Matt oil, preparation method and frosted touch film bag using the matt oil

By using pure acrylic resin, polyfunctional acrylate resin and silicone powder in the matte ink film, combined with turpentine oil, a high shrinkage ink film is formed, which solves the slow drying speed and poor adhesion of the matte ink film in the prior art. The problem of high flexibility, good matte effect and low gloss are achieved.

CN118620462BActive Publication Date: 2024-12-06上海上源印务有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411111683.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-12-06
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The existing matte ink film has slow drying speed, poor adhesion, and it is difficult to form a good matte effect and low gloss.

Method used

Pure acrylic resin and polyfunctional acrylate resin are used as the main resin, combined with silicone powder and turpentine oil, and a high shrinkage ink film is formed by UV light curing, creating a wrinkle structure to improve the matte touch and low gloss.

Benefits of technology

It realizes high flexibility, wear resistance and good adhesion of the ink film, has excellent matte effect and low gloss, and improves light transmittance, avoiding the problem of whiteness and impermeability of the surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present application relates to the technical field of packaging materials, and specifically discloses a matte oil, a preparation method and a frosted touch film bag using the matte oil. The matte oil includes the following components in parts by weight: 40-50 parts of pure acrylic resin, 20-30 parts of multifunctional acrylate resin, 30-40 parts of reactive diluent, 1-10 parts of turpentine, 5-10 parts of silicone powder, 1-3 parts of photoinitiator, 0.5-1 parts of leveling agent, and 0.5-1 parts of defoaming agent. The number of functional groups of the multifunctional acrylate resin is 9-15, and the multifunctional acrylate resin adopts Lencolo L-6901 and / or Lencolo L-6902. The present application adopts pure acrylic resin and multifunctional acrylate resin as the main resin, and the ink film has a high shrinkage rate, is easy to combine with silicone powder to form a low-gloss, matte, and frosted ink film with good frosting effect, and the ink film has good flexibility, strong wear resistance, and excellent solvent resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of packaging materials, and more specifically, to a matte oil, a preparation method and a frosted touch film bag using the matte oil. Background Art

[0002] With the development of economy and the progress of science and technology, people have higher and higher requirements for the appearance of products. Traditional glossy materials can no longer meet people's aesthetics. Touch film is widely used in various packaging manufacturers due to its special velvet, delicate touch, high fog, and more special matte effect. Touch film, also called soft film, is a special matte film with a special velvety smooth and delicate touch. It is mainly achieved by coating touch oil on the surface of the film. It can be used for luxury goods packaging, high-end book and magazine packaging, and high-end hang tags. It has the advantages of friction resistance, no fingerprints, and velvety feel.

[0003] Chinese patent CN201510267025.2 discloses a non-processed frosted varnish ink for PET film gravure printing, which is composed of varnish, diluent and curing agent, wherein the weight ratio of varnish: diluent: curing agent is 10:4-18:0.5, and the varnish is composed of the following components in weight percentage: 25-40% polyurethane resin liquid, 3-7% butyl acetate, 8-12% ethyl acetate, 8-25% inorganic pigment, 1-3% PE wax powder, 2-4% dispersant, 15-20% modified material, 20-35% n-propyl acetate. The ink of the invention can be printed with ordinary PET film to achieve partial matte or full matte, and can also adjust the product matte degree 2° to 15° freely, but compared with UV curing ink, the solvent-based ink dries slowly, is easy to get dirty, has low production efficiency, and has relatively poor ink film adhesion.

