A corrosion-resistant composite coating based on fluorescence-induced corrosion and preparation method thereof
By combining composite epoxy resin, loaded kaolin, reinforced silicone and modified fluororesin in corrosion-resistant composite coatings, the color-changing induction corrosion coatings is solved, and the problem of coating insensitivity to the initial corrosion induction of metal substrates is improved. The corrosion-proof performance is improved and wear resistance, achieving efficient protection of coatings and extending the service life of metal materials.
Patent Information
- Application Number
- CN202410569639.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-09
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-05-09
AI Technical Summary
The existing corrosion-resistant composite coatings are not sensitive to the initial corrosion-induced discoloration of metal substrates, and their corrosion resistance, wear resistance and adhesion strength need to be improved.
Using the preparation method of corrosion-resistant composite coating based on fluorescence induction, the color-changing inductive corrosion coating is constructed by combining composite epoxy resin, loaded kaolin, reinforced silicone resin and modified fluororesin, and the hydrophobicity of fluororesin and adhesion of epoxy resin is used. The junction performance is to form a dense hydrophobic layer and an adhesive layer, improve the corrosion resistance of the coating, and improve the dispersion and cross-linking of kaolin through modification treatment.
It achieves the efficient corrosion resistance, wear resistance and adhesion of the coating, and can promptly induce initial corrosion of metals and show fluorescent discoloration, extending the service life of metal materials.
Smart Images

Figure BDA0004830453080000161
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of corrosion-resistant composite coating processing, and in particular to a corrosion-resistant composite coating based on fluorescence-induced corrosion and a preparation method thereof. Background Art
[0002] With the continuous development of industrial technology, metal materials are increasingly used in various fields. In industrial production, metal corrosion is a common problem, which can lead to damage to equipment, components or products and reduce their service life. In order to protect the metal surface from corrosion, people usually use coating technology to cover the metal surface with paint to prevent it from contacting with corrosive media in the environment.
[0003] The existing coating technology mainly forms a coating barrier on the outside of the substrate through coating, isolating the contact between the metal and the external medium, and playing an anti-corrosion effect. However, the coating will inevitably be damaged by the external environment during the curing process and in the use process, such as physical wear, chemical erosion, etc., which will lead to a decrease in the protective ability of the coating and shorten the service life of the metal material. The traditional corrosion-resistant composite coating often cannot reflect the metal corrosion situation, resulting in metal corrosion, especially the initial corrosion of the metal is difficult to be discovered in time. In the prior art, epoxy resin has excellent corrosion resistance, water resistance and wear resistance, and is often used in the research and processing of corrosion-resistant composite coatings. Rhodamine B hydrazide can complex with iron ions and show strong orange-yellow fluorescence. However, the structural difference between rhodamine B hydrazide and epoxy resin is large, and a weak interface will be formed in the coating during the coating forming process. In addition, the dispersibility of rhodamine B hydrazide in epoxy resin is limited, and it is difficult to be evenly dispersed in epoxy resin, resulting in the coating being insensitive to the induction color change of substrate corrosion. The corrosion-resistant composite coating has excellent corrosion resistance, water resistance and wear resistance. The anti-corrosion performance, wear resistance and adhesion strength need to be further improved.
[0004] In view of the technical defects in this aspect, a solution is now proposed. Summary of the invention
[0005] The purpose of the present invention is to provide a corrosion-resistant composite coating based on fluorescent corrosion induction and a preparation method thereof, so as to solve the technical problems in the prior art that the corrosion-resistant composite coating is not sensitive to the initial corrosion induction discoloration of the substrate and the corrosion resistance, wear resistance and adhesion strength of the corrosion-resistant composite coating need to be further improved.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A method for preparing a corrosion-resistant composite coating based on fluorescence-induced corrosion comprises the following steps:
[0008] S1, adding pretreated kaolin, anhydrous ethanol and KH-540 into a reactor and ultrasonically dispersing for 30-50 minutes, raising the temperature of the reactor to 55-65°C, dropping purified water into the reactor, keeping the temperature for reaction for 40-60 minutes, and post-treating to obtain modified kaolin;
[0009] S2, adding modified kaolin, rhodamine B hydrazide and the mixed solution into a reactor and stirring, raising the temperature of the reactor to 55-65° C., stirring for 20-30 min, lowering the temperature of the reactor to room temperature, adding acetone into the reactor, and stirring at this temperature for 30-50 min to obtain loaded kaolin;
[0010] S3, adding bisphenol A epoxy resin, toluene and hydroquinone into a nitrogen-protected reactor, raising the temperature of the reactor to 65-75°C, stirring until the system is dissolved, and dripping a mixed solution of triethylamine and acrylic acid into the reactor. After the dripping is complete, heat the reaction for 4-6 hours, and perform post-treatment to obtain a modified epoxy resin;
[0011] The synthetic reaction principle of modified epoxy resin is:
[0012] With hydroquinone as an inhibitor and triethylamine as an alkaline catalyst, under the catalytic action of the catalyst, the carboxylate ions of acrylic acid attack the epoxy groups of the epoxy resin to cause an addition or esterification reaction. By selecting epoxy resins with different epoxy values, the dosage ratio of the epoxy resin to acrylic acid is optimized and adjusted, and an acrylic acid end-capping modification is formed at one end of the epoxy resin to prepare a modified epoxy resin.
