Preparation method of nano silicon-based self-infiltration desorbent and its application in coalbed methane fracturing

Through the preparation of nano-silica-based self-absorption desorbent, the use of multi-branched surfactants and organic silicon surfactants to reduce interfacial tension, combined with modified nano-materials, solves the problem of slow flowback speed and slow flowback in coal bed methane fracturing technology. The problem of large capillary resistance enables more efficient coalbed methane production and higher recovery rate.

CN118620599BActive Publication Date: 2024-10-25SHANDONG KEXING CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411101531.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-10-25
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

Existing coalbed methane fracturing technology causes huge damage to coal seams, resulting in slow flowback speed, low flowback rate, large capillary resistance, and slow coalbed methane analysis speed, which limits the high production and high recovery rate of coalbed methane.

Method used

The preparation method of nano-silica-based self-absorption desorbent is adopted, and the interfacial tension is reduced, the permeability of the coal seam and the methane desorption rate are increased by compounding multi-branched surfactants, organosilicon surfactants and sucrose fatty acid esters. Modified nanomaterials improve storage stability.

Benefits of technology

Significantly improves the desorption rate and recovery rate of methane, reduces the expansion and capillary pressure of the coal seam, increases the permeability of the coal seam, and achieves more efficient coal bed methane production, and the nano-silica-based self-permeation desorbent has good chemical properties stability and storage stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention provides a preparation method of a nano silicon-based self-infiltration desorbent and its application in coalbed methane fracturing, belonging to the technical field of coal seam mining, and the preparation method comprises the following steps: step 1: preparing an organosilicon surfactant; step 2: preparing a multi-branched surfactant; step 3: by mass, 10-15 parts of a multi-branched surfactant, 20-25 parts of an organosilicon surfactant, 4-9 parts of a sucrose fatty acid ester, 6-12 parts of a modified nano material, and 13-17 parts of hexanediol are mixed, heated to 72-77°C, 32-37 parts of water are added, and reacted for 3-4 hours to obtain a nano silicon-based self-infiltration desorbent. The nano silicon-based self-infiltration desorbent of the present invention can replace the KCl auxiliary agent system currently used in coalbed methane fracturing, has good interfacial activity, changes or reverses the wettability of rocks, and makes methane molecules easy to resolve from the surface of coal particles, thereby improving the methane resolution speed and permeability speed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coal seam mining, and in particular relates to a preparation method of a nano silicon-based self-imbibing desorbent and an application thereof in coal seam gas fracturing. Background Art

[0002] my country has abundant reserves of coalbed methane. Since coal seams are three-low reservoirs (low porosity, low permeability, and low formation pressure), with the increase in the scale of fracturing fluid, the damage to coal seams caused by the fracturing currently used in construction is gradually apparent. At the macro level, it is manifested in the slow return rate and low return rate of the fracturing fluid. At the micro level, it is manifested in the large capillary resistance, slow coalbed methane analysis speed, and slow expansion of the coal seam pressure drop funnel. These phenomena restrict the coalbed methane from obtaining higher gas production and higher recovery rates.

[0003] With the advancement of coalbed methane fracturing technology, the scale of single-stage fracturing fluid for coalbed volume fracturing has reached 2500-3000 cubic meters, and the scale of single-stage (single-layer) fracturing fluid for medium-deep coalbed methane fracturing has reached 3000-5000 cubic meters. The room for increasing coalbed methane production from the perspective of fracturing scale alone is very limited. The negative effect of injecting such a huge volume of fracturing fluid into the coal seam is also huge.

[0004] The coalbed methane development industry urgently needs to develop an efficient and economical coalbed methane fracturing aid that can not only protect the coal reservoir, prevent clay expansion, increase the return speed and return rate of the fracturing fluid, and reduce the pollution of the fracturing fluid to the coal seam, but also promote the rapid desorption and rapid seepage of methane from the surface of coal particles, thereby increasing the coalbed methane production and recovery rate. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a nano silicon-based self-imbibing desorbent and its application in coal-bed methane fracturing.