[0004] Chinese patent CN201410372189.7 discloses a scratch-resistant UV matt oil for matt film and its preparation method, the scratch-resistant UV matt oil for matt film is composed of 5-15 parts of epoxy acrylic resin, 20-35 parts of modified acrylic resin, 50-65 parts of acrylic monomer, 10-15 parts of photoinitiator, 5-15 parts of matting agent, and 1-5 parts of auxiliary agent. Compared with traditional solvent-based inks, this UV curing ink basically does not contain volatile components, and the film-forming and curing principle is completely different from that of solvent-based inks. It can complete drying and curing within a few seconds, there is no large amount of solvent volatilization process, and the ink film volume will not be greatly reduced, which makes it difficult for inorganic filler particles to be exposed on the surface of the ink film, and it is difficult to form a concave and convex surface, resulting in a poor sand feeling. Summary of the invention

[0005] In order to solve the above-mentioned technical problems, the present application provides a matt oil, a preparation method and a frosted tactile film bag using the matt oil. The matt oil formula of the present application adopts pure acrylic resin and multi-functional acrylate resin as the main resins. The ink film has a high shrinkage rate and is easy to combine with silicone powder to form a low-gloss, matte, and frosted ink film. The ink film has good flexibility, strong wear resistance, and excellent solvent resistance.

[0006] In a first aspect, the present application provides a matt oil comprising the following components in parts by weight: 40-50 parts of pure acrylic resin, 20-30 parts of multifunctional acrylate resin, 30-40 parts of reactive diluent, 1-10 parts of turpentine, 5-10 parts of silicone powder, 1-3 parts of photoinitiator, 0.5-1 parts of leveling agent, and 0.5-1 parts of defoaming agent.

[0007] Furthermore, the multifunctional acrylate resin has 9-15 functional groups.

[0008] Preferably, the multifunctional acrylate resin is Lencolo L-6901 and / or Lencolo L-6902.

[0009] Preferably, the pure acrylic resin is Lencolo L-6020.

[0010] This application uses pure acrylic resin as the main raw material, and the ink film obtained has high flexibility and high adhesion, and when used as a tactile matt oil, the ink film has good permeability. This application introduces a multifunctional acrylic resin with high shrinkage energy, which, combined with pure acrylic resin, can increase the film volume shrinkage when the matt oil is cured. During light curing, the surface of the ink film shrinks and wrinkles, and at the same time forces the matting powder to be exposed on the surface of the cured ink film. The wrinkled structure and the exposed matting powder on the surface of the ink film make the ink film have a good frosted touch. At the same time, the wrinkled structure and the matting powder jointly produce diffuse reflection of the incident light, thereby producing a delicate low-gloss effect.

[0011] Furthermore, the turpentine oil includes at least one of α-pinene, β-pinene and dipentene.

[0012] The present application adds a small amount of turpentine to further increase the shrinkage of the ink film when it is solidified, thereby improving the matte and frosted effects of the ink film.

[0013] Furthermore, the active diluent includes at least one of tripropylene glycol diacrylate, 2-phenoxyethyl acrylate, isononyl acrylate, ethoxylated bisphenol A dimethacrylate, pentaerythritol triacrylate, ethoxylated trimethylolpropane triacrylate, tris(2-hydroxyethyl)isocyanuric acid triacrylate, dipentaerythritol hexaacrylate, and 1,6-hexanediol diacrylate.

[0014] Furthermore, the organic silicon powder includes at least one of TY-609, TY-610, TY-605, and TY-608.

[0015] Preferably, the organic silicon powder is TY-609 and TY-608.

[0016] Further, the photoinitiator includes at least one of a free radical photoinitiator and a cationic photoinitiator. Among them, the free radical photoinitiator includes 1-hydroxycyclohexyl phenyl ketone, 2-phenylbenzyl-2-dimethylamine-1-(4-morpholinobenzylphenyl)butanone, 2-isopropylthioxanthone, 2-methyl-1-(4-methylthiophenyl)-2-morpholino-1-propanone, diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide, 2,4-diethylthioxanthone and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, etc.; the cationic photoinitiator includes bis-2,6-difluoro-3-pyrrolophenyl titanocene, sulfonium hexafluoroantimonate, diphenyl-(4-phenylthio)phenylsulfonium hexafluorophosphate and η6-isopropylphenylferrocene hexafluorophosphate, etc.

[0017] Preferably, the photoinitiator is a mixture of 1-hydroxycyclohexyl phenyl ketone and bis(2,6-difluoro-3-pyrrolephenyl)titanocene. The above two photoinitiators are compounded so that the matt oil can be well adapted to the multi-band light source, thereby being completely cured, quickly drying the surface and achieving deep curing.