[0013] S4, adding modified epoxy resin, modified siloxane, acrylic acid, tetrahydrofuran and initiator into a nitrogen-protected reactor and stirring, raising the temperature of the reactor to reflux the system, keeping the temperature for 4-5 hours, and post-treating to obtain a composite epoxy resin;
[0014] The synthetic reaction principle of composite epoxy resin is:
[0015] Under the action of a free radical initiator, the olefin double bonds on the modified epoxy resin, modified siloxane and acrylic acid are induced to undergo a free radical polymerization reaction, and the modified epoxy resin, modified siloxane and acrylic acid are polycondensed in the form of polyolefin to form a polymer, and an acid-base neutralization reaction is carried out between the amino group and the carboxyl group in the polymer to form ammonium carboxylate in the polymer, thereby preparing a composite epoxy resin.
[0016] S5. Add composite epoxy resin, reinforced silicone resin, modified fluororesin, loaded kaolin and additives into a reactor, raise the temperature of the reactor to 50-60°C, add toluene into the reactor while stirring, adjust the viscosity of the system to 80-120KU, and obtain a corrosion-resistant composite coating.
[0017] Further, in step S1, the amount ratio of the pretreated kaolin, anhydrous ethanol, KH-540 and purified water is 5g:50mL:1-2g:10mL, and the post-treatment operation includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, filtered, the filter cake is washed 3 times with 50wt% ethanol aqueous solution and then dried, the filter cake is transferred to a drying oven at a temperature of 70-80°C, and vacuum dried to constant weight to obtain modified kaolin; in step S2, the amount ratio of the modified kaolin, rhodamine B hydrazide, mixed solution and acetone is 5g:2-3g:20mL :200mL, the mixed solution is composed of ethanol and dimethyl sulfoxide in a volume ratio of 7:1, the post-processing operation includes: after the reaction is completed, suction filtration, the filter cake is washed with acetone for 3 times and then dried, the filter cake is transferred to a drying oven at a temperature of 65-75°C, and vacuum dried to constant weight to obtain loaded kaolin; in step S3, the amount ratio of the bisphenol A epoxy resin, toluene, hydroquinone, acrylic acid and triethylamine is 100g:500mL:8mL:17g:5g, the model of the bisphenol A epoxy resin is E-51, and the post-processing operation includes: after the reaction is completed After the reaction is completed, the temperature of the reactor is kept at 65-75°C, and the low-boiling point substances are evaporated under reduced pressure to obtain a modified epoxy resin; in step S4, the amount ratio of the modified epoxy resin, modified siloxane, acrylic acid, tetrahydrofuran and initiator is 7-10g:2-5g:1.5-2g:80-100mL:0.3-0.5g, and the initiator is azobisisobutyronitrile. The post-treatment operation includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, ammonia water is added dropwise to the reactor, the pH of the system is adjusted to 6-7, the temperature of the reactor is raised to 60-65°C, and the pressure is reduced. The low-boiling point substances are evaporated to obtain a composite epoxy resin; in step S5, the weight ratio of the composite epoxy resin, reinforced silicone resin, modified fluororesin, loaded kaolin and additives is 70-80:10-20:15-25:5-10:2-3, and the additives are composed of a dispersant, a film-forming aid, a leveling agent, a preservative and a defoaming agent in a ratio of 1:2:1:1, the dispersant is polyoxyethylene ether, the film-forming aid is lauryl alcohol ester, the leveling agent is one or more of polyether polyester modified organosiloxane, polyacrylic acid, and carboxymethyl cellulose, and the preservative is isothiazolinone.
[0018] Further, the pretreated kaolin is processed by the following steps:
[0019] A1. Completely immerse the kaolin in an acid solution at a temperature of 60-70°C, keep the temperature and perform ultrasonic treatment for 60-90 minutes, and then post-treat to obtain acid-leached kaolin;
[0020] A2. Put the acid-leached kaolin into a muffle furnace, increase the temperature of the muffle furnace to 400-450°C, and keep it warm for 3-5 hours. Then, reduce the temperature of the muffle furnace to room temperature, discharge the material, and obtain pretreated kaolin.
[0021] Furthermore, in step A1, the acid solution is composed of 0.4-0.6 mol / L nitric acid and 0.1-0.3 mol / L hydrochloric acid in a volume ratio of 1:3, and the post-treatment operation includes: after the reaction is completed, the temperature of the acid solution is lowered to room temperature, filtered, and the filter cake is transferred to a drying oven at a temperature of 70-80°C, and vacuum dried to constant weight to obtain acid-leached kaolin.
[0022] Furthermore, the preparation method of modified siloxane is: nonamethyl-1-hydroxytetrasiloxane and toluene are added to a nitrogen-protected reactor and stirred, the temperature of the reactor is increased to 60-70°C, 3-isocyanate propylene solution is added dropwise to the reactor, and after the addition is completed, the reaction is kept warm for 60-80 minutes, and the modified siloxane is obtained by post-treatment.
[0023] The synthetic reaction principle of modified siloxane is:
[0024] The hydroxyl end groups on the long siloxane chain segments of nonamethyl-1-hydroxytetrasiloxane undergo condensation reaction with the isocyanate groups of 3-isocyanate propylene to obtain modified siloxane having acryl-end long siloxane chain segments.
[0025] Furthermore, the dosage ratio of nonamethyl-1-hydroxytetrasiloxane to 3-isocyanate propylene is 1 mol:1 mol, the dosage ratio of nonamethyl-1-hydroxytetrasiloxane to toluene is 1 g:4 mL, the 3-isocyanate propylene solution consists of 3-isocyanate propylene and toluene in a weight ratio of 1:1, and the post-treatment operation includes: after the reaction is completed, the temperature of the reactor is increased to 70-80°C, and the solvent is evaporated under reduced pressure to obtain modified siloxane.
