A low-smoke, halogen-free, flame-retardant, radiation-crosslinked cable material for energy storage cable and a preparation method thereof
By using a combination technology of modified aluminum hydroxide, nano silica and long-chain polyphosphazene structures in cable materials, the problems of flammable and toxic gases in traditional cable materials were solved, and excellent flame retardant, mechanical and Low-smoke, halogen-free flame-retardant irradiation crosslinked cable material with smoke suppression performance.
Patent Information
- Application Number
- CN202411118686.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-15
AI Technical Summary
Traditional halogen-containing cable materials produce toxic gases during combustion, and ethylene-vinyl acetate copolymers are flammable, limiting their application in low-smoke, halogen-free flame-retardant cable materials.
Low-smoke, halogen-free flame retardant irradiation crosslinking is used to melt blend materials such as low-smoke, halogen-free flame retardant irradiation crosslinking. The cable joint material uses the modification treatment of modified aluminum hydroxide and nano-silica to improve the degree of cross-linking and dispersion performance, and combines the flame retardant of the long-chain polyphosphazene structure to enhance the flame retardant and mechanical properties.
It significantly improves the flame retardant performance, mechanical properties and smoke suppression properties of cable materials, solves the flammable problem, and expands its application areas.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flame-retardant cross-linked irradiated cable materials, in particular to a low-smoke halogen-free flame-retardant irradiated cross-linked cable material for energy storage cables and a preparation method thereof. Background Art
[0002] Traditional halogen-containing cable materials have advantages such as high flame retardancy and good processing performance, but because they contain halogens, a large amount of toxic gases are produced during the combustion process, which can cause secondary damage to personnel and electronic and electrical equipment; in order to solve this problem, ethylene-vinyl acetate copolymer is widely used in low-smoke halogen-free flame retardant cable materials because its main chain does not contain double bonds, benzene rings, acyl groups, amine groups and other groups that are easy to burn and produce smoke; but due to its low limiting oxygen index, it is flammable, which hinders its development in the field of low-smoke halogen-free flame retardant cable materials.
[0003] Therefore, in order to solve its flammability problem and improve its application field, it is of great significance to invent a halogen-free radiation cross-linked rubber with excellent mechanical properties and low smoke resistance. Summary of the invention
[0004] The object of the present invention is to provide a low-smoke, halogen-free, flame-retardant, radiation-crosslinked cable material for energy storage cables and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A method for preparing a low-smoke, halogen-free, flame-retardant, radiation-crosslinked cable material for an energy storage cable comprises the following steps:
[0007] Low-density polyethylene, ethylene-vinyl acetate copolymer, modified aluminum hydroxide, modified nano-silicon dioxide and flame retardant are added into a double-roll mill, melt-blended, hot-pressed and cross-linked by electron beam irradiation to obtain low-smoke halogen-free flame-retardant radiation-cross-linked cable material.
[0008] Furthermore, the proportions of the components in the low-smoke halogen-free flame-retardant radiation cross-linked cable material, by mass fraction, are 80-100 parts of low-density polyethylene, 20-40 parts of ethylene vinyl acetate copolymer, 10-15 parts of modified aluminum hydroxide, 2-5 parts of modified nano-silicon dioxide, and 2-5 parts of flame retardant.
[0009] Furthermore, the preparation method of the modified aluminum hydroxide comprises the following steps:
[0010] Add KH550 and aluminum hydroxide to an ethanol solution, heat to 80-85°C and reflux for 6-7h, filter, wash, and vacuum dry at 60-65°C to obtain amino-modified aluminum hydroxide; ultrasonically disperse the amino-modified aluminum hydroxide in xylene, add maleic anhydride, heat to 120-125°C and react for 3-4h, filter, wash, and dry to obtain modified aluminum hydroxide.
[0011] Furthermore, the mass ratio of KH550:aluminum hydroxide in the amino-modified aluminum hydroxide is (1.5-3):100; and the mass ratio of amino-modified aluminum hydroxide:maleic anhydride in the modified aluminum hydroxide is 10:(1-2).
[0012] Furthermore, the preparation method of the modified nano-silicon dioxide comprises the following steps:
[0013] A tetrahydrofuran solution of eugenol is added to a tetrahydrofuran solution of metallic sodium under ice bath conditions and nitrogen protection, and the reaction is carried out at room temperature until the metallic sodium disappears, and a tetrahydrofuran solution of hexachlorocyclotriphosphazene is added, and the mixture is heated to 66-68° C. and reacted for 48-50 hours, and rotary evaporated to obtain eugenol-modified triphosphazene; nano-silica is ultrasonically dispersed in an ethanol solution, the pH is adjusted, KH590 is added, the mixture is heated to 75-85° C. and reacted for 10-12 hours, and filtered, washed, and dried to obtain KH590-modified nano-silica; eugenol-grafted triphosphazene, KH590-modified nano-silica, and 2-hydroxy-2-methylpropiophenone are added to a reaction container, and the mixture is irradiated with ultraviolet light to react to obtain modified nano-silica.