[0018] Furthermore, the leveling agent includes at least one of BTK-300, BTK-306, BTK-307, BTK-310, BTK-315, BTK-320, BTK-323, BTK-325, and BTK-331.

[0019] Leveling agent can promote the matt oil to form a flat, smooth and uniform coating film during the drying and film-forming process, and can effectively reduce the surface tension of the matt oil and improve its leveling and uniformity.

[0020] Furthermore, the defoaming agent is a polyether-modified silicone defoaming agent.

[0021] Ether-modified silicone defoamers have the advantages of both polyether defoamers and silicone defoamers. They can adjust the bubbles formed in the ink matrix or eliminate the bubbles generated during the ink production process, thereby allowing the various components of the ink to be evenly combined and improving the overall performance of the ink.

[0022] In the second aspect, the present application provides a method for preparing the above-mentioned matte oil, and the specific steps are: weigh each component according to the above-mentioned mass requirements, start stirring, and add pure acrylic resin, multifunctional acrylate resin, active diluent, turpentine, leveling agent, photoinitiator, defoaming agent, and silicone powder in sequence, stir and disperse evenly, and grind to obtain the matte oil.

[0023] In a third aspect, the present application provides a frosted tactile film bag using the above-mentioned matte oil.

[0024] Fourthly, the present application provides a method for preparing the above-mentioned frosted tactile film bag, and the specific steps are: subjecting the substrate to be coated to dust removal, corona treatment, and heating and ironing treatment in turn, and evenly coating the matte oil on the surface of the substrate by micro-concave precision coating, and then drying the coated substrate first, and then performing oxygen-proof UV curing twice to obtain the obtained product.

[0025] Preferably, the coating amount of the matt oil on the substrate is 2.8-3.5 g / m 2 .

[0026] Preferably, the drying temperature is 40-60° C. More preferably, the drying temperature is 50° C.

[0027] Preferably, the energy of the two UV curing processes is 200-500 mj / cm 2 and 1000-1200mj / cm 2 .

[0028] In summary, this application has the following beneficial effects:

[0029] 1. The present application uses pure acrylic resin, which helps to improve the flexibility of the system and ensure the adhesion and anti-bursting properties of the matte oil. In addition, compared with the matte oil that needs to add a large amount of silica, calcium carbonate and other covering fillers to obtain a frosted effect, the matte oil provided by the present application has a high transmittance and will not cause the surface to become white and opaque.

[0030] 2. The present application adopts a mixture of a high-yield energy multi-functional acrylate resin and an acrylic resin to increase the film volume shrinkage rate when the ink is cured. During light curing, the surface of the ink film shrinks and produces wrinkles, and at the same time forces the matting powder to be exposed on the surface of the cured ink film. The wrinkle structure and the matting powder exposed on the surface of the ink film give the ink film a good matte touch. At the same time, the wrinkle structure and the matting powder jointly produce a diffuse reflection effect on the incident light, thereby producing a delicate low-gloss effect.

[0031] 3. This application adds a small amount of volatile solvent turpentine and adds a drying process before UV curing. The ink film achieves initial shrinkage in the early stage of curing, allowing the silicone powder to quickly migrate and be exposed on the surface of the ink film, thereby improving the matte and frosted effects of the ink film after drying. DETAILED DESCRIPTION

[0032] The present application is further described in detail below with reference to the embodiments.

[0033] Example 1

[0034] A matt oil is prepared by the following steps: 4kg of pure acrylic resin, 2kg of multifunctional acrylic resin, 3kg of active diluent and 0.1kg of turpentine are added into a stirring kettle, dispersed evenly at 1200r / min, the rotation speed is adjusted to 350r / min, 0.5kg of organosilicon powder, 0.1kg of photoinitiator, 0.05kg of leveling agent and 0.05kg of defoaming agent are added, dispersed evenly and then transferred to a grinder for grinding to obtain the matt oil.