[0026] Furthermore, the preparation method of the enhanced silicone resin is as follows: add hexamethyl-1,15-dihydroxyoctasiloxane and tetrahydrofuran into a nitrogen-protected reactor and stir, increase the temperature of the reactor to 50-60°C, add isocyanatepropyltriethoxysilane dropwise into the reactor, and after the addition is complete, keep the reaction warm for 2-3 hours to obtain the enhanced silicone resin.
[0027] The synthetic reaction principle of enhanced silicone resin is:
[0028] The hydroxyl end groups at both ends of the long siloxane chain segment of hexadecyl-1,15-dihydroxyoctasiloxane react with the isocyanate groups on two isocyanatepropyltriethoxysilane molecules respectively to obtain a reinforced silicone resin with a triethoxysilane-terminated long siloxane chain segment.
[0029] Furthermore, the dosage ratio of hexadecyl-1,15-dihydroxyoctasiloxane and isocyanatepropyltriethoxysilane is 1 mol:2 mol, the dosage ratio of hexadecyl-1,15-dihydroxyoctasiloxane and tetrahydrofuran is 1 g:5 mL, and the post-treatment operation includes: after the reaction is completed, distilling off the tetrahydrofuran under reduced pressure to obtain a reinforced silicone resin.
[0030] Furthermore, the preparation method of the modified fluororesin is: adding N-ethyl perfluorooctane sulfonamidoethyl methacrylate, modified epoxy resin, tetrahydrofuran and initiator to a nitrogen-protected reactor and stirring, raising the temperature of the reactor to reflux the system, keeping the reaction temperature for 4-5 hours, and post-treating to obtain the modified fluororesin, wherein the amount ratio of the N-ethyl perfluorooctane sulfonamidoethyl methacrylate, modified epoxy resin, tetrahydrofuran and initiator is 6g:1g:30mL:0.03-0.05g, and the initiator is azobisisobutyronitrile.
[0031] The synthetic reaction principle of modified fluororesin is:
[0032] Under the action of a free radical initiator, a free radical polymerization reaction is initiated between N-ethyl perfluorooctane sulfonamidoethyl methacrylate and the olefin double bonds on the modified epoxy resin molecule, and N-ethyl perfluorooctane sulfonamidoethyl methacrylate and the modified epoxy resin are polycondensed in the form of polyolefin to form a polymer, thereby preparing a modified fluororesin.
[0033] A corrosion-resistant composite coating based on fluorescence induction corrosion, wherein the corrosion-resistant composite coating is prepared by a preparation method of a corrosion-resistant composite coating based on fluorescence induction corrosion.
[0034] The present invention has the following beneficial effects:
[0035] 1. The preparation method of the corrosion-resistant composite coating based on fluorescence-induced corrosion of the present invention uses a composite epoxy resin as a matrix, loaded kaolin as a color-changing sensing matrix, and reinforced silicone resin and modified fluororesin as reinforcing materials to construct a color-changing corrosion-resistant composite coating. By utilizing the difference in surface energy between fluororesin and epoxy resin, the fluororesin with low surface energy migrates to the upper surface of the coating coating, forming a dense hydrophobic layer on the surface of the coating, thereby improving the corrosion resistance of the coating. The bonding layer constructed by the epoxy resin and the reinforced silicone resin can effectively improve the adhesion between the carriers of the coating. In addition, kaolin, as an inorganic filler, is evenly dispersed in the coating, thereby effectively improving the wear resistance of the coating.
[0036] 2. The preparation method of the corrosion-resistant composite coating based on fluorescent induced corrosion of the present invention comprises the following steps: modifying nonamethyltetrasiloxane, acrylic acid and bisphenol A epoxy resin, and using ammonia water and carboxylic acid for acid-base neutralization reaction to form ammonium carboxylate, optimizing the composition ratio of siloxane, ammonium carboxylate and epoxy resin, and preparing composite epoxy resin; bisphenol A epoxy resin itself has good bonding properties, and the introduction of acrylate further improves the polarity and wettability of the composite epoxy resin, thereby enhancing the interaction between the composite epoxy resin and the substrate, and increasing the bonding strength between the composite epoxy resin and the substrate; methyltetrasiloxane has excellent weather resistance and chemical stability, and can improve the chemical corrosion resistance of the coating; and the rigid structure of methyltetrasiloxane can improve the hardness and wear resistance of the coating.
[0037] 3. The preparation method of the corrosion-resistant composite coating based on fluorescent induced corrosion of the present invention comprises the following steps: N-ethyl perfluorooctane sulfonamidoethyl methacrylate and modified epoxy resin are subjected to free radical polymerization reaction to form a fluororesin modified with epoxy resin; when reinforcing the composite epoxy resin, the modified fluororesin can use the epoxy resin as a bridge to improve the dispersibility of the modified fluororesin in the composite epoxy resin, so that the modified fluororesin can be evenly dispersed in the composite epoxy resin; and there is a large polarity difference between the low polarity of the fluororesin itself and the high polarity of the composite epoxy resin, so that the fluororesin can quickly diffuse to the surface of the coating to form a hydrophobic layer on the surface of the coating; during the preparation process, the loaded kaolin is modified by acidification, roasting and amino modification to improve the high polarity. The loading performance and surface activity of kaolin make it possible for rhodamine B hydrazide to be uniformly dispersed and loaded on kaolin to prepare loaded kaolin. The treated modified kaolin introduces new functional groups on the kaolin, changes the surface properties and structure of the kaolin, and makes the modified kaolin uniformly dispersed in the epoxy resin. The rhodamine B hydrazide is uniformly dispersed by the loaded accompanying kaolin, so that the rhodamine B hydrazide can be uniformly dispersed in the epoxy resin, thereby improving its fluorescence sensing effect; the epoxy group on the epoxy resin and the isocyanate group on the reinforced silicone resin can react with the active amino group modified on the surface of the loaded kaolin to form chemical crosslinking, thereby improving the crosslinking degree of the coating, and further improving the wear resistance, adhesion and corrosion resistance of the coating. DETAILED DESCRIPTION
[0038] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] Example 1
[0040] This embodiment provides a method for preparing a corrosion-resistant composite coating based on fluorescent induction corrosion, comprising the following steps:
[0041] S1. Preparation of pretreated kaolin
[0042] Mix 0.4 mol / L nitric acid and 0.1 mol / L hydrochloric acid in a volume ratio of 1:3 to obtain an acid solution for later use;
[0043] The kaolin was completely immersed in an acid solution at a temperature of 60°C, and the temperature was kept and ultrasonicated for 60 minutes. After the reaction was completed, the temperature of the acid solution was lowered to room temperature, and the filter cake was transferred to a drying oven at a temperature of 70°C and vacuum dried to constant weight to obtain acid-leached kaolin;
[0044] The acid-leached kaolin was placed in a muffle furnace, the temperature of the muffle furnace was raised to 400°C, and the temperature was kept for 3 hours. The temperature of the muffle furnace was lowered to room temperature, and the material was discharged to obtain pretreated kaolin.