[0014] Furthermore, in the eugenol-modified triphosphazene, the molar ratio of eugenol: metallic sodium: hexachlorocyclotriphosphazene is (9-10):6:1; in the KH590-modified nano-silica, the mass ratio of nano-silica: KH590 is 100:(14-16); in the modified nano-silica, the mass ratio of eugenol-grafted triphosphazene: KH590-modified nano-silica: 2-hydroxy-2-methylpropiophenone is (18-20):(198-238):(2.5-3).
[0015] Furthermore, the method for preparing the flame retardant comprises the following steps:
[0016] Hexachlorocyclotriphosphazene, aminosulfonic acid, calcium sulfate dihydrate, and 1,2,4-trichlorobenzene are added to a reaction container, heated to 190-195°C under nitrogen protection for 10-15 minutes, the nitrogen is stopped, heated to 208-210°C to react until a large number of small bubbles are generated, filtered, and washed to obtain polyphosphazene; a tetrahydrofuran solution of cardanol is added to a tetrahydrofuran solution of metallic sodium under ice bath conditions and nitrogen protection, heated to 66-68°C to react until the metallic sodium disappears, and added A tetrahydrofuran solution of polyphosphazene is heated to 66-68°C and reacted for 48-50 hours, rotary evaporated, precipitated, and vacuum dried at 60-65°C to obtain cardanol-based polyphosphazene; a dichloromethane solution of meta-chloroperbenzoic acid is added to a dichloromethane solution of cardanol-based polyphosphazene under ice bath conditions, heated to 30-32°C and reacted for 24-26 hours, filtered, washed, vacuum dried at 60-65°C, DOPO is added, heated to 160-165°C and reacted for 6-6.5 hours to obtain a flame retardant.
[0017] Furthermore, in the polyphosphazene, the mass ratio of hexachlorocyclotriphosphazene: aminosulfonic acid: calcium sulfate dihydrate is 10: (0.3-0.35): (0.03-0.035); in the cardanol-based polyphosphazene, the molar ratio of cardanol: metallic sodium: polyphosphazene is (1.5-1.67): 1: (0.5-0.55); in the flame retardant, the molar ratio of cardanol-based polyphosphazene: meta-chloroperbenzoic acid: DOPO is (0.05-0.07): (0.4-0.45): (0.2-0.22).
[0018] Furthermore, the temperature of the melt blending is 125-130° C., the temperature of the hot pressing molding is 140-150° C., the pressure is 8-10 MPa, the irradiation dose of the electron beam irradiation cross-linking is 110-130 kGy, and the dose rate is 30 kGy / pass.
[0019] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0020] The invention uses a silane coupling agent KH550 to modify the surface of aluminum hydroxide so that the surface of the aluminum hydroxide carries amino functional groups, and then reacts with maleic anhydride to generate modified aluminum hydroxide with a maleimide structure; uses a silane coupling agent KH590 to modify the surface of nano silicon dioxide so that the surface of the nano silicon dioxide carries thiol functional groups, and then generates a thiol-ene click chemical reaction with olefin functional groups on the surface of triphosphazene modified by eugenol to prepare modified nano silicon dioxide; in the cable material, the modified aluminum hydroxide, on the one hand, utilizes the maleimide structure carried on the surface of the modified aluminum hydroxide to act as a crosslinking sensitizer under the condition of electron beam irradiation crosslinking, and can greatly improve the crosslinking degree of the cable material matrix rubber and improve the mechanical properties of the cable material; on the other hand, utilizes the different molecular sizes of the modified aluminum hydroxide and the modified nano silicon dioxide, utilizes the large molecule modified aluminum hydroxide to help the dispersion performance of the small molecule modified nano silicon dioxide in the cable material, and improves the flame retardant property and mechanical properties of the cable material. With the help of modified aluminum hydroxide, modified nano-silica, on the one hand, solves the problems of poor dispersibility and easy agglomeration as a reinforcing material; on the other hand, the triphosphazene flame retardant group grafted on its surface can work together with its own nano-silica to increase the carbonization rate and the density of the carbon layer during the thermal decomposition process of the cable material, further improving the smoke suppression performance of the cable material.