[0035] The pure acrylic resin is Lencolo L-6020 purchased from Lancolu; the multifunctional acrylate resin is a mixture of Lencolo L-6901 (9-official, Lancolu) and Lencolo L-6902 (15-official, Lancolu), and the mass ratio of Lencolo L-6901 to Lencolo L-6902 is 2:1; the active diluent is propylene glycol diacrylate (TPGDA); the turpentine oil is α-pinene purchased from Jishui County Jianmin Natural Flavor Oil Factory; the silicone powder is a mixture of TY-609 (15-30μm) and TY-608 (1.5-2μm), and the weight ratio is 4:1, which is purchased from Tuoyi New Materials (Guangzhou) Co., Ltd.; the photoinitiator is photoinitiator 784; the leveling agent is leveling agent BYK-315 (Bick, Germany); the defoamer is polyether modified silicone defoamer B-0518 (Zhonglian Federation).

[0036] Example 2

[0037] A matt oil, the components and process are the same as those of Example 1, and the difference from Example 1 is that the amount of each component is: 4.5kg pure acrylic resin, 2.5kg multifunctional acrylate resin, 3.5kg active diluent, 0.5kg turpentine, 0.75kg organosilicon powder, 0.2kg photoinitiator, 0.075kg leveling agent, 0.075kg defoaming agent.

[0038] Example 3

[0039] A matt oil, the components and process are the same as those of Example 1, and the difference from Example 1 is that the amount of each component is: 5kg pure acrylic resin, 3kg multifunctional acrylate resin, 4kg active diluent, 1kg turpentine, 1kg silicone powder, 0.3kg photoinitiator, 0.1kg leveling agent, 0.1kg defoaming agent.

[0040] Example 4

[0041] A matte oil, the components, dosage and process are the same as those of Example 1, and the difference from Example 1 is that the multifunctional acrylate resin is a mixture of Lencolo L-6901 (9-official, Lencolo) and Lencolo L-6902 (15-official, Lencolo), and the mass ratio of Lencolo L-6901 to Lencolo L-6902 is 1:2.

[0042] Example 5

[0043] A matt oil, the components, dosage and process are the same as those of Example 1, and the difference from Example 1 is that the multifunctional acrylate resin uses Lencolo L-6901 (9-functional, Lancolo).

[0044] Example 6

[0045] A matt oil, the components, dosage and process are the same as those of Example 1, and the difference from Example 1 is that the multifunctional acrylate resin uses Lencolo L-6902 (15-functional, Lancolo).

[0046] Example 7

[0047] A matt oil, the components, dosage and process are the same as those of Example 1, and the difference from Example 1 is that the organic silicone powder is a mixture of TY-609 (15-30 μm) and TY-608 (1.5-2 μm), the weight ratio of the two is 1:4, and the mixture is purchased from Tuoyi New Materials (Guangzhou) Co., Ltd.

[0048] Example 8

[0049] A matt oil, the components, dosage and process are the same as those of Example 1, and the difference from Example 1 is that the organic silicon powder is TY-609 (15-30 μm) purchased from Tuoyi New Materials (Guangzhou) Co., Ltd.

[0050] Comparative Example

[0051] Comparative Example 1

[0052] A matt oil, the components, dosage and process are the same as those of Example 1, and the difference from Example 1 is that the multifunctional acrylate resin adopts Lencolo L-6206 (2-functional, Lancolo).

[0053] Comparative Example 2

[0054] A matt oil, the components, dosage and process are the same as those of Example 1, and the difference from Example 1 is that the multifunctional acrylate resin adopts Lencolo L-6126 (4-functional hyperbranched, Lencol).

[0055] Comparative Example 3

[0056] A matt oil, the components, dosage and process are the same as those of Example 1, and the difference from Example 1 is that the organic silicon powder is TY-608 (1.5-2 μm) purchased from Tuoyi New Materials (Guangzhou) Co., Ltd.

[0057] Comparative Example 4

[0058] A matt oil, which is different from Example 1 in that toluene is used in the formula to replace turpentine.