[0045] S2. Preparation of loaded kaolin
[0046] Weigh: 50 g of pretreated kaolin, 500 mL of anhydrous ethanol and 10 g of KH-540 are added to a reactor for ultrasonic dispersion for 30 min, the temperature of the reactor is raised to 55° C., 100 mL of purified water is added dropwise to the reactor, and the reaction is kept warm for 40 min. After the reaction is completed, the temperature of the reactor is lowered to room temperature, filtered, the filter cake is washed 3 times with 50 wt% ethanol aqueous solution and then dried, the filter cake is transferred to a drying oven at a temperature of 70° C., and vacuum dried to constant weight to obtain modified kaolin;
[0047] Ethanol and dimethyl sulfoxide were mixed uniformly in a volume ratio of 7:1 to obtain a mixed solution for later use;
[0048] Weigh: 50 g of modified kaolin, 20 g of rhodamine B hydrazide and 200 mL of the mixed solution, add them into the reactor and stir, raise the temperature of the reactor to 55 ° C, stir for 20 minutes, lower the temperature of the reactor to room temperature, add 2000 mL of acetone to the reactor, keep warm and stir for 30 minutes, after the reaction is completed, filter, wash the filter cake with acetone 3 times and then dry it, transfer the filter cake to a drying oven at a temperature of 65 ° C, and vacuum dry it to constant weight to obtain loaded kaolin.
[0049] S3. Preparation of modified epoxy resin
[0050] Weigh: 1200g of bisphenol A epoxy resin E-5, 1000mL of toluene, and 16mL of hydroquinone, add them into a nitrogen-protected reactor, raise the temperature of the reactor to 65°C, stir until the system is dissolved, and drop a mixed solution consisting of 10g of triethylamine and 34g of acrylic acid into the reactor. After the addition is complete, keep the temperature for 4h. After the reaction is completed, keep the reactor temperature at 65°C, and evaporate the low-boiling point substances under reduced pressure to obtain a modified epoxy resin.
[0051] S4. Preparation of composite epoxy resin
[0052] Weigh: 312.7 g of nonamethyl-1-hydroxytetrasiloxane and 1250.8 mL of toluene are added to a nitrogen-protected reactor and stirred. The temperature of the reactor is raised to 60° C., and a 3-isocyanate propylene solution consisting of 83.1 g of 3-isocyanate propylene and 83.1 g of toluene is added dropwise to the reactor. After the addition is complete, the reaction is kept warm for 60 minutes. After the reaction is completed, the temperature of the reactor is raised to 70° C., and the solvent is evaporated under reduced pressure to obtain modified siloxane;
[0053] Weigh: 140 g of modified epoxy resin, 40 g of modified siloxane, 30 g of acrylic acid, 1600 mL of tetrahydrofuran and 6 g of azobisisobutyronitrile, add them into a nitrogen-protected reactor and stir, raise the temperature of the reactor to reflux the system, and keep the reaction warm for 4 hours. After the reaction is completed, lower the temperature of the reactor to room temperature, add ammonia water dropwise to the reactor, adjust the pH of the system to 6, raise the temperature of the reactor to 60°C, and evaporate low-boiling substances under reduced pressure to obtain a composite epoxy resin.
[0054] S5. Preparation of reinforced silicone resin
[0055] Weigh: 122.3 g of hexamethyl-1,15-dihydroxyoctasiloxane and 611.5 mL of tetrahydrofuran are added into a nitrogen-protected reactor with stirring. The temperature of the reactor is raised to 50°C. 98.9 g of isocyanatepropyltriethoxysilane is added dropwise into the reactor. After the addition is complete, the reaction is kept warm for 2 hours. After the reaction is completed, the tetrahydrofuran is evaporated under reduced pressure to obtain a reinforced silicone resin.
[0056] S6. Preparation of modified fluororesin
[0057] Weigh: 60 g of N-ethyl perfluorooctanesulfonamidoethyl methacrylate, 10 g of modified epoxy resin, 300 mL of tetrahydrofuran and 0.3 g of azobisisobutyronitrile, add into a nitrogen-protected reactor and stir, raise the temperature of the reactor to reflux the system, keep the reaction warm for 4 hours, and after the reaction is completed, evaporate the solvent under reduced pressure to obtain a modified fluororesin.
