Heat-resistant and shear-resistant organic boron and zirconium composite cross-linking agent for oil field fracturing and preparation method thereof

A composite cross-linking agent with polyvinyl alcohol, zirconium hydroxide, ferrocene modifier, and nano boron nitride improves heat and shear resistance, stabilizing fracturing fluids for efficient oilfield operations.

CN118620598BActive Publication Date: 2024-12-03东营江源化工有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411079408.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-12-03
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

Existing cross-linking agents for oilfield fracturing lack both heat resistance and shear resistance, affecting the efficiency of fracturing fluids.

Method used

A composite cross-linking agent composed of polyvinyl alcohol, zirconium hydroxide, ferrocene modifier, nano boron nitride, and water, prepared through specific chemical reactions to enhance heat and shear resistance.

Benefits of technology

The composite cross-linking agent exhibits improved heat resistance and shear resistance, enhancing the stability and efficiency of fracturing fluids under high temperature and shear conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118620598B_ABST
    Figure CN118620598B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of oilfield fracturing, and discloses a heat-resistant and shear-resistant organic boron and zirconium composite crosslinking agent for oilfield fracturing and a preparation method. The invention provides a heat-resistant and shear-resistant organic boron and zirconium composite crosslinking agent for oilfield fracturing by adding polyvinyl alcohol, zirconium hydroxide, ferrocene modifier, nano boron nitride and water into a stirring container and stirring at room temperature. During the stirring process, the terminal isocyanate in the ferrocene modifier reacts with the surface hydroxyl group of the nano boron nitride, and crosslinks with each other to form a tight network, so that the shear resistance is better, and the boron nitride has good high temperature resistance in the fracturing fluid, and has good thermal conductivity, so that the oil recovery efficiency is improved, and the polyurethane contained therein can also improve the high temperature resistance of the crosslinking agent, and the polyurethane chain forms a crosslinking effect with the polyvinyl alcohol and the nano boron nitride, so that the connection is more dense, and the shear resistance is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oilfield fracturing, in particular to a temperature-resistant and shear-resistant organic boron and zirconium composite crosslinking agent for oilfield fracturing and a preparation method thereof. Background Art

[0002] Oilfield fracturing technology is an important measure to increase the production of oil and gas wells. It uses a ground high-pressure pump group to pump fracturing fluid into the formation at a displacement that greatly exceeds the absorption capacity of the formation, forming cracks in the formation, improving the conductivity of the oil and gas layer, and thus achieving the purpose of increasing production. The selection of cross-linking agents in the acidic fracturing fluid system in the prior art plays a key role in the performance of the fracturing fluid. If the cross-linking agent has poor heat resistance and shear resistance, it will affect the efficiency of oil production. Patent CN111943990B discloses an organic aluminum zirconium boron cross-linking agent and a preparation method thereof, and an acidic guar gum fracturing fluid. The organic aluminum zirconium boron cross-linking agent has excellent heat resistance. However, the cross-linking agent and the fracturing fluid do not show good shear resistance. The present invention compounds an organic boron cross-linking agent with raw materials such as zirconium hydroxide and nano boron nitride to prepare a composite cross-linking agent with heat resistance and shear resistance. Summary of the invention

[0003] 1. Technical issues to be resolved

[0004] In view of the deficiencies in the prior art, the present invention provides a heat-resistant and shear-resistant organic boron and zirconium composite cross-linking agent for oilfield fracturing, which has good heat resistance and shear resistance.

[0005] (II) Technical solution

[0006] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a heat-resistant and shear-resistant organic boron and zirconium composite cross-linking agent for oilfield fracturing, comprising the following components by weight: 4-8 parts by weight of polyvinyl alcohol, 1-2 parts by weight of zirconium hydroxide, 2-5 parts by weight of ferrocene modifier, 2-3 parts by weight of nano boron nitride, and 4-6 parts by weight of water.

[0007] Preferably, the preparation method of the ferrocene modifier is:

[0008] (1) Add ferrocenylboric acid to toluene solvent, stir and disperse, then add N-methyl-2-hydroxyethylamine, react at 110-130°C for 10-14h. After the reaction is completed, distill under reduced pressure, filter and dry to obtain an intermediate.

[0009] (2) Add the intermediate and 3-chloropropylene to N,N-dimethylformamide solvent, stir and disperse, react at 65-80°C for 12-20h, then continue to add sodium 3-chloro-2-hydroxypropanesulfonate, react at 70-90°C for 6-8h, and then distill under reduced pressure and filter to obtain olefinated ferrocene.