[0006] In order to achieve the above object, the present invention provides the following technical solution: a method for preparing a nano-silicon-based self-infiltration desorbent, the preparation method comprising the following steps:

[0007] Step 1: Prepare the silicone surfactant as follows:

[0008] (1) Propynol, ethylene oxide and potassium hydroxide in a molar ratio of 1: (5-8): (0.03-0.06) are mixed, heated to 80-85°C at a pressure of 0.1-0.2 MPa, and reacted for 6-8 hours to obtain product A;

[0009] (2) Mix product A and sodium hydroxide in a molar ratio of 1:(2-3), heat to 40-50°C and react for 2-3 hours, continue to add chlorobutane as a capping agent, heat to 50-60°C and react for 6-8 hours to obtain product B;

[0010] (3) Mixing the product B and hydrogenated silicone oil in a molar ratio of 1:(2.3-2.8) as reactants, under chloroplatinic acid catalysis, the reaction temperature is 100-110°C, the reaction time is 2-4 minutes, and an organosilicon surfactant is obtained;

[0011] Step 2: Prepare a multi-branched surfactant as follows:

[0012] (1) Mix palmitic acid and N,N-dimethylaminopropylamine in a mass ratio of 100:(37-45), add alkali, and heat to 140°C-145°C under alkaline conditions, react for 7-9 hours to obtain product C;

[0013] (2) Mix product C and dichloroisopropyl ether in a mass ratio of (3-4): 1, heat to 110°C-115°C, and react for 5-6 hours to obtain product D;

[0014] (3) Mixing the product D, solvent, and sodium chloroacetate aqueous solution in a mass ratio of (6.5-7.5):(4-5):1, heating to 73-78°C, and reacting for 7-9 hours to obtain a multi-branched surfactant;

[0015] Step 3: Mix 10-15 parts of multi-branched surfactant, 20-25 parts of silicone surfactant, 4-9 parts of sucrose fatty acid ester, 6-12 parts of modified nanomaterial and 13-17 parts of hexanediol by mass, heat to 72-77° C., add 32-37 parts of water, and react for 3-4 hours to obtain a nano-silicon-based self-infiltration desorption agent.

[0016] The surfactants on the market have a poor desorption effect on methane and other substances in coal seams. It is analyzed that the commercially available surfactants may not be able to sufficiently reduce the interfacial tension between water and methane bubbles in the pores of coal seams, thereby affecting the desorption and flow of methane. The present invention can improve the coalbed methane (methane) resolution rate by compounding a multi-branched surfactant, an organosilicon surfactant, and a sucrose fatty acid ester. It is analyzed that in the preparation of the multi-branched surfactant, palmitic acid and N, N-dimethylaminopropylamine are reacted under base catalysis to generate a tertiary amine; dichloroethyl ether reacts with the tertiary amine to introduce an alkyl chain on the two nitrogen atoms of the tertiary amine, thereby forming a compound containing two long alkyl groups, and finally reacts with isopropanol and sodium chloroacetate to form a multi-branched surfactant. In the preparation of the organosilicon surfactant, propargyl alcohol and ethylene oxide are first subjected to a ring-opening addition reaction to generate a polyether chain. After the end-capping reaction, it continues to react with hydrogen-containing silicone oil, and the Si-H bond in the hydrogen-containing silicone oil reacts with the unsaturated bond in the product B to generate an organosilicon surfactant. After the multi-branched surfactant, the organosilicon surfactant, and the sucrose fatty acid ester are compounded, the three have a synergistic effect, which can significantly reduce the interfacial tension between water and the pore wall of the coal seam, as well as the interfacial tension between water and methane bubbles. This helps methane bubbles to be released more easily from the tiny pores of the coal seam, thereby increasing the desorption rate of methane. At the same time, the three can penetrate into the micropores of the coal seam after compounding, and by changing the microstructure of the coal seam, the permeability of the coal seam is increased, making it easier for methane to be desorbed and extracted from the coal seam. The compounding of these three surfactants can produce a synergistic effect. The organosilicon surfactant has good chemical stability, while the sucrose fatty acid ester can significantly reduce the interfacial tension between water and the pore surface of the coal seam, and the multi-branched surfactant has better wetting properties. The combination of these different properties can optimize the overall performance and improve the methane desorption rate. The inventor found that when the three are added to the system in a specific mass fraction, the anti-swelling rate and shrinkage rate of the desorbent can be improved. Analysis shows that surfactants compounded in specific proportions can work together on the microstructure and fluid dynamics of coal seams, thereby affecting the expansion and contraction behavior of coal seams under moisture changes. They can significantly reduce the capillary pressure of water in the pores of coal seams, thereby reducing the retention of water in the pores of coal seams. Low capillary pressure helps reduce the expansion of coal seams caused by increased moisture.