[0058] S7. Preparation of corrosion-resistant composite coating
[0059] Mix polyoxyethylene ether, lauryl alcohol ester, polyether polyester modified organosiloxane and isothiazolinone in a ratio of 1:2:1:1 to obtain an additive, which is set aside;
[0060] Weigh: 700g of composite epoxy resin, 100g of reinforced silicone resin, 150g of modified fluororesin, 50g of loaded kaolin and 20g of additives and add them into a reactor. The temperature of the reactor is raised to 50°C. Toluene is added to the reactor while stirring. The viscosity of the system is adjusted to 80KU to obtain a corrosion-resistant composite coating.
[0061] Example 2
[0062] This embodiment provides a method for preparing a corrosion-resistant composite coating based on fluorescent induction corrosion, comprising the following steps:
[0063] S1. Preparation of pretreated kaolin
[0064] 0.5 mol / L nitric acid and 0.2 mol / L hydrochloric acid were mixed uniformly in a volume ratio of 1:3 to obtain an acid solution for later use;
[0065] The kaolin was completely immersed in an acid solution at a temperature of 65°C, and the temperature was kept and ultrasonicated for 75 minutes. After the reaction was completed, the temperature of the acid solution was lowered to room temperature, and the filter cake was transferred to a drying oven at a temperature of 75°C and vacuum dried to constant weight to obtain acid-leached kaolin;
[0066] The acid-leached kaolin was placed in a muffle furnace, the temperature of the muffle furnace was raised to 425°C, and the temperature was kept for 4 hours. The temperature of the muffle furnace was lowered to room temperature, and the material was discharged to obtain pretreated kaolin.
[0067] S2. Preparation of loaded kaolin
[0068] Weigh: 50 g of pretreated kaolin, 500 mL of anhydrous ethanol and 15 g of KH-540 are added to a reactor for ultrasonic dispersion for 40 min, the temperature of the reactor is raised to 60° C., 100 mL of purified water is added dropwise to the reactor, and the reaction is kept warm for 50 min. After the reaction is completed, the temperature of the reactor is lowered to room temperature, filtered, the filter cake is washed 3 times with 50 wt% ethanol aqueous solution and then dried, the filter cake is transferred to a drying oven at a temperature of 75° C., and vacuum dried to constant weight to obtain modified kaolin;
[0069] Ethanol and dimethyl sulfoxide were mixed uniformly in a volume ratio of 7:1 to obtain a mixed solution for later use;
[0070] Weigh: 50 g of modified kaolin, 25 g of rhodamine B hydrazide and 200 mL of the mixed solution, add them into the reactor and stir, raise the temperature of the reactor to 60 ° C, stir for 25 minutes, lower the temperature of the reactor to room temperature, add 2000 mL of acetone to the reactor, keep warm and stir for 40 minutes, after the reaction is completed, filter, wash the filter cake with acetone 3 times and then dry it, transfer the filter cake to a drying oven at a temperature of 70 ° C, and vacuum dry it to constant weight to obtain loaded kaolin.
[0071] S3. Preparation of modified epoxy resin
[0072] Weigh: 1200 g of bisphenol A epoxy resin E-5, 1000 mL of toluene, and 16 mL of hydroquinone, add them into a nitrogen-protected reactor, raise the temperature of the reactor to 70°C, stir until the system is dissolved, and drop a mixed solution consisting of 10 g of triethylamine and 34 g of acrylic acid into the reactor. After the addition is complete, keep the temperature for reaction for 5 hours. After the reaction is completed, keep the reactor temperature at 70°C, and evaporate the low-boiling point substances under reduced pressure to obtain a modified epoxy resin.
[0073] S4. Preparation of composite epoxy resin
[0074] Weigh: 312.7 g of nonamethyl-1-hydroxytetrasiloxane and 1250.8 mL of toluene are added to a nitrogen-protected reactor and stirred. The temperature of the reactor is raised to 65° C., and a 3-isocyanate propylene solution consisting of 83.1 g of 3-isocyanate propylene and 83.1 g of toluene is added dropwise to the reactor. After the addition is complete, the reaction is kept warm for 70 minutes. After the reaction is completed, the temperature of the reactor is raised to 75° C., and the solvent is evaporated under reduced pressure to obtain modified siloxane;
[0075] Weigh: 170 g of modified epoxy resin, 70 g of modified siloxane, 35 g of acrylic acid, 1800 mL of tetrahydrofuran and 8 g of azobisisobutyronitrile, add them into a nitrogen-protected reactor and stir, raise the temperature of the reactor to reflux the system, and keep the reaction warm for 4.5 hours. After the reaction is completed, lower the temperature of the reactor to room temperature, add ammonia water dropwise to the reactor, adjust the pH of the system to 6.5, raise the temperature of the reactor to 63°C, and evaporate low-boiling substances under reduced pressure to obtain a composite epoxy resin.
[0076] S5. Preparation of reinforced silicone resin
[0077] Weigh: 122.3 g of hexamethyl-1,15-dihydroxyoctasiloxane and 611.5 mL of tetrahydrofuran are added into a nitrogen-protected reactor with stirring. The temperature of the reactor is raised to 55°C. 98.9 g of isocyanatepropyltriethoxysilane is added dropwise into the reactor. After the addition is complete, the reaction is kept warm for 2.5 hours. After the reaction is completed, the tetrahydrofuran is evaporated under reduced pressure to obtain a reinforced silicone resin.