[0010] (3) Under a nitrogen atmosphere, add olefinic polyurethane, olefinic ferrocene, and methyl acrylate into a reactor, stir evenly, and continue to add azobisisobutyronitrile initiator, react at 90-110°C for 12-16h, cool to room temperature, wash with deionized water, and dry to obtain a ferrocene modifier.

[0011] Preferably, the mass ratio of ferrocenylboric acid to N-methyl-2-hydroxyethylamine in (1) is 1:1.3-1.6.

[0012] Preferably, the mass ratio of the intermediate, 3-chloropropylene and sodium 3-chloro-2-hydroxypropanesulfonate in (2) is 1:(2.1-2.4):(1.4-1.8).

[0013] Preferably, the mass ratio of olefinic polyurethane, olefinic ferrocene, methyl acrylate and azobisisobutyronitrile initiator in (3) is (1.1-1.2):1:(1.3-1.5):(0.02-0.03).

[0014] Preferably, the preparation method of the olefinic polyurethane in (3) is as follows: add 1.6-5.1 g of purified polyurethane particles to dimethylformamide solvent, stir and dissolve at 85-110° C. for 6-10 h, dry after completion, continue to add 2.4-3.1 g of methyl methacrylate isothiocyanate, introduce nitrogen for protection, then add 0.01-0.03 g of triethylamine, and oil bath at 50-70° C. for 8-10 h. After the reaction, wash with acetonitrile and dry to obtain the olefinic polyurethane.

[0015] Preferably, the preparation method of the heat-resistant and shear-resistant organic boron and zirconium composite cross-linking agent for oilfield fracturing comprises the following steps: adding polyvinyl alcohol, zirconium hydroxide, ferrocene modifier, nano boron nitride and water into a stirring container, stirring at room temperature for 15-20 minutes, and obtaining the heat-resistant and shear-resistant organic boron and zirconium composite cross-linking agent for oilfield fracturing.

[0016] 3. Beneficial technical effects

[0017] The invention prepares a heat-resistant and shear-resistant organic boron and zirconium composite crosslinking agent for oilfield fracturing by adding polyvinyl alcohol, zirconium hydroxide, ferrocene modifier, nano boron nitride and water into a stirring container and stirring at room temperature.

[0018] The boric acid group in ferrocenylboric acid reacts with the hydroxyl group in N-methyl-2-hydroxyethylamine, and a secondary amine group is introduced to obtain an intermediate, which is then further reacted with the chlorine in 3-chloropropylene to introduce a tertiary amine group, and then reacted with the chlorine in sodium 3-chloro-2-hydroxypropanesulfonate to generate a quaternary ammonium salt group, and a hydroxyl group and a sulfonic acid group are introduced to obtain olefinated ferrocene; olefinated polyurethane, olefinated ferrocene, and methyl acrylate are copolymerized under the action of an azobisisobutyronitrile initiator to obtain a ferrocene modifier.

[0019] During the stirring process, the terminal isocyanate in the ferrocene modifier will react with the hydroxyl group in the nano-boron nitride, and they will cross-link with each other to form a tight network, making it more resistant to shearing. Boron nitride has good high temperature resistance in the fracturing fluid, and also has good thermal conductivity, which improves the oil recovery efficiency. The ferrocene contained therein can also promote cross-linking to improve its fracturing effect, and the quaternary ammonium salt therein can improve the stability of the fracturing fluid. The polyurethane contained therein can also improve the high temperature resistance of the cross-linking agent, and the polyurethane chain will form a cross-linking effect with polyvinyl alcohol and nano-boron nitride, making the connection denser and improving its shear resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is the reaction formula for the preparation of olefinated ferrocene. DETAILED DESCRIPTION

[0021] Example 1

[0022] (1) Add 1 g of ferrocenylboric acid to 50 mL of toluene solvent, stir and disperse, then add 1.3 g of N-methyl-2-hydroxyethylamine, react at 110°C for 10 h. After the reaction is completed, evaporate under reduced pressure, filter and dry to obtain an intermediate.

[0023] (2) Add 1.2 g of the intermediate and 2.52 g of 3-chloropropylene to 60 mL of N,N-dimethylformamide solvent, stir and disperse, react at 65 °C for 12 h, then continue to add 1.68 g of sodium 3-chloro-2-hydroxypropanesulfonate, react at 70 °C for 6 h, and then distill under reduced pressure and filter to obtain olefinated ferrocene.