[0017] Furthermore, the preparation method of the modified nanomaterial is:

[0018] (1) mixing nano silicon dioxide, nano titanium oxide and nano zinc oxide in a mass ratio of (1.4-1.8):1:(0.2-0.6) to obtain a nano material;

[0019] (2) mixing the nanomaterial, γ-aminopropyltriethoxysilane and ethanol aqueous solution in a mass ratio of 10: (0.2-0.4): (60-80), reacting at 55-60° C. for 5-8 hours, filtering, washing, and obtaining a silane-modified nanomaterial;

[0020] (3) Mix silane-modified nanomaterials, N,N-dimethylformamide, N-(4-anilinophenyl)maleimide and triethylamine in a mass ratio of 1: (3-4): (20-25): (0.2-0.3), heat to 55-60° C. and react for 20-25 h, filter, wash and dry to obtain modified nanomaterials.

[0021] Furthermore, the nano-silicon dioxide has an average particle size of 10 nm and an average specific surface area of ​​380 m 2 / g. Purchased from Ningbo Jinlei Nanomaterial Technology Co., Ltd.

[0022] Furthermore, the average particle size of the nano titanium oxide is 15 nm, and the specific surface area is 60-120 m 2 / g. Purchased from Zhejiang Zhiti Nano Micro New Materials Co., Ltd., model ZT-TA15.

[0023] Furthermore, the average particle size of the nano zinc oxide is 20 nm, and the specific surface area is 20-60 m 2 / g. Purchased from Zhejiang Zhiti Nano Micro New Materials Co., Ltd., model ZT-J20.

[0024] Nanomaterials in desorbents can change the properties of fluids in coal seam pores, such as reducing the viscosity of the fluid, improving its permeability and fluidity in narrow pores, thereby promoting the desorption and transportation of gases such as methane. However, the inventors have found that the addition of nanomaterials to the system of the present invention has poor compatibility with other components in the system, which will affect the storage stability of the desorbent, and it is easy to stratify or precipitate during long-term storage, affecting the use effect. The present invention improves the storage stability of the desorbent by modifying the nanomaterials, which is conducive to long-term storage. The analysis is to modify the surface of the nanomaterial by using γ-aminopropyltriethoxysilane, which contains amino groups and silane structures. The silane structure can form a strong chemical bond with the active groups on the surface of the nanomaterial through hydrolysis and condensation reaction, thereby fixing the organic functional groups on the surface of the nanomaterial, and then use N-(4-anilinophenyl)maleimide and N,N-dimethylformamide to perform secondary modification on the silane-modified nanomaterial. The maleimide group in N-(4-anilinophenyl)maleimide can react with the introduced amino group to form a stable amide bond, thereby increasing the compatibility of the nanomaterial with the remaining components in the system of the present invention, and having better stability and temperature resistance. At the same time, adding the modified nanomaterial of the present invention can increase the interfacial tension and surface tension of the desorbent.

[0025] Furthermore, the mass fraction of ethanol in the ethanol aqueous solution is 60-70%.

[0026] Furthermore, the alkali is sodium hydroxide, and the amount of sodium hydroxide used is 0.2-0.3% of the mass of palmitic acid.