[0059] Comparative Example 5

[0060] A matt oil, which is different from Example 1 in that turpentine is not added in the formula.

[0061] Application Examples

[0062] Application Examples 1-8

[0063] Preparation of frosted touch film bag: PP is used as the substrate, and dust removal, corona treatment, heating and ironing treatment are carried out in sequence. Micro-concave precision coating is adopted, and the surface is coated with 3.2g / m 2 The matt oil obtained in Examples 1-8 was evenly coated on the surface of the PP substrate, and the coated PP substrate was dried at 50°C for 2 minutes and then heated at 350mj / cm 2 、1000mj / cm 2 The films are cured under UV energy, and finally cut and sealed to obtain frosted touch film bags.

[0064] Comparative Application Examples 1-4

[0065] Preparation of frosted touch film bag: PP is used as the substrate, and dust removal, corona treatment, heating and ironing treatment are carried out in sequence. Micro-concave precision coating is adopted, and the surface is coated with 3.2g / m 2 The matt oil obtained in Comparative Examples 1-4 was evenly coated on the surface of the PP substrate, and the coated PP substrate was dried at 50°C for 2 minutes, and then heated at 350mj / cm 2 、1000mj / cm 2 The films are cured under UV energy, and finally cut and sealed to obtain frosted touch film bags.

[0066] Comparative Application Example 5

[0067] Preparation of frosted touch film bag: PP is used as the substrate, and dust removal, corona treatment, heating and ironing treatment are carried out in sequence. Micro-concave precision coating is adopted, and the surface is coated with 3.2g / m 2 The matt oil obtained in Comparative Example 5 was evenly coated on the surface of the PP substrate, and the coated PP substrate was placed on a 350mj / cm2 、1000mj / cm 2 The films are cured under UV energy, and finally cut and sealed to obtain frosted touch film bags.

[0068] Comparative Application Example 6

[0069] Preparation of frosted touch film bag: PP is used as the substrate, and dust removal, corona treatment, heating and ironing treatment are carried out in sequence. Micro-concave precision coating is adopted, and the surface is coated with 3.2g / m 2 The matt oil obtained in Example 1 was evenly coated on the surface of the PP substrate, and the coated PP substrate was dried at 50°C for 2 minutes, and then heated at 1000mj / cm 2 The film is cured under UV energy, and finally cut and sealed to obtain a frosted touch film bag.

[0070] Performance testing

[0071] The performance tests were conducted on the frosted touch film bags prepared in Example 1-8 and Comparative Application Examples 1-6, respectively.

[0072] Adhesion: According to GB / T 9286-2021 "Scratch test for paint and varnish films".

[0073] Hardness: According to ASTM D3363-00 "Standard Test Method for Pencil Hardness of Coatings".

[0074] Transmittance and haze: tested with a transmittance-haze tester.

[0075] Matte effect: visual and tactile.

[0076]

[0077] It can be seen from the test results in Table 1 that the frosted touch film bag prepared in the present application has excellent frosted touch, matte property and light transmittance, and the adhesion can reach level 0, the hardness reaches 4H, and the mechanical properties are excellent.

[0078] By comparing application examples 1, 4-6, it can be seen that the specific selection of multifunctional acrylate resin will affect the optical properties and frosted touch of the ink film. When the multifunctional acrylate resin is Lencolo L-6901 and Lencolo L-6902 and is combined in a mass ratio of 2:1, the ink film has the best performance.

[0079] By comparing Application Example 1 and Application Example 7, it can be seen that when the silicone powder is combined with TY-609 and TY-608 in a mass ratio of 1:4, the frosted touch and matte performance of the ink film are reduced.

[0080] By comparing Application Example 1 and Application Example 8, it can be seen that although the silicone powder only uses TY-609, it can maintain a high frosted touch and matte properties, but the adhesion, hardness and transmittance are all reduced to a certain extent.

