesium element in the tungsten source and cesium source, so that the ratio of tungsten to cesium in the nano-cesium tungsten oxide changes, resulting in a decrease in comprehensive performance; Example 8 changes the amount of reducing surfactant used, and Comparative Example 2 does not add reducing surfactant, which may cause the size uniformity of nano-cesium tungsten oxide to be poor during the heating and heat preservation process, affecting its dispersibility, and thus resulting in a decrease in the aging resistance and light-blocking effect of nano-cesium tungsten oxide; Example 9, the insulation temperature is changed, which affects the reaction process of nano-cesium tungsten oxide and causes its comprehensive performance to decline; in comparative example 1, oleic acid is used instead of the mixed solvent. Due to the lack of isobutanol, the dispersibility of the precursor may be weakened and the degree of side reactions may be deepened, so that the yield and comprehensive performance of nano-cesium tungsten oxide are reduced, resulting in the aging resistance and light barrier effect of the prepared nano-cesium tungsten oxide to decline; in comparative example 3, dodecyltrimethylammonium bromide is used instead of the reducing surfactant. Dodecyltrimethylammonium bromide has a weak dispersion effect on the tungsten source and the cesium source in the solvent, the structure of the precursor changes, and the texture uniformity declines, which affects the light barrier rate and aging resistance of the nano-cesium tungsten oxide.
[0101] The above is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present application. Although the present application is disclosed as above in the preferred embodiment, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases. However, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution.
Claims
1. A preparation process of nano-cesium tungsten oxide, characterized in that: The method comprises the following preparation steps: (1) placing a tungsten source and a cesium source in an ethanol aqueous solution, adding a reducing surfactant thereto, reacting in a sealed container at 75-85°C for 2-3 hours, and drying to obtain a precursor; (2) placing the precursor obtained in step (1) into a mixed solvent, stirring for 1-2 hours, then keeping warm in a reaction kettle, cooling to room temperature, washing, and drying to obtain nano-cesium tungsten oxide; The preparation steps of the reducing surfactant are: Dispersing 2,3-dihydroxypropylamine and dodecyltrimethylammonium bromide in anhydrous ethanol at a molar ratio of 1:(2-2.3), stirring and reacting at 75-85° C. for 6-9 hours, rotary evaporating, separating, and drying to obtain a reducing surfactant; The amount of the reducing surfactant is 5-25wt% of the tungsten source; The mixed solvent comprises oleic acid and isobutanol in a mass ratio of (48-53):1; the ratio of the mass of the precursor in step (2) to the volume of the mixed solvent is 1 g:(4.5-5.5) mL; The tungsten source is one or more of tungsten chloride, sodium tungstate and ammonium tungstate; The cesium source is one or more of cesium carbonate, cesium hydroxide, cesium sulfate and cesium nitrate.
2. The preparation process of nano-cesium tungsten oxide according to claim 1, characterized in that: The concentration of the ethanol aqueous solution is 90-95wt%.
3. The preparation process of nano-cesium tungsten oxide according to claim 1, characterized in that: The molar ratio of tungsten element to cesium element in the tungsten source and the cesium source is (2-4):
1.
4. The preparation process of nano-cesium tungsten oxide according to claim 1, characterized in that: The insulation temperature is 210-250° C., and the insulation time is 2-4 hours.
5. A nano-cesium tungsten oxide prepared by the preparation process according to any one of claims 1 to 4, characterized in that: The average particle size of the nano-cesium tungsten oxide is 10-30nm.
6. Application of the nano-cesium tungsten oxide according to claim 5 in the field of thermal insulation coatings.