[0021] The invention uses hexachlorocyclotriphosphazene as a matrix to prepare a long-chain polyphosphazene structure, and uses polyphosphazene as a main chain segment to prepare a synergistic flame retardant with a long alkyl side chain and a phosphaphenanthrene group structure; by utilizing the interaction of a flexible polyphosphazene main chain of the flame retardant, a flexible long alkyl cardanol side chain and a DOPO group with a rigid structure, in a cable material, on the one hand, the tensile strength and elongation at break of the cable material are enhanced; on the other hand, the common gas phase flame retardant and catalytic carbonization effects of the polyphosphazene main chain and the DOPO group can give the material a rapid self-extinguishing performance, thereby greatly improving the smoke suppression performance and flame retardant performance of the cable material. DETAILED DESCRIPTION
[0022] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] In the following examples, the aluminum hydroxide particle size is 25 μm, purchased from Shandong Keheng Crystal Material Technology Co., Ltd.; the nano-silicon dioxide particle size is 50 nm, purchased from Evonik Industries AG of Germany; the ethylene vinyl acetate copolymer model is EA19400, purchased from LG Co., Ltd. of South Korea; the low-density polyethylene model is 7102-0140, purchased from Thermo Fisher Scientific; the remaining raw materials are commercially available.
[0024] Example 1: A method for preparing a low-smoke, halogen-free, flame-retardant, radiation-crosslinked cable material for energy storage cables: S1: Add 1.5 g KH550 and 100 g aluminum hydroxide to a 75 wt% ethanol solution, heat to 80°C and reflux for 6 h, filter, wash, and vacuum dry at 60°C to obtain amino-modified aluminum hydroxide; ultrasonically disperse 100 g of amino-modified aluminum hydroxide in xylene, add 10 g of maleic anhydride, heat to 120°C and react for 3 h, filter, wash, and dry to obtain modified aluminum hydroxide;
[0025] S2: Add a tetrahydrofuran solution containing 9 mol of eugenol to a tetrahydrofuran solution containing 6 mol of metallic sodium under an ice bath and nitrogen protection, react at room temperature until the metallic sodium disappears, add a tetrahydrofuran solution containing 1 mol of hexachlorocyclotriphosphazene, heat to 66°C for reaction for 40 hours, and rotary evaporate to obtain eugenol-modified triphosphazene; ultrasonically disperse 100 g of nano-silica in an ethanol solution, adjust the pH to 4, add 14 g of KH590, heat to 80°C for reaction for 10 hours, filter, wash, and dry to obtain KH590-modified nano-silica; add 18 g of eugenol-grafted triphosphazene, 198 g of KH590-modified nano-silica, and 2.5 g of 2-hydroxy-2-methylpropiophenone into a reaction vessel, and react under ultraviolet irradiation to obtain modified nano-silica;
[0026] S3: 10 g of hexachlorocyclotriphosphazene, 0.3 g of aminosulfonic acid, 0.03 g of calcium sulfate dihydrate, and 20 mL of 1,2,4-trichlorobenzene were added to a reaction vessel, heated to 190°C for 10 min under nitrogen protection, the nitrogen was stopped, and the reaction was heated to 208°C until a large number of small bubbles were generated, filtered, and washed to obtain polyphosphazene; a tetrahydrofuran solution containing 1.5 mol of cardanol was added to a tetrahydrofuran solution containing 1 mol of metallic sodium under ice bath conditions and nitrogen protection, and heated to 66°C to react until the metal After the sodium disappears, a tetrahydrofuran solution containing 0.5 mol of polyphosphazene is added, and the mixture is heated to 66°C for reaction for 48 hours, rotary evaporated, precipitated, and vacuum dried at 60°C to obtain cardanol-based polyphosphazene; a dichloromethane solution containing 0.4 mol of meta-chloroperbenzoic acid is added to a dichloromethane solution containing 0.05 mol of cardanol-based polyphosphazene under ice bath conditions, and the mixture is heated to 30°C for reaction for 24 hours, filtered, washed, and vacuum dried at 60°C, and 0.2 mol of DOPO is added, and the mixture is heated to 160°C for reaction for 6 hours to obtain a flame retardant;
[0027] S4: Add 100g low-density polyethylene, 40g ethylene-vinyl acetate copolymer, 10g modified aluminum hydroxide, 2g modified nano-silica and 2g flame retardant into a double-roll mill, melt blend at 125°C, hot press mold at 140°C and 10MPa, and cross-link by electron beam irradiation at 120kGy and 30kGy / pass to obtain low-smoke halogen-free flame-retardant irradiation cross-linked cable material.