[0024] (3) Add 1.6 g of purified polyurethane particles to 80 mL of dimethylformamide solvent, stir and dissolve at 85 °C for 6 h, dry after completion, continue to add 2.4 g of methyl methacrylate isothiocyanate, introduce nitrogen for protection, add 0.01 g of triethylamine, and oil bath at 50 °C for 8 h. After the reaction, wash with acetonitrile and dry to obtain olefinic polyurethane.

[0025] (4) Under a nitrogen atmosphere, 1.1 g of olefinated polyurethane, 1 g of olefinated ferrocene, and 1.3 g of methyl acrylate were added into a reactor and stirred evenly. 0.02 g of azobisisobutyronitrile initiator was added thereto and the mixture was reacted at 90 °C for 12 h. After the reaction, the mixture was cooled to room temperature, washed with deionized water, and dried to obtain a ferrocene modifier.

[0026] (5) Add 4 g of polyvinyl alcohol, 1 g of zirconium hydroxide, 2 g of ferrocene modifier, 2 g of nano boron nitride, and 4 g of water into a stirring container and stir at room temperature for 15 min to obtain a heat-resistant and shear-resistant organic boron and zirconium composite cross-linking agent for oil field fracturing.

[0027] Example 2

[0028] (1) Add 2 g of ferrocenylboric acid to 70 mL of toluene solvent, stir and disperse, then add 3.2 g of N-methyl-2-hydroxyethylamine, react at 130 ° C for 14 h. After the reaction is completed, distill under reduced pressure, filter and dry to obtain an intermediate.

[0029] (2) Add 2 g of the intermediate and 4.8 g of 3-chloropropylene to 80 mL of N,N-dimethylformamide solvent, stir and disperse, react at 80 °C for 20 h, then continue to add 3.6 g of sodium 3-chloro-2-hydroxypropanesulfonate, react at 90 °C for 8 h, and then distill under reduced pressure and filter to obtain olefinated ferrocene.

[0030] (3) Add 5.1 g of purified polyurethane particles to 120 mL of dimethylformamide solvent, stir and dissolve at 110 °C for 10 h, dry after completion, add 3.1 g of methyl methacrylate isothiocyanate, introduce nitrogen for protection, add 0.03 g of triethylamine, and place in an oil bath at 70 °C for 10 h. After the reaction, wash with acetonitrile and dry to obtain olefinic polyurethane.

[0031] (4) Under a nitrogen atmosphere, 1.2 g of olefinated polyurethane, 1 g of olefinated ferrocene, and 1.5 g of methyl acrylate were added into a reactor and stirred evenly. 0.03 g of azobisisobutyronitrile initiator was added thereto and the mixture was reacted at 110 °C for 16 h. After the reaction, the mixture was cooled to room temperature, washed with deionized water, and dried to obtain a ferrocene modifier.

[0032] (5) 8 g of polyvinyl alcohol, 2 g of zirconium hydroxide, 5 g of ferrocene modifier, 3 g of nano boron nitride, and 6 g of water were added to a stirring container and stirred at room temperature for 20 min to obtain a heat-resistant and shear-resistant organic boron and zirconium composite cross-linking agent for oil field fracturing.

[0033] Example 3

[0034] (1) Add 1.5 g of ferrocenylboric acid to 60 mL of toluene solvent, stir and disperse, then add 2.25 g of N-methyl-2-hydroxyethylamine, react at 120 °C for 12 h. After the reaction is completed, evaporate under reduced pressure, filter and dry to obtain an intermediate.

[0035] (2) Add 1.6 g of the intermediate and 3.66 g of 3-chloropropylene to 70 mL of N,N-dimethylformamide solvent, stir and disperse, react at 72 °C for 16 h, then continue to add 2.64 g of sodium 3-chloro-2-hydroxypropanesulfonate, react at 80 °C for 7 h, and then distill under reduced pressure and filter to obtain olefinated ferrocene.

[0036] (3) Add 3.35 g of purified polyurethane particles to 100 mL of dimethylformamide solvent, stir and dissolve at 97 °C for 8 h, dry after completion, continue to add 2.75 g of methyl methacrylate isothiocyanate, introduce nitrogen for protection, then add 0.02 g of triethylamine, and oil bath at 60 °C for 9 h. After the reaction, wash with acetonitrile and dry to obtain olefinic polyurethane.

[0037] (4) Under a nitrogen atmosphere, 1.15 g of olefinated polyurethane, 1 g of olefinated ferrocene, and 1.4 g of methyl acrylate were added into a reactor and stirred evenly. 0.025 g of azobisisobutyronitrile initiator was added thereto and the mixture was reacted at 100 °C for 14 h. After the reaction, the mixture was cooled to room temperature, washed with deionized water, and dried to obtain a ferrocene modifier.