[0081] Application Example 1 and Comparative Example By comparing Application Examples 1 and 2, it can be seen that when the acrylic resin adopts a low (2) functional group polyester resin, the frosted feeling of the ink film is weaker, and the light transmittance and extinction performance are reduced; when the acrylic resin adopts a 4-functional group hyperbranched polyester resin, the ink film has no frosted feeling at all. This is because the increase in the branch chain of the polyester resin leads to a decrease in the shrinkage rate of the ink film, making it difficult to form an ink film with a frosted touch.

[0082] Comparing Application Example 1 and Comparative Application Example 3, it can be seen that when only TY-608 is used as silicone powder, the ink film completely loses its frosted feel and the matte performance decreases significantly.

[0083] By comparing Application Example 1 and Comparative Application Examples 4-6, it can be seen that the addition of a small amount of solvent has basically no effect on the mechanical and optical properties of the matte oil, but has a greater impact on the matte touch of the ink film. When a small amount of turpentine is added and combined with the steps of drying and two UV curing, the formula provided in this application can have an obvious matte touch. This may be because turpentine has a certain volatility when drying, and as a solvent itself has a certain positive promoting effect on the performance of the formula of this application.

[0084] The above is only the preferred implementation of the present application. The protection scope of the present application is not limited to the above embodiments. All technical solutions under the concept of the present application belong to the protection scope of the present application. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present application should also be regarded as the protection scope of the present application.

Claims

1. A method for preparing a frosted touch film bag, characterized in that: The following steps are involved: The substrate to be coated is subjected to dust removal, corona treatment, and heating and ironing treatment in sequence, and the matt oil is evenly coated on the surface of the substrate by micro-concave precision coating. The coated substrate is first dried, and then subjected to oxygen-proof UV curing twice to obtain the matt oil. The coating amount of the matt oil on the substrate is 2.8-3.5g / m 2 The energy of the two UV curing processes is 200-500 mj / cm 2 and 1000-1200mj / cm 2 The matt oil comprises the following components in parts by weight: 40-50 parts of pure acrylic resin, 20-30 parts of multifunctional acrylate resin, 30-40 parts of reactive diluent, 1-10 parts of turpentine, 5-10 parts of silicone powder, 1-3 parts of photoinitiator, 0.5-1 parts of leveling agent, and 0.5-1 parts of defoaming agent. The number of functional groups of the multifunctional acrylate resin is 9-15, and the silicone powder comprises at least one of TY-609, TY-610, TY-605, and TY-608.

2. The method for preparing the frosted touch film bag according to claim 1, characterized in that: The multifunctional acrylate resin is Lencolo L-6901 and / or Lencolo L-6902.

3. The method for preparing the frosted touch film bag according to claim 1, characterized in that: The turpentine oil includes at least one of α-pinene, β-pinene and dipentene.

4. The method for preparing the frosted touch film bag according to claim 1, characterized in that: The active diluent includes at least one of tripropylene glycol diacrylate, 2-phenoxyethyl acrylate, isononyl acrylate, ethoxylated bisphenol A dimethacrylate, pentaerythritol triacrylate, ethoxylated trimethylolpropane triacrylate, tris(2-hydroxyethyl)isocyanuric acid triacrylate, dipentaerythritol hexaacrylate, and 1,6-hexanediol diacrylate.

5. The method for preparing the frosted touch film bag according to claim 1, characterized in that: The photoinitiator includes at least one of a free radical photoinitiator and a cationic photoinitiator, the leveling agent includes at least one of BTK-300, BTK-306, BTK-307, BTK-310, BTK-315, BTK-320, BTK-323, BTK-325, and BTK-331, and the defoamer is a polyether-modified silicone defoamer.

6. The method for preparing the frosted touch film bag according to claim 1, characterized in that: The matt oil is prepared by the following steps: weighing each component for use, stirring, sequentially adding pure acrylic resin, multifunctional acrylic resin, reactive diluent, turpentine, leveling agent, photoinitiator, defoamer, and silicone powder, stirring and dispersing evenly, and grinding to obtain the matt oil.

7. A frosted touch film bag prepared by the method according to any one of claims 1 to 6.