[0027] Furthermore, the mass fraction of chloroacetic acid in the sodium chloroacetate aqueous solution is 42-45%.

[0028] Furthermore, the solvent is isopropanol.

[0029] The CAS number of N,N-dimethylaminopropylamine is 109-55-7.

[0030] The CAS number of N-(4-anilinophenyl)maleimide is 32099-65-3.

[0031] Furthermore, the molar ratio of chlorobutane to product A is 2-3:1.

[0032] Furthermore, the amount of chloroplatinic acid added per kilogram of the total amount of reactants is 14-18 mg.

[0033] The present invention also provides application of the nano silicon-based self-infiltration desorbent prepared by the preparation method, which is used for mining methane from coal seams.

[0034] Compared with the prior art, the advantages and beneficial effects of the present invention are:

[0035] 1. The present invention discloses a preparation method of a nano silicon-based self-infiltration desorbent and its application in coalbed methane fracturing. The nano silicon-based self-infiltration desorbent can replace the KCl additive system currently used in coalbed methane fracturing, and can increase the coalbed methane production by more than 50% or even higher. Due to the unique structure of the nano material, the present invention forms a specific "concave and convex" hydrophobic surface on the surface of the reservoir rock, reduces the thickness of the water film layer, and reduces the water flow resistance under high pressure. At the same time, the desorbent has multiple active sites, which can flexibly adjust the interface hydrophilicity / hydrophobicity, and has multiple properties such as interface activity and anti-swelling and shrinking expansion.

[0036] 2. The present invention discloses a nano-silicon-based self-infiltration desorbent that can reduce capillary pressure and minimize capillary end effect, reduce capillary resistance, and has good interfacial activity, so that rock wettability changes or reverses, making methane molecules easy to decompose, copolymerize, and self-drive from the surface of coal particles, thereby increasing the methane decomposition rate and permeability rate, thereby achieving the effect of increasing production and recovery rate.

[0037] 3. The nano silicon-based self-infiltration desorbent of the present invention is assembled from a variety of surfactants and nano-scale materials, has the function of intelligent amphiphilic active agent, automatically analyzes and displaces methane gas, automatically and quickly discharges methane, and automatically discharges it along the seepage channel under the pressure of the coal reservoir. In summary, the nano silicon-based self-infiltration desorbent of the present invention can regulate the wettability of reservoir rocks, surface tension <25mN / m, improve wetting angle >30°C, nano active water resistance reduction rate >50%, anti-swelling rate >85%, shrinkage rate >35% and other multifunctional water seepage characteristics, achieve pressure reduction and injection, and finally achieve the purpose of analyzing and returning coalbed methane horizontal wells to stabilize production, improve the development level of coalbed methane and shale gas, change rock wettability, form a neutral wetting mechanism, thereby improving the flow capacity of injected active water, reducing injection pressure, and inhibiting the formation of secondary precipitation at the same time, and the effective period of injection is long. The product of the present invention has extremely low corrosion to metals such as casing, and is mainly used in coalbed methane and shale gas fracturing, with a recommended concentration of 0.1-0.3%. DETAILED DESCRIPTION

[0038] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] Example 1

[0040] This embodiment provides a method for preparing a nano-silicon-based self-imbibing desorbent, the preparation method comprising the following steps:

[0041] Step 1: Prepare the silicone surfactant as follows:

[0042] (1) Propylene alcohol, ethylene oxide and potassium hydroxide in a molar ratio of 1:6:0.05 were mixed, heated to 82°C at a pressure of 0.15 MPa, and reacted for 7 hours to obtain product A;

[0043] (2) Mix product A and sodium hydroxide in a molar ratio of 1:2.4, heat to 45°C and react for 2.6 hours, continue to add chlorobutane as a capping agent, the molar ratio of chlorobutane to product A is 2.7:1, heat to 55°C and react for 7 hours to obtain product B;