[0078] S6. Preparation of modified fluororesin
[0079] Weigh: 60 g of N-ethyl perfluorooctanesulfonamidoethyl methacrylate, 10 g of modified epoxy resin, 300 mL of tetrahydrofuran and 0.4 g of azobisisobutyronitrile, add into a nitrogen-protected reactor and stir, raise the temperature of the reactor to reflux the system, keep the reaction warm for 4.5 hours, and after the reaction is completed, evaporate the solvent under reduced pressure to obtain a modified fluororesin.
[0080] S7. Preparation of corrosion-resistant composite coating
[0081] Mix polyoxyethylene ether, lauryl alcohol ester, polyacrylic acid and isothiazolinone in a ratio of 1:2:1:1 to obtain an additive, which is set aside;
[0082] Weigh: 750g of composite epoxy resin, 150g of reinforced silicone resin, 200g of modified fluororesin, 75g of loaded kaolin and 25g of additives and add them into a reactor. Raise the temperature of the reactor to 55°C, add toluene to the reactor while stirring, adjust the viscosity of the system to 100KU, and obtain a corrosion-resistant composite coating.
[0083] Example 3
[0084] This embodiment provides a method for preparing a corrosion-resistant composite coating based on fluorescent induction corrosion, comprising the following steps:
[0085] S1. Preparation of pretreated kaolin
[0086] Mix 0.6 mol / L nitric acid and 0.3 mol / L hydrochloric acid in a volume ratio of 1:3 to obtain an acid solution for later use;
[0087] The kaolin was completely immersed in an acid solution at a temperature of 70°C, and the temperature was kept and ultrasonicated for 90 minutes. After the reaction was completed, the temperature of the acid solution was lowered to room temperature, and the filter cake was transferred to a drying oven at a temperature of 80°C and vacuum dried to constant weight to obtain acid-leached kaolin;
[0088] The acid-leached kaolin was placed in a muffle furnace, the temperature of the muffle furnace was increased to 450°C, and the temperature was kept for 5 hours. The temperature of the muffle furnace was lowered to room temperature, and the material was discharged to obtain pretreated kaolin.
[0089] S2. Preparation of loaded kaolin
[0090] Weigh: 50 g of pretreated kaolin, 500 mL of anhydrous ethanol and 20 g of KH-540 are added to a reactor for ultrasonic dispersion for 50 min, the temperature of the reactor is raised to 65° C., 100 mL of purified water is added dropwise to the reactor, and the reaction is kept warm for 60 min. After the reaction is completed, the temperature of the reactor is lowered to room temperature, filtered, the filter cake is washed 3 times with 50 wt% ethanol aqueous solution and then dried, the filter cake is transferred to a drying oven at a temperature of 80° C., and vacuum dried to constant weight to obtain modified kaolin;
[0091] Ethanol and dimethyl sulfoxide were mixed uniformly in a volume ratio of 7:1 to obtain a mixed solution for later use;
[0092] Weigh: 50 g of modified kaolin, 30 g of rhodamine B hydrazide and 200 mL of the mixed solution, add them into the reactor and stir, raise the temperature of the reactor to 65 ° C, stir for 30 minutes, lower the temperature of the reactor to room temperature, add 2000 mL of acetone to the reactor, keep warm and stir for 50 minutes, after the reaction is completed, filter, wash the filter cake with acetone 3 times and then dry it, transfer the filter cake to a drying oven at a temperature of 75 ° C, and vacuum dry it to constant weight to obtain loaded kaolin.
[0093] S3. Preparation of modified epoxy resin
[0094] Weigh: 1200g of bisphenol A epoxy resin E-5, 1000mL of toluene, and 16mL of hydroquinone, add them into a nitrogen-protected reactor, raise the temperature of the reactor to 75°C, stir until the system is dissolved, and drop a mixed solution consisting of 10g of triethylamine and 34g of acrylic acid into the reactor. After the addition is complete, keep the temperature for reaction for 6h. After the reaction is completed, keep the reactor temperature at 75°C, and evaporate the low-boiling point substances under reduced pressure to obtain a modified epoxy resin.
[0095] S4. Preparation of composite epoxy resin
[0096] Weigh: 312.7 g of nonamethyl-1-hydroxytetrasiloxane and 1250.8 mL of toluene are added to a nitrogen-protected reactor and stirred. The temperature of the reactor is raised to 70° C., and a 3-isocyanate propylene solution consisting of 83.1 g of 3-isocyanate propylene and 83.1 g of toluene is added dropwise to the reactor. After the addition is complete, the reaction is carried out by heat preservation for 80 minutes. After the reaction is completed, the temperature of the reactor is raised to 80° C., and the solvent is evaporated under reduced pressure to obtain modified siloxane;
[0097] Weigh: 200 g of modified epoxy resin, 100 g of modified siloxane, 40 g of acrylic acid, 2000 mL of tetrahydrofuran and 10 g of azobisisobutyronitrile, add them into a nitrogen-protected reactor and stir, raise the temperature of the reactor to reflux the system, and keep the reaction warm for 5 hours. After the reaction is completed, lower the temperature of the reactor to room temperature, add ammonia water dropwise to the reactor, adjust the pH of the system to 7, raise the temperature of the reactor to 65°C, and remove low-boiling substances under reduced pressure to obtain a composite epoxy resin.
[0098] S5. Preparation of reinforced silicone resin
[0099] Weigh: 122.3 g of hexamethyl-1,15-dihydroxyoctasiloxane and 611.5 mL of tetrahydrofuran are added into a nitrogen-protected reactor with stirring. The temperature of the reactor is raised to 60°C. 98.9 g of isocyanatepropyltriethoxysilane is added dropwise into the reactor. After the addition is complete, the reaction is kept warm for 3 hours. After the reaction is completed, the tetrahydrofuran is evaporated under reduced pressure to obtain a reinforced silicone resin.