[0038] (5) 6 g of polyvinyl alcohol, 1.5 g of zirconium hydroxide, 3.5 g of ferrocene modifier, 2.5 g of nano boron nitride, and 5 g of water were added to a stirring container and stirred at room temperature for 17 min to obtain a heat-resistant and shear-resistant organic boron and zirconium composite cross-linking agent for oil field fracturing.

[0039] Example 4

[0040] (1) Add 1 g of ferrocenylboric acid to 50 mL of toluene solvent, stir and disperse, then add 1.3 g of N-methyl-2-hydroxyethylamine, react at 110°C for 10 h. After the reaction is completed, evaporate under reduced pressure, filter and dry to obtain an intermediate.

[0041] (2) Add 1.2 g of the intermediate and 2.52 g of 3-chloropropylene to 60 mL of N,N-dimethylformamide solvent, stir and disperse, react at 65 °C for 12 h, then continue to add 1.68 g of sodium 3-chloro-2-hydroxypropanesulfonate, react at 70 °C for 6 h, and then distill under reduced pressure and filter to obtain olefinated ferrocene.

[0042] (3) Add 5.1 g of purified polyurethane particles to 120 mL of dimethylformamide solvent, stir and dissolve at 110 °C for 10 h, dry after completion, add 3.1 g of methyl methacrylate isothiocyanate, introduce nitrogen for protection, add 0.03 g of triethylamine, and place in an oil bath at 70 °C for 10 h. After the reaction, wash with acetonitrile and dry to obtain olefinic polyurethane.

[0043] (4) Under a nitrogen atmosphere, 1.2 g of olefinated polyurethane, 1 g of olefinated ferrocene, and 1.5 g of methyl acrylate were added into a reactor and stirred evenly. 0.03 g of azobisisobutyronitrile initiator was added thereto and the mixture was reacted at 110 °C for 16 h. After the reaction, the mixture was cooled to room temperature, washed with deionized water, and dried to obtain a ferrocene modifier.

[0044] (5) 6 g of polyvinyl alcohol, 1.5 g of zirconium hydroxide, 3.5 g of ferrocene modifier, 2.5 g of nano boron nitride, and 5 g of water were added to a stirring container and stirred at room temperature for 17 min to obtain a heat-resistant and shear-resistant organic boron and zirconium composite cross-linking agent for oil field fracturing.

[0045] Example 5

[0046] (1) Add 2 g of ferrocenylboric acid to 70 mL of toluene solvent, stir and disperse, then add 3.2 g of N-methyl-2-hydroxyethylamine, react at 130 ° C for 14 h. After the reaction is completed, distill under reduced pressure, filter and dry to obtain an intermediate.

[0047] (2) Add 2 g of the intermediate and 4.8 g of 3-chloropropylene to 80 mL of N,N-dimethylformamide solvent, stir and disperse, react at 80 °C for 20 h, then continue to add 3.6 g of sodium 3-chloro-2-hydroxypropanesulfonate, react at 90 °C for 8 h, and then distill under reduced pressure and filter to obtain olefinated ferrocene.

[0048] (3) Add 3.35 g of purified polyurethane particles to 100 mL of dimethylformamide solvent, stir and dissolve at 97 °C for 8 h, dry after completion, continue to add 2.75 g of methyl methacrylate isothiocyanate, introduce nitrogen for protection, then add 0.02 g of triethylamine, and oil bath at 60 °C for 9 h. After the reaction, wash with acetonitrile and dry to obtain olefinic polyurethane.

[0049] (4) Under a nitrogen atmosphere, 1.15 g of olefinated polyurethane, 1 g of olefinated ferrocene, and 1.4 g of methyl acrylate were added into a reactor and stirred evenly. 0.025 g of azobisisobutyronitrile initiator was added thereto and the mixture was reacted at 100 °C for 14 h. After the reaction, the mixture was cooled to room temperature, washed with deionized water, and dried to obtain a ferrocene modifier.

[0050] (5) Add 4 g of polyvinyl alcohol, 1 g of zirconium hydroxide, 2 g of ferrocene modifier, 2 g of nano boron nitride, and 4 g of water into a stirring container and stir at room temperature for 15 min to obtain a heat-resistant and shear-resistant organic boron and zirconium composite cross-linking agent for oil field fracturing.