[0028] Example 2: A method for preparing a low-smoke, halogen-free, flame-retardant, radiation-crosslinked cable material for energy storage cables: S1: Add 3g KH550 and 100g aluminum hydroxide to a 75wt% ethanol solution, heat to 80°C and reflux for 6h, filter, wash, and vacuum dry at 60°C to obtain amino-modified aluminum hydroxide; ultrasonically disperse 100g of amino-modified aluminum hydroxide in xylene, add 20g of maleic anhydride, heat to 120°C and react for 3h, filter, wash, and dry to obtain modified aluminum hydroxide;
[0029] S2: Add a tetrahydrofuran solution containing 9 mol of eugenol to a tetrahydrofuran solution containing 6 mol of metallic sodium under an ice bath and nitrogen protection, react at room temperature until the metallic sodium disappears, add a tetrahydrofuran solution containing 1 mol of hexachlorocyclotriphosphazene, heat to 66°C for reaction for 40 hours, and rotary evaporate to obtain eugenol-modified triphosphazene; ultrasonically disperse 100 g of nano-silica in an ethanol solution, adjust the pH to 4, add 14 g of KH590, heat to 80°C for reaction for 10 hours, filter, wash, and dry to obtain KH590-modified nano-silica; add 18 g of eugenol-grafted triphosphazene, 198 g of KH590-modified nano-silica, and 2.5 g of 2-hydroxy-2-methylpropiophenone into a reaction vessel, and react under ultraviolet irradiation to obtain modified nano-silica;
[0030] S3: 10 g of hexachlorocyclotriphosphazene, 0.3 g of aminosulfonic acid, 0.03 g of calcium sulfate dihydrate, and 20 mL of 1,2,4-trichlorobenzene were added to a reaction vessel, heated to 190°C for 10 min under nitrogen protection, the nitrogen was stopped, and the reaction was heated to 208°C until a large number of small bubbles were generated, filtered, and washed to obtain polyphosphazene; a tetrahydrofuran solution containing 1.5 mol of cardanol was added to a tetrahydrofuran solution containing 1 mol of metallic sodium under ice bath conditions and nitrogen protection, and heated to 66°C to react until the metal After the sodium disappears, a tetrahydrofuran solution containing 0.5 mol of polyphosphazene is added, and the mixture is heated to 66°C for reaction for 48 hours, rotary evaporated, precipitated, and vacuum dried at 60°C to obtain cardanol-based polyphosphazene; a dichloromethane solution containing 0.4 mol of meta-chloroperbenzoic acid is added to a dichloromethane solution containing 0.05 mol of cardanol-based polyphosphazene under ice bath conditions, and the mixture is heated to 30°C for reaction for 24 hours, filtered, washed, and vacuum dried at 60°C, and 0.2 mol of DOPO is added, and the mixture is heated to 160°C for reaction for 6 hours to obtain a flame retardant;
[0031] S4: Add 100g low-density polyethylene, 40g ethylene-vinyl acetate copolymer, 10g modified aluminum hydroxide, 2g modified nano-silica and 2g flame retardant into a double-roll mill, melt blend at 125°C, hot press mold at 140°C and 10MPa, and cross-link by electron beam irradiation at 120kGy and 30kGy / pass to obtain low-smoke halogen-free flame-retardant irradiation cross-linked cable material.
[0032] Example 3: A method for preparing a low-smoke, halogen-free, flame-retardant, radiation-crosslinked cable material for energy storage cables: S1: Add 2g KH550 and 100g aluminum hydroxide to a 75wt% ethanol solution, heat to 80°C and reflux for 6h, filter, wash, and vacuum dry at 60°C to obtain amino-modified aluminum hydroxide; ultrasonically disperse 100g of amino-modified aluminum hydroxide in xylene, add 20g of maleic anhydride, heat to 120°C and react for 3h, filter, wash, and dry to obtain modified aluminum hydroxide;
[0033] S2: Add a tetrahydrofuran solution containing 9 mol of eugenol to a tetrahydrofuran solution containing 6 mol of metallic sodium under ice bath conditions and nitrogen protection, react at room temperature until the metallic sodium disappears, add a tetrahydrofuran solution containing 1 mol of hexachlorocyclotriphosphazene, heat to 66°C for reaction for 40 hours, and rotary evaporate to obtain eugenol-modified triphosphazene; ultrasonically disperse 100 g of nano-silica in an ethanol solution, adjust the pH to 4, add 14 g of KH590, heat to 80°C for reaction for 10 hours, filter, wash, and dry to obtain KH590-modified nano-silica; add 20 g of eugenol-grafted triphosphazene, 238 g of KH590-modified nano-silica, and 2.5 g of 2-hydroxy-2-methylpropiophenone into a reaction vessel, and react under ultraviolet irradiation to obtain modified nano-silica;