[0044] (3) Product B and hydrogenated silicone oil in a molar ratio of 1:2.5 are mixed as reactants. Under chloroplatinic acid catalysis conditions, the amount of chloroplatinic acid added is 16 mg per kilogram of the total amount of reactants, the reaction temperature is 105°C, and the reaction time is 3 min to obtain an organosilicon surfactant; the hydrogen content of the hydrogenated silicone oil is ≥1.58 (m / m)%, and the viscosity is 20~28 mm 2 / s, 25 °C, purchased from Jiangxi Yadi Chemical Co., Ltd.;

[0045] Step 2: Prepare a multi-branched surfactant as follows:

[0046] (1) Palmitic acid and N,N-dimethylaminopropylamine in a mass ratio of 100:41 were mixed, sodium hydroxide was added, and the amount of sodium hydroxide used was 0.25% of the mass of palmitic acid. Under alkaline conditions, the temperature was raised to 142°C and the reaction was carried out for 8 hours to obtain product C;

[0047] (2) Mix product C and dichloroisopropyl ether in a mass ratio of 3.6:1, heat to 113°C, and react for 5.5 hours to obtain product D;

[0048] (3) Mixing product D, isopropanol, and sodium chloroacetate aqueous solution in a mass ratio of 7:4.5:1, wherein the mass fraction of chloroacetic acid in the sodium chloroacetate aqueous solution is 43%, heating to 75°C, and reacting for 8 hours to obtain a multi-branched surfactant;

[0049] Step 3: Mix 12 parts of multi-branched surfactant, 23 parts of silicone surfactant, 6 parts of sucrose fatty acid ester, 10 parts of modified nanomaterial and 15 parts of hexanediol by mass, heat to 75°C, add 36 parts of water, and react for 3.5 hours to obtain a nano-silicon-based self-infiltration desorption agent.

[0050] The preparation method of the modified nanomaterial is:

[0051] (1) mixing nano silicon dioxide, nano titanium oxide and nano zinc oxide in a mass ratio of 1.6:1:0.4 to obtain a nano material;

[0052] (2) mixing the nanomaterial, γ-aminopropyltriethoxysilane and ethanol aqueous solution in a mass ratio of 10:0.3:70, reacting at 58°C for 6 hours, filtering and washing to obtain a silane-modified nanomaterial; the mass fraction of ethanol in the ethanol aqueous solution is 65%;

[0053] (3) Mix the silane-modified nanomaterial, N,N-dimethylformamide, N-(4-anilinophenyl)maleimide and triethylamine in a mass ratio of 1:3.6:22:0.24, heat to 57°C and react for 23 hours, filter, wash and dry to obtain the modified nanomaterial.

[0054] The nano-silicon dioxide has an average particle size of 10 nm and an average specific surface area of ​​380 m 2 / g. Purchased from Ningbo Jinlei Nanomaterial Technology Co., Ltd.

[0055] The average particle size of the nano titanium oxide is 15nm, and the specific surface area is 60-120m 2 / g. Purchased from Zhejiang Zhiti Nano Micro New Materials Co., Ltd., model ZT-TA15.

[0056] The average particle size of the nano zinc oxide is 20nm, and the specific surface area is 20-60m 2 / g. Purchased from Zhejiang Zhiti Nano Micro New Materials Co., Ltd., model ZT-J20.

[0057] Example 2

[0058] A method for preparing a nano-silicon-based self-imbibing and desorbing agent, the method comprising the following steps:

[0059] Step 1: Prepare the silicone surfactant as follows:

[0060] (1) Propynol, ethylene oxide and potassium hydroxide in a molar ratio of 1:5:0.06 were mixed, heated to 85°C at a pressure of 0.1 MPa, and reacted for 6 hours to obtain product A;

[0061] (2) Mix product A and sodium hydroxide in a molar ratio of 1:2, heat to 50°C and react for 2 hours, continue to add chlorobutane as a capping agent, the molar ratio of chlorobutane to product A is 3:1, heat to 50°C and react for 8 hours to obtain product B;