[0100] S6. Preparation of modified fluororesin
[0101] Weigh: 60 g of N-ethyl perfluorooctanesulfonamidoethyl methacrylate, 10 g of modified epoxy resin, 300 mL of tetrahydrofuran and 0.5 g of azobisisobutyronitrile, add into a nitrogen-protected reactor and stir, raise the temperature of the reactor to reflux the system, keep the reaction warm for 5 hours, and after the reaction is completed, evaporate the solvent under reduced pressure to obtain a modified fluororesin.
[0102] S7. Preparation of corrosion-resistant composite coating
[0103] Mix polyoxyethylene ether, lauryl alcohol ester, carboxymethyl cellulose and isothiazolinone in a ratio of 1:2:1:1 to obtain an additive, which is set aside;
[0104] Weigh: 800g of composite epoxy resin, 200g of reinforced silicone resin, 250g of modified fluororesin, 100g of loaded kaolin and 30g of additives and add them into a reactor. The temperature of the reactor is raised to 60°C. Toluene is added to the reactor while stirring. The viscosity of the system is adjusted to 120KU to obtain a corrosion-resistant composite coating.
[0105] Comparative Example 1
[0106] The difference between this comparison and Example 3 is that step S1 is eliminated, and the pretreated kaolin in step S2 is replaced by the kaolin in step S1.
[0107] Comparative Example 2
[0108] The difference between this comparison and Example 3 is that in step S4, when preparing the composite epoxy resin, no modified siloxane is added.
[0109] Comparative Example 3
[0110] The difference between this comparison and Example 3 is that step S5 is eliminated and no reinforcing silicone resin is added in step S7.
[0111] Comparative Example 4
[0112] The difference between this comparison and Example 3 is that step S6 is eliminated, and the modified fluororesin in step S7 is replaced by N-ethyl perfluorooctanesulfonamidoethyl methacrylate in step S6.
[0113] Performance Testing:
[0114] The wear resistance, adhesion, anti-corrosion performance and inductive color change performance of the corrosion-resistant composite coatings prepared in Examples 1-3 and Comparative Examples 1-4 were tested, wherein the wear resistance was measured according to the standard GB / T 1768-2006 "Determination of the wear resistance of paints and varnishes - Rotating rubber grinding wheel method" to determine the average number of revolutions required for the coating to be worn through; the adhesion was measured according to the standard GB / T 5210-2006 "Adhesion test of paints and varnishes by pull-off method" to determine the destructive strength of the damaged coating; the anti-corrosion performance was measured according to the standard GB / T30790.6-2014 "Corrosion protection of steel structures by protective coating systems of paints and varnishes - Part 6: Laboratory performance test methods" to determine the durability grade of the specimen after the specimen coating was formed on the steel substrate in a C3 corrosion environment; the inductive color change performance was measured according to the standard GB / T The minimum corrosion level of carbon steel when the coating changes color fluorescently is observed on carbon steel materials of different corrosion levels specified in 19292.2-2018 "Atmospheric Corrosion of Metals and Alloys Part 2: Guidance Values of Corrosion Levels". The specific test results are shown in Table 1 below:
[0115] Table 1.
[0116]
[0117] Data Analysis:
[0118] A comparative analysis of the data in Table 1 above shows that the average number of revolutions required for the coating of the corrosion-resistant composite coating prepared by the present invention to be worn through reaches 8200 revolutions, the destructive strength of the coating reaches 25.1 MPa, the durability grade reaches high level, and the minimum corrosion grade of carbon steel during fluorescent color change reaches C1 level, which can sense the initial corrosion of metal materials by color change, and various performance tests are better than the control example as a whole. This shows that the present invention uses a composite epoxy resin as a matrix, loaded kaolin as a color change sensing matrix, and reinforced silicone resin and modified fluororesin as reinforcing materials to construct a color change sensing corrosion anti-corrosion coating, which can not only effectively sense the early corrosion of metal materials by fluorescent color change, but also effectively improve the anti-corrosion performance, wear resistance and bonding strength of the anti-corrosion coating.