[0034] S3: 10 g of hexachlorocyclotriphosphazene, 0.3 g of aminosulfonic acid, 0.03 g of calcium sulfate dihydrate, and 20 mL of 1,2,4-trichlorobenzene were added to a reaction vessel, heated to 190°C for 10 min under nitrogen protection, the nitrogen was stopped, and the reaction was heated to 208°C until a large number of small bubbles were generated, filtered, and washed to obtain polyphosphazene; a tetrahydrofuran solution containing 1.5 mol of cardanol was added to a tetrahydrofuran solution containing 1 mol of metallic sodium under ice bath conditions and nitrogen protection, and heated to 66°C to react until the metal After the sodium disappears, a tetrahydrofuran solution containing 0.5 mol of polyphosphazene is added, and the mixture is heated to 66°C for reaction for 48 hours, rotary evaporated, precipitated, and vacuum dried at 60°C to obtain cardanol-based polyphosphazene; a dichloromethane solution containing 0.4 mol of meta-chloroperbenzoic acid is added to a dichloromethane solution containing 0.05 mol of cardanol-based polyphosphazene under ice bath conditions, and the mixture is heated to 30°C for reaction for 24 hours, filtered, washed, and vacuum dried at 60°C, and 0.2 mol of DOPO is added, and the mixture is heated to 160°C for reaction for 6 hours to obtain a flame retardant;
[0035] S4: Add 100g low-density polyethylene, 40g ethylene-vinyl acetate copolymer, 10g modified aluminum hydroxide, 2g modified nano-silica and 2g flame retardant into a double-roll mill, melt blend at 125°C, hot press mold at 140°C and 10MPa, and cross-link by electron beam irradiation at 120kGy and 30kGy / pass to obtain low-smoke halogen-free flame-retardant irradiation cross-linked cable material.
[0036] Example 4: A method for preparing a low-smoke, halogen-free, flame-retardant, radiation-crosslinked cable material for energy storage cables: S1: Add 2g KH550 and 100g aluminum hydroxide to a 75wt% ethanol solution, heat to 80°C and reflux for 6h, filter, wash, and vacuum dry at 60°C to obtain amino-modified aluminum hydroxide; ultrasonically disperse 100g of amino-modified aluminum hydroxide in xylene, add 20g of maleic anhydride, heat to 120°C and react for 3h, filter, wash, and dry to obtain modified aluminum hydroxide;
[0037] S2: Add a tetrahydrofuran solution containing 9 mol of eugenol to a tetrahydrofuran solution containing 6 mol of metallic sodium under ice bath conditions and nitrogen protection, react at room temperature until the metallic sodium disappears, add a tetrahydrofuran solution containing 1 mol of hexachlorocyclotriphosphazene, heat to 66°C for reaction for 40 hours, and rotary evaporate to obtain eugenol-modified triphosphazene; ultrasonically disperse 100 g of nano-silica in an ethanol solution, adjust the pH to 4, add 14 g of KH590, heat to 80°C for reaction for 10 hours, filter, wash, and dry to obtain KH590-modified nano-silica; add 20 g of eugenol-grafted triphosphazene, 238 g of KH590-modified nano-silica, and 2.5 g of 2-hydroxy-2-methylpropiophenone into a reaction vessel, and react under ultraviolet irradiation to obtain modified nano-silica;
[0038] S3: 10 g of hexachlorocyclotriphosphazene, 0.3 g of aminosulfonic acid, 0.03 g of calcium sulfate dihydrate, and 20 mL of 1,2,4-trichlorobenzene were added to a reaction vessel, heated to 190°C for 10 min under nitrogen protection, the nitrogen was stopped, and the reaction was heated to 208°C until a large number of small bubbles were generated, filtered, and washed to obtain polyphosphazene; a tetrahydrofuran solution containing 1.5 mol of cardanol was added to a tetrahydrofuran solution containing 1 mol of metallic sodium under ice bath conditions and nitrogen protection, and heated to 66°C to react until the metal After the sodium disappears, a tetrahydrofuran solution containing 0.5 mol of polyphosphazene is added, and the mixture is heated to 66°C for reaction for 48 hours, rotary evaporated, precipitated, and vacuum dried at 60°C to obtain cardanol-based polyphosphazene; a dichloromethane solution containing 0.4 mol of meta-chloroperbenzoic acid is added to a dichloromethane solution containing 0.05 mol of cardanol-based polyphosphazene under ice bath conditions, and the mixture is heated to 30°C for reaction for 24 hours, filtered, washed, and vacuum dried at 60°C, and 0.2 mol of DOPO is added, and the mixture is heated to 160°C for reaction for 6 hours to obtain a flame retardant;
[0039] S4: Add 100g low-density polyethylene, 40g ethylene-vinyl acetate copolymer, 15g modified aluminum hydroxide, 5g modified nano-silica and 2g flame retardant into a double-roll mill, melt blend at 125°C, hot press mold at 140°C and 10MPa, and cross-link by electron beam irradiation at 120kGy and 30kGy / pass to obtain low-smoke halogen-free flame-retardant irradiation cross-linked cable material.