[0062] (3) Product B and hydrogenated silicone oil in a molar ratio of 1:2.3 are mixed as reactants. Under chloroplatinic acid catalysis conditions, the amount of chloroplatinic acid added is 14 mg per kilogram of the total amount of reactants, the reaction temperature is 110°C, and the reaction time is 2 min to obtain an organosilicon surfactant; the hydrogen content of the hydrogenated silicone oil is ≥1.58 (m / m)%, and the viscosity is 20~28 mm 2 / s, 25 °C, purchased from Jiangxi Yadi Chemical Co., Ltd.;

[0063] Step 2: Prepare a multi-branched surfactant as follows:

[0064] (1) Palmitic acid and N,N-dimethylaminopropylamine in a mass ratio of 100:37 were mixed, sodium hydroxide was added, and the amount of sodium hydroxide used was 0.2% of the mass of palmitic acid. Under alkaline conditions, the temperature was raised to 145°C and the reaction was carried out for 7 hours to obtain product C;

[0065] (2) Mix product C and dichloroisopropyl ether in a mass ratio of 3:1, heat to 110°C, and react for 6 hours to obtain product D;

[0066] (3) Mixing product D, isopropanol, and sodium chloroacetate aqueous solution in a mass ratio of 6.5:4:1, wherein the mass fraction of chloroacetic acid in the sodium chloroacetate aqueous solution is 42%, heating to 78°C, and reacting for 7 hours to obtain a multi-branched surfactant;

[0067] Step 3: Mix 10 parts of multi-branched surfactant, 25 parts of silicone surfactant, 4 parts of sucrose fatty acid ester, 12 parts of modified nanomaterial and 13 parts of hexanediol by mass, heat to 77°C, add 32 parts of water, and react for 4 hours to obtain a nano-silicon-based self-infiltration desorption agent.

[0068] The preparation method of the modified nanomaterial is:

[0069] (1) mixing nano silicon dioxide, nano titanium oxide and nano zinc oxide in a mass ratio of 1.4:1:0.6 to obtain a nano material;

[0070] (2) Mixing the nanomaterial, γ-aminopropyltriethoxysilane and ethanol aqueous solution in a mass ratio of 10:0.2:80, reacting at 55°C for 8 hours, filtering and washing to obtain a silane-modified nanomaterial; the mass fraction of ethanol in the ethanol aqueous solution is 70%;

[0071] (3) Mix the silane-modified nanomaterial, N,N-dimethylformamide, N-(4-anilinophenyl)maleimide and triethylamine in a mass ratio of 1:3:20:0.2, heat to 55°C and react for 25 hours, filter, wash and dry to obtain the modified nanomaterial.

[0072] The nano-silicon dioxide has an average particle size of 10 nm and an average specific surface area of ​​380 m 2 / g. Purchased from Ningbo Jinlei Nanomaterial Technology Co., Ltd.

[0073] The average particle size of the nano titanium oxide is 15nm, and the specific surface area is 60-120m 2 / g. Purchased from Zhejiang Zhiti Nano Micro New Materials Co., Ltd., model ZT-TA15.

[0074] The average particle size of the nano zinc oxide is 20nm, and the specific surface area is 20-60m 2 / g. Purchased from Zhejiang Zhiti Nano Micro New Materials Co., Ltd., model ZT-J20.

[0075] Comparative Example 1

[0076] The difference between this comparative example and Example 1 is that the organosilicon surfactant is replaced by polyalkyl dodecyl methacrylate (CAS: 25719-52-2).

[0077] Comparative Example 2

[0078] The difference between this comparative example and Example 1 is that the multi-branched surfactant is replaced by polyalkyl dodecyl methacrylate (CAS: 25719-52-2).

[0079] Comparative Example 3

[0080] The difference between this comparative example and Example 1 is that 12 parts of multi-branched surfactants, 23 parts of silicone surfactants, and 6 parts of sucrose fatty acid esters are replaced by: 6 parts of multi-branched surfactants, 12 parts of silicone surfactants, and 23 parts of sucrose fatty acid esters.