[0051] Comparative Example 1

[0052] (1) Add 4 g of polyvinyl alcohol, 1 g of zirconium hydroxide, 2 g of nano boron nitride, and 4 g of water into a stirring container and stir at room temperature for 15 min to obtain a composite cross-linking agent.

[0053] Comparative Example 2

[0054] (1) The ferrocene modifier was prepared according to the method of Example 1.

[0055] (2) Add 4 g of polyvinyl alcohol, 1 g of zirconium hydroxide, 2 g of ferrocene modifier, and 4 g of water into a stirring container and stir at room temperature for 15 min to obtain a composite cross-linking agent.

[0056] Comparative Example 3

[0057] (1) Add 4 g of polyvinyl alcohol, 1 g of zirconium hydroxide, and 4 g of water into a stirring container and stir at room temperature for 15 min to obtain a composite cross-linking agent.

[0058] Performance Testing

[0059] Preparation method of fracturing fluid base fluid: add 0.50g thickener polyacrylamide, 1g clay stabilizer KCl, and 0.03g pH adjuster NaOH to 100mL water, stir evenly, and obtain fracturing fluid base fluid. Then add 0.3% cross-linking agent by mass fraction to form gel. The gel was measured on a Hake MARSⅢ rotational rheometer at temperatures of 135℃, 160℃, and 200℃, and a shear rate of 170s -1 The temperature and shear resistance of the product under different conditions are shown in Table 1.

[0060] Table 1: Temperature resistance and shear resistance test

[0061]

[0062] As can be seen from Table 1, the heat-resistant and shear-resistant organic boron and zirconium composite cross-linking agents for oilfield fracturing prepared in Examples 1-5 of the present invention have better heat-resistant and shear-resistant properties than those of Comparative Examples 1-3.

[0063] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A heat-resistant and shear-resistant organic boron and zirconium composite crosslinking agent for oilfield fracturing, characterized in that: The invention comprises the following components by weight: 4-8 parts by weight of polyvinyl alcohol, 1-2 parts by weight of zirconium hydroxide, 2-5 parts by weight of ferrocene modifier, 2-3 parts by weight of nano boron nitride, and 4-6 parts by weight of water; The preparation method of the ferrocene modifier is: (1) Add ferrocenylboric acid to toluene solvent, stir and disperse, then add N-methyl-2-hydroxyethylamine, react at 110-130°C for 10-14 hours, and after the reaction is completed, distill under reduced pressure, filter and dry to obtain an intermediate; (2) Add the intermediate and 3-chloropropylene to N,N-dimethylformamide solvent, stir and disperse, react at 65-80°C for 12-20h, then continue to add sodium 3-chloro-2-hydroxypropanesulfonate, react at 70-90°C for 6-8h, and then distill under reduced pressure and filter to obtain olefinated ferrocene; (3) Under a nitrogen atmosphere, add olefinic polyurethane, olefinic ferrocene, and methyl acrylate into a reactor, stir evenly, continue to add azobisisobutyronitrile initiator, react at 90-110°C for 12-16h, cool to room temperature after reaction, wash with deionized water, and dry to obtain ferrocene modifier; The mass ratio of ferrocenylboric acid to N-methyl-2-hydroxyethylamine in (1) is 1:1.3-1.6; The mass ratio of the intermediate, 3-chloropropylene, and sodium 3-chloro-2-hydroxypropanesulfonate in (2) is 1:(2.1-2.4):(1.4-1.8); The mass ratio of olefinic polyurethane, olefinic ferrocene, methyl acrylate and azobisisobutyronitrile initiator in (3) is (1.1-1.2):1:(1.3-1.5):(0.02-0.03); The preparation method of the olefinic polyurethane in (3) is as follows: add polyurethane particles to dimethylformamide solvent, stir and dissolve at 85-110°C for 6-10 hours, dry after completion, continue to add methyl methacrylate isothiocyanate, introduce nitrogen for protection, then add triethylamine, and oil bath at 50-70°C for 8-10 hours. After the reaction, wash with acetonitrile and dry to obtain the olefinic polyurethane.

2. A method for preparing the heat-resistant and shear-resistant organic boron and zirconium composite cross-linking agent for oil field fracturing as claimed in claim 1, characterized in that: The preparation method of the heat-resistant and shear-resistant organic boron and zirconium composite crosslinking agent for oilfield fracturing comprises the following steps: adding polyvinyl alcohol, zirconium hydroxide, ferrocene modifier, nano boron nitride and water into a stirring container, stirring at room temperature for 15-20 minutes, and obtaining the heat-resistant and shear-resistant organic boron and zirconium composite crosslinking agent for oilfield fracturing.