[0040] Example 5: A method for preparing a low-smoke, halogen-free, flame-retardant, radiation-crosslinked cable material for energy storage cables: S1: Add 2g KH550 and 100g aluminum hydroxide to a 75wt% ethanol solution, heat to 80°C and reflux for 6h, filter, wash, and vacuum dry at 60°C to obtain amino-modified aluminum hydroxide; ultrasonically disperse 100g of amino-modified aluminum hydroxide in xylene, add 20g of maleic anhydride, heat to 120°C and react for 3h, filter, wash, and dry to obtain modified aluminum hydroxide;
[0041] S2: Add a tetrahydrofuran solution containing 9 mol of eugenol to a tetrahydrofuran solution containing 6 mol of metallic sodium under ice bath conditions and nitrogen protection, react at room temperature until the metallic sodium disappears, add a tetrahydrofuran solution containing 1 mol of hexachlorocyclotriphosphazene, heat to 66°C for reaction for 40 hours, and rotary evaporate to obtain eugenol-modified triphosphazene; ultrasonically disperse 100 g of nano-silica in an ethanol solution, adjust the pH to 4, add 14 g of KH590, heat to 80°C for reaction for 10 hours, filter, wash, and dry to obtain KH590-modified nano-silica; add 20 g of eugenol-grafted triphosphazene, 238 g of KH590-modified nano-silica, and 2.5 g of 2-hydroxy-2-methylpropiophenone into a reaction vessel, and react under ultraviolet irradiation to obtain modified nano-silica;
[0042] S3: 10 g of hexachlorocyclotriphosphazene, 0.3 g of aminosulfonic acid, 0.03 g of calcium sulfate dihydrate, and 20 mL of 1,2,4-trichlorobenzene were added to a reaction vessel, heated to 190°C for 10 min under nitrogen protection, the nitrogen was stopped, and the reaction was heated to 208°C until a large number of small bubbles were generated, filtered, and washed to obtain polyphosphazene; a tetrahydrofuran solution containing 1.5 mol of cardanol was added to a tetrahydrofuran solution containing 1 mol of metallic sodium under ice bath conditions and nitrogen protection, and heated to 66°C to react until the metal After the sodium disappears, a tetrahydrofuran solution containing 0.5 mol of polyphosphazene is added, and the mixture is heated to 66°C for reaction for 48 hours, rotary evaporated, precipitated, and vacuum dried at 60°C to obtain cardanol-based polyphosphazene; a dichloromethane solution containing 0.4 mol of meta-chloroperbenzoic acid is added to a dichloromethane solution containing 0.05 mol of cardanol-based polyphosphazene under ice bath conditions, and the mixture is heated to 30°C for reaction for 24 hours, filtered, washed, and vacuum dried at 60°C, and 0.2 mol of DOPO is added, and the mixture is heated to 160°C for reaction for 6 hours to obtain a flame retardant;
[0043] S4: Add 100g low-density polyethylene, 40g ethylene-vinyl acetate copolymer, 15g modified aluminum hydroxide, 5g modified nano-silica and 5g flame retardant into a double-roll mill, melt blend at 125°C, hot press mold at 140°C and 10MPa, and cross-link by electron beam irradiation at 120kGy and 30kGy / pass to obtain low-smoke halogen-free flame-retardant irradiation cross-linked cable material.
[0044] Comparative Example 1: A method for preparing a low-smoke, halogen-free, flame-retardant, radiation-cross-linked cable material for energy storage cables: S4: Add 100g of low-density polyethylene, 40g of ethylene-vinyl acetate copolymer, 10g of modified aluminum hydroxide, 1g of modified nano-silicon dioxide, and 2g of flame retardant into a double-roll mill, melt blend at 125°C, hot press molded at 140°C, 10MPa, and electron beam irradiation cross-linked at 120kGy, 30kGy / pass to obtain a low-smoke, halogen-free, flame-retardant, radiation-cross-linked cable material.
[0045] The remaining steps are the same as those in Example 1.
[0046] Comparative Example 2: A method for preparing a low-smoke, halogen-free, flame-retardant, radiation-cross-linked cable material for energy storage cables: S4: Add 100g of low-density polyethylene, 40g of ethylene-vinyl acetate copolymer, 10g of modified aluminum hydroxide, 6g of modified nano-silicon dioxide, and 2g of flame retardant into a double-roll mill, melt blend at 125°C, hot press mold at 140°C, 10MPa, and electron beam irradiation cross-linking at 120kGy, 30kGy / pass to obtain a low-smoke, halogen-free, flame-retardant, radiation-cross-linked cable material.