[0081] Comparative Example 4

[0082] The difference between this comparative example and Example 1 is that the preparation method of the modified nanomaterial is:

[0083] (1) mixing nano silicon dioxide, nano titanium oxide and nano zinc oxide in a mass ratio of 1.6:1:0.4 to obtain a nano material;

[0084] (2) The nanomaterial, silane coupling agent KH550 and ethanol aqueous solution in a mass ratio of 10:0.3:70 are mixed, wherein the mass fraction of ethanol in the ethanol aqueous solution is 65%, and the mixture is reacted at 58° C. for 6 h, filtered, and washed to obtain the silane-modified nanomaterial.

[0085] The nano-silicon dioxide has an average particle size of 10 nm and an average specific surface area of ​​380 m 2 / g. Purchased from Ningbo Jinlei Nanomaterial Technology Co., Ltd.

[0086] The average particle size of the nano titanium oxide is 15nm, and the specific surface area is 60-120m 2 / g. Purchased from Zhejiang Zhiti Nano Micro New Materials Co., Ltd., model ZT-TA15.

[0087] The average particle size of the nano zinc oxide is 20nm, and the specific surface area is 20-60m 2 / g. Purchased from Zhejiang Zhiti Nano Micro New Materials Co., Ltd., model ZT-J20.

[0088] Comparative Example 5

[0089] The difference between this comparative example and Example 1 is:

[0090] The average particle size of the silicon dioxide is 50 nm and the average specific surface area is 210 m 2 / g. Purchased from Ningbo Jinlei Nanomaterial Technology Co., Ltd.

[0091] The nano titanium oxide has an average particle size of 200 nm and an average specific surface area of ​​5-15 m 2 / g. Purchased from Zhejiang Zhiti Nano Micro New Materials Co., Ltd., model ZT-TA200.

[0092] The average particle size of the nano zinc oxide is 200nm, and the specific surface area is 5-15m 2 / g. Purchased from Zhejiang Zhiti Nano Micro New Materials Co., Ltd., model ZT-J300.

[0093] Performance Testing

[0094] 1. The desorbents of Examples 1-2 and Comparative Examples 1-5 were subjected to performance tests. The results are shown in Table 1. The test methods are as follows: Density: measured using a pycnometer method. Interfacial tension: measured using an interfacial tension meter in accordance with GB / T6541-1986. Coalbed methane resolution: measured in accordance with GB / T 28753-2012. Anti-swelling rate, shrinkage rate, drag reduction rate, and drag reduction rate: measured in accordance with the relevant standards of the American Petroleum Institute (API) and the International Organization for Standardization (ISO).

[0095] Table 1 Performance test results

[0096]

[0097] The results show that the desorbents of Examples 1-2 have excellent comprehensive performance. Comparative Examples 1-3 show that by changing the type and content of the surfactant, the desorption rate of methane decreases, and the anti-swelling rate and shrinkage rate decrease significantly. Comparative Examples 4-5 show that different preparation methods of modified nanomaterials have a greater impact on interfacial tension and surface tension.

[0098] 2. The desorbents of Examples 1-2 and Comparative Examples 1-5 were packed in 200 kg plastic barrels and stored indoors (25° C.) in a dark place for 18 months, and then observed for stratification or precipitation. The results are shown in Table 2.

[0099] Table 2 Storage test results

[0100] sample Phenomenon Example 1 No stratification or precipitation Example 2 No stratification or precipitation Comparative Example 1 No stratification or precipitation Comparative Example 2 Layering Comparative Example 3 No stratification or precipitation Comparative Example 4 Layering occurs, with a small amount of precipitation Comparative Example 5 No stratification or precipitation

[0101] The results show that the desorbents of Examples 1-2 of the present invention have good storage stability and can be stored for 18 months. Comparative Example 2 shows that when the multi-branched surfactant is replaced with polyalkyl methacrylate, the stability of the components in the system decreases over a long period of time due to the different hydrophilic-lipophilic balances of different surfactants, resulting in stratification. Comparative Example 4 shows that the interface stability between the modified nanomaterial and the surfactant is insufficient due to different nanomaterial modification methods, resulting in the separation of the filler and the surfactant, and the sedimentation of some nanomaterials.