[0119] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
[0120] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0121] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for preparing a corrosion-resistant composite coating based on fluorescence-induced corrosion, characterized in that: The following steps are involved: S1, adding pretreated kaolin, anhydrous ethanol and KH-540 into a reactor and ultrasonically dispersing for 30-50 minutes, raising the temperature of the reactor to 55-65°C, dropping purified water into the reactor, keeping the temperature for reaction for 40-60 minutes, and post-treating to obtain modified kaolin; S2, adding modified kaolin, rhodamine B hydrazide and the mixed solution into a reactor and stirring, raising the temperature of the reactor to 55-65° C., stirring for 20-30 min, lowering the temperature of the reactor to room temperature, adding acetone into the reactor, and stirring at this temperature for 30-50 min to obtain loaded kaolin; S3, adding bisphenol A epoxy resin, toluene and hydroquinone into a nitrogen-protected reactor, raising the temperature of the reactor to 65-75°C, stirring until the system is dissolved, and dripping a mixed solution of triethylamine and acrylic acid into the reactor. After the dripping is complete, heat the reaction for 4-6 hours, and perform post-treatment to obtain a modified epoxy resin; S4, adding modified epoxy resin, modified siloxane, acrylic acid, tetrahydrofuran and initiator into a nitrogen-protected reactor and stirring, raising the temperature of the reactor to reflux the system, keeping the temperature for reaction for 4-5 hours, and post-treating to obtain a composite epoxy resin, wherein the post-treating operation includes: after the reaction is completed, lowering the temperature of the reactor to room temperature, adding ammonia water to the reactor, adjusting the pH of the system to 6-7, raising the temperature of the reactor to 60-65°C, and removing low-boiling substances under reduced pressure to obtain a composite epoxy resin; S5, adding composite epoxy resin, reinforced silicone resin, modified fluororesin, loaded kaolin and additives into a reactor, raising the temperature of the reactor to 50-60° C., adding toluene into the reactor while stirring, adjusting the viscosity of the system to 80-120 KU, and obtaining a corrosion-resistant composite coating; The preparation method of modified siloxane is as follows: nonamethyl-1-hydroxytetrasiloxane and toluene are added to a nitrogen-protected reactor and stirred, the temperature of the reactor is increased to 60-70° C., 3-isocyanate propylene solution is added dropwise to the reactor, and after the addition is completed, the reaction is carried out by heat preservation for 60-80 minutes, and the modified siloxane is obtained by post-treatment; The preparation method of the enhanced silicone resin is as follows: hexamethyl-1,15-dihydroxyoctasiloxane and tetrahydrofuran are added into a nitrogen-protected reactor and stirred, the temperature of the reactor is raised to 50-60° C., isocyanatepropyltriethoxysilane is added dropwise into the reactor, and after the addition is completed, the reaction is carried out by heat preservation for 2-3 hours to obtain the enhanced silicone resin; The preparation method of the modified fluororesin is as follows: N-ethyl perfluorooctanesulfonamidoethyl methacrylate, modified epoxy resin, tetrahydrofuran and initiator are added into a nitrogen-protected reactor and stirred, the temperature of the reactor is increased to reflux, the reaction is kept warm for 4-5 hours, and the modified fluororesin is obtained by post-treatment.
2. The method for preparing a corrosion-resistant composite coating based on fluorescent induction corrosion according to claim 1, characterized in that: In step S1, the amount ratio of the pretreated kaolin, anhydrous ethanol, KH-540 and purified water is 5g:50mL:1-2g:10mL; in step S2, the amount ratio of the modified kaolin, rhodamine B hydrazide, mixed solution and acetone is 5g:2-3g:20mL:200mL, and the mixed solution is composed of ethanol and dimethyl sulfoxide in a volume ratio of 7:1; in step S3, the amount ratio of the bisphenol A epoxy resin, toluene, hydroquinone, acrylic acid and triethylamine is 100g:500mL:8mL:17g:5g, and the model of the bisphenol A epoxy resin is E-51; in step S4, the modified epoxy resin, modified siloxane, acrylic acid, The dosage ratio of tetrahydrofuran and initiator is 7-10g:2-5g:1.5-2g:80-100mL:0.3-0.5g, and the initiator is azobisisobutyronitrile; in step S5, the weight ratio of the composite epoxy resin, reinforced silicone resin, modified fluororesin, loaded kaolin and additives is 70-80:10-20:15-25:5-10:2-3, and the additives are composed of a dispersant, a film-forming aid, a leveling agent, and a preservative in a ratio of 1:2:1:1, the dispersant is polyoxyethylene ether, the film-forming aid is dodecanol ester, the leveling agent is one or more of polyether polyester modified organic siloxane, polyacrylic acid, and carboxymethyl cellulose, and the preservative is isothiazolinone.
3. The method for preparing a corrosion-resistant composite coating based on fluorescent induction corrosion according to claim 1, characterized in that: Pretreated kaolin is processed by the following steps: A1. Completely immerse the kaolin in an acid solution at a temperature of 60-70°C, keep the temperature and perform ultrasonic treatment for 60-90 minutes, and then post-treat to obtain acid-leached kaolin; A2. Put the acid-leached kaolin into a muffle furnace, increase the temperature of the muffle furnace to 400-450°C, and keep it warm for 3-5 hours. Then, reduce the temperature of the muffle furnace to room temperature, discharge the material, and obtain pretreated kaolin.
4. The method for preparing a corrosion-resistant composite coating based on fluorescent induction corrosion according to claim 3 is characterized in that: In step A1, the acid solution is composed of 0.4-0.6 mol / L nitric acid and 0.1-0.3 mol / L hydrochloric acid in a volume ratio of 1:
3.
5. The method for preparing a corrosion-resistant composite coating based on fluorescent induction corrosion according to claim 1, characterized in that: The usage ratio of nonamethyl-1-hydroxytetrasiloxane and 3-isocyanate propylene is 1 mol:1 mol, the usage ratio of nonamethyl-1-hydroxytetrasiloxane and toluene is 1 g:4 mL, and the 3-isocyanate propylene solution consists of 3-isocyanate propylene and toluene in a weight ratio of 1:
1.
6. The method for preparing a corrosion-resistant composite coating based on fluorescent induction corrosion according to claim 1, characterized in that: The usage ratio of hexadecyl-1,15-dihydroxyoctasiloxane to isocyanatepropyltriethoxysilane is 1 mol:2 mol, and the usage ratio of hexadecyl-1,15-dihydroxyoctasiloxane to tetrahydrofuran is 1 g:5 mL.
7. The method for preparing a corrosion-resistant composite coating based on fluorescent induction corrosion according to claim 1, characterized in that: In the preparation process of the modified fluororesin, the usage ratio of N-ethyl perfluorooctanesulfonamidoethyl methacrylate, modified epoxy resin, tetrahydrofuran and initiator is 6g:1g:30mL:0.03-0.05g, and the initiator is azobisisobutyronitrile.
8. A corrosion-resistant composite coating based on fluorescent induction corrosion, characterized in that: The corrosion-resistant composite coating is prepared by the method for preparing a corrosion-resistant composite coating based on fluorescence-induced corrosion as described in any one of claims 1 to 7.