[0047] The remaining steps are the same as those in Example 1.
[0048] Comparative Example 3: A method for preparing a low-smoke, halogen-free, flame-retardant, radiation-cross-linked cable material for energy storage cables: S4: Add 100g of low-density polyethylene, 40g of ethylene-vinyl acetate copolymer, 8g of modified aluminum hydroxide, 2g of modified nano-silicon dioxide, and 2g of flame retardant into a double-roll mill, melt blend at 125°C, hot press molded at 140°C, 10MPa, and electron beam irradiation cross-linking at 120kGy, 30kGy / pass to obtain a low-smoke, halogen-free, flame-retardant, radiation-cross-linked cable material.
[0049] The remaining steps are the same as those in Example 1.
[0050] Comparative Example 4: A method for preparing a low-smoke, halogen-free, flame-retardant, radiation-cross-linked cable material for energy storage cables: S4: Add 100g of low-density polyethylene, 40g of ethylene-vinyl acetate copolymer, 18g of modified aluminum hydroxide, 2g of modified nano-silicon dioxide, and 2g of flame retardant into a double-roll mill, melt blend at 125°C, hot press molded at 140°C, 10MPa, and electron beam irradiation cross-linking at 120kGy, 30kGy / pass to obtain a low-smoke, halogen-free, flame-retardant, radiation-cross-linked cable material.
[0051] The remaining steps are the same as those in Example 1.
[0052] Experiment: Limiting oxygen index: Use oxygen index instrument, test according to ASTM D2863, the sample size is 100mm×6.5mm×3.5mm;
[0053] Cone calorimeter: Use a cone calorimeter based on the oxygen consumption principle, test according to ISO 5660, sample size is 100mm×100mm×3.5mm, 35kW / m 2 Tested under radiant heat flux.
[0054] Mechanical properties: The test was carried out in accordance with GB / T 528-2009. The sample size was a dumbbell-shaped sample with a length of 25 mm.
[0055] Table 1 Performance test data of irradiation cross-linked cable materials
[0056]
[0057] Conclusion: The irradiation cross-linked cable material prepared by the present invention has excellent flame retardant properties, mechanical properties and smoke suppression properties;
[0058] In Example 1, too little modified nano-silicon dioxide was added, resulting in reduced carbonization and reinforcement effects, resulting in reduced performance; in Example 2, excessive modified nano-silicon dioxide was added, resulting in uneven dispersion, resulting in a significant reduction in elongation at break under the same tensile strength; in Example 3, too little modified aluminum hydroxide was added, resulting in reduced dispersant and cross-linking sensitizer effects, resulting in reduced performance; in Example 4, excessive modified aluminum hydroxide was added, resulting in increased cross-linking effects, increased internal cross-linking degree of cable materials, resulting in reduced mechanical properties
[0059] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a low-smoke, halogen-free, flame-retardant, radiation-crosslinked cable material for energy storage cables, characterized in that: The following steps are involved: Low-density polyethylene, ethylene-vinyl acetate copolymer, modified aluminum hydroxide, modified nano-silicon dioxide and flame retardant are added into a double-roll mill, melt blended, hot-pressed and cross-linked by electron beam irradiation to obtain low-smoke halogen-free flame-retardant radiation-cross-linked cable material; The preparation method of the modified aluminum hydroxide comprises the following steps: Add KH550 and aluminum hydroxide to an ethanol solution, heat to 80-85°C and reflux for 6-7h, filter, wash, and vacuum dry at 60-65°C to obtain amino-modified aluminum hydroxide; ultrasonically disperse the amino-modified aluminum hydroxide in xylene, add maleic anhydride, heat to 120-125°C and react for 3-4h, filter, wash, and dry to obtain modified aluminum hydroxide; The proportion of each component in the low-smoke halogen-free flame-retardant radiation cross-linked cable material, by mass fraction, is 80-100 parts of low-density polyethylene, 20-40 parts of ethylene vinyl acetate copolymer, 10-15 parts of modified aluminum hydroxide, 2-5 parts of modified nano silicon dioxide, and 2-5 parts of flame retardant; The preparation method of the modified nano silicon dioxide comprises the following steps: The tetrahydrofuran solution of eugenol is added to the tetrahydrofuran solution of sodium metal under the condition of ice bath and nitrogen protection, and the reaction is carried out at room temperature until the sodium metal disappears, and the tetrahydrofuran solution of hexachlorocyclotriphosphazene is added, and the mixture is heated to 66-68° C. and reacted for 48-50 hours, and rotary evaporated to obtain eugenol-modified triphosphazene; nano-silica is ultrasonically dispersed in an ethanol solution, the pH is adjusted, KH590 is added, the mixture is heated to 75-85° C. and reacted for 10-12 hours, filtered, washed, and dried to obtain KH590-modified nano-silica; eugenol-modified triphosphazene, KH590-modified nano-silica, and 2-hydroxy-2-methylpropiophenone are added to a reaction container, and the mixture is irradiated with ultraviolet light to obtain modified nano-silica; The method for preparing the flame retardant comprises the following steps: Hexachlorocyclotriphosphazene, aminosulfonic acid, calcium sulfate dihydrate, and 1,2,4-trichlorobenzene are added to a reaction container, heated to 190-195°C under nitrogen protection for 10-15 minutes, the nitrogen is stopped, heated to 208-210°C to react until a large number of small bubbles are generated, filtered, and washed to obtain polyphosphazene; a tetrahydrofuran solution of cardanol is added to a tetrahydrofuran solution of metallic sodium under ice bath conditions and nitrogen protection, heated to 66-68°C to react until the metallic sodium disappears, and added A tetrahydrofuran solution of polyphosphazene is heated to 66-68°C and reacted for 48-50 hours, rotary evaporated, precipitated, and vacuum dried at 60-65°C to obtain cardanol-based polyphosphazene; a dichloromethane solution of meta-chloroperbenzoic acid is added to a dichloromethane solution of cardanol-based polyphosphazene under ice bath conditions, heated to 30-32°C and reacted for 24-26 hours, filtered, washed, vacuum dried at 60-65°C, DOPO is added, heated to 160-165°C and reacted for 6-6.5 hours to obtain a flame retardant.
2. The method for preparing a low-smoke, halogen-free, flame-retardant, radiation-crosslinked cable material for energy storage cables according to claim 1, characterized in that: The mass ratio of KH550:aluminum hydroxide in the amino-modified aluminum hydroxide is (1.5-3):100; and the mass ratio of amino-modified aluminum hydroxide:maleic anhydride in the modified aluminum hydroxide is 10:(1-2).
3. The method for preparing a low-smoke, halogen-free, flame-retardant, radiation-crosslinked cable material for energy storage cables according to claim 1, characterized in that: In the eugenol-modified triphosphazene, the molar ratio of eugenol: metallic sodium: hexachlorocyclotriphosphazene is (9-10):6:1; in the KH590-modified nano-silica, the mass ratio of nano-silica: KH590 is 100:(14-16); in the modified nano-silica, the mass ratio of eugenol-modified triphosphazene: KH590-modified nano-silica: 2-hydroxy-2-methylpropiophenone is (18-20):(198-238):(2.5-3).
4. The method for preparing a low-smoke, halogen-free, flame-retardant, radiation-crosslinked cable material for energy storage cables according to claim 1, characterized in that: In the polyphosphazene, the mass ratio of hexachlorocyclotriphosphazene:aminosulfonic acid:calcium sulfate dihydrate is 10:(0.3-0.35):(0.03-0.035); in the cardanol-based polyphosphazene, the molar ratio of cardanol:metallic sodium:polyphosphazene is (1.5-1.67):1:(0.5-0.55); in the flame retardant, the molar ratio of cardanol-based polyphosphazene:meta-chloroperbenzoic acid:DOPO is (0.05-0.07):(0.4-0.45):(0.2-0.22).
5. The method for preparing a low-smoke, halogen-free, flame-retardant, radiation-crosslinked cable material for energy storage cables according to claim 1, characterized in that: The temperature of the melt blending is 125-130° C., the temperature of the hot pressing molding is 140-150° C., the pressure is 8-10 MPa, and the irradiation dose of the electron beam irradiation cross-linking is 110-130 kGy.
6. A low-smoke, halogen-free, flame-retardant, radiation-crosslinked cable material prepared according to the method for preparing a low-smoke, halogen-free, flame-retardant, radiation-crosslinked cable material for energy storage cables according to any one of claims 1 to 5.
Citation Information
Patent Citations
Method for fabricating heat-insulating polymer composite
EA019400B1
Aryloxy substituted tripolyphosphazene epoxide and preparation method and application thereof
CN102718802A
Oil-resistant flame-retardant cable material and preparation method thereof
CN109306111A
Flame retardant and degradable polyphosphazene epoxy resin and preparation technology thereof
CN109608620A
Preparation method of high-flame-retardant cross-linked polyphosphazene elastomer
CN111303434A