[0102] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a nano-silicon-based self-infiltration desorbent, characterized in that: The preparation method comprises the following steps: Step 1: Prepare the silicone surfactant as follows: (1) Propynol, ethylene oxide and potassium hydroxide in a molar ratio of 1: (5-8): (0.03-0.06) are mixed, heated to 80-85°C at a pressure of 0.1-0.2 MPa, and reacted for 6-8 hours to obtain product A; (2) Mix product A and sodium hydroxide in a molar ratio of 1:(2-3), heat to 40-50°C and react for 2-3 hours, continue to add chlorobutane as a capping agent, heat to 50-60°C and react for 6-8 hours to obtain product B; (3) Mixing the product B and hydrogenated silicone oil in a molar ratio of 1:(2.3-2.8) as reactants, under chloroplatinic acid catalysis, the reaction temperature is 100-110°C, the reaction time is 2-4 minutes, and an organosilicon surfactant is obtained; Step 2: Prepare a multi-branched surfactant as follows: (1) Mix palmitic acid and N,N-dimethylaminopropylamine in a mass ratio of 100:(37-45), add alkali, and heat to 140°C-145°C under alkaline conditions, react for 7-9 hours to obtain product C; (2) Mix product C and dichloroisopropyl ether in a mass ratio of (3-4): 1, heat to 110°C-115°C, and react for 5-6 hours to obtain product D; (3) Mixing the product D, solvent, and sodium chloroacetate aqueous solution in a mass ratio of (6.5-7.5):(4-5):1, heating to 73-78°C, and reacting for 7-9 hours to obtain a multi-branched surfactant; Step 3: Mix 10-15 parts of multi-branched surfactant, 20-25 parts of silicone surfactant, 4-9 parts of sucrose fatty acid ester, 6-12 parts of modified nanomaterial, and 13-17 parts of hexanediol by mass, heat to 72-77° C., add 32-37 parts of water, and react for 3-4 hours to obtain a nano-silicon-based self-infiltration desorption agent; The preparation method of the modified nanomaterial is: (1) mixing nano silicon dioxide, nano titanium oxide and nano zinc oxide in a mass ratio of (1.4-1.8):1:(0.2-0.6) to obtain a nano material; (2) mixing the nanomaterial, γ-aminopropyltriethoxysilane and ethanol aqueous solution in a mass ratio of 10: (0.2-0.4): (60-80), reacting at 55-60° C. for 5-8 hours, filtering, washing, and obtaining a silane-modified nanomaterial; (3) mixing silane-modified nanomaterial, N,N-dimethylformamide, N-(4-anilinophenyl)maleimide and triethylamine in a mass ratio of 1:(3-4):(20-25):(0.2-0.3), heating to 55-60° C. for reaction for 20-25 h, filtering, washing and drying to obtain a modified nanomaterial; The nano-silicon dioxide has an average particle size of 10 nm and an average specific surface area of ​​380 m 2 / g; The average particle size of the nano titanium oxide is 15nm, and the specific surface area is 60-120m 2 / g; The average particle size of the nano zinc oxide is 20nm, and the specific surface area is 20-60m 2 / g.

2. The method for preparing the nano silicon-based self-infiltration desorbent according to claim 1, characterized in that: The mass fraction of ethanol in the ethanol aqueous solution is 60-70%.

3. The method for preparing the nano silicon-based self-infiltration desorbent according to claim 1, characterized in that: The alkali is sodium hydroxide, and the amount of sodium hydroxide used is 0.2-0.3% of the mass of palmitic acid.

4. The method for preparing the nano silicon-based self-imbibing desorbent according to claim 1, characterized in that: The mass fraction of chloroacetic acid in the sodium chloroacetate aqueous solution is 42-45%.

5. The method for preparing the nano silicon-based self-infiltration desorbent according to claim 1, characterized in that: The molar ratio of the chlorobutane to the product A is 2-3:

1.

6. Application of the nano silicon-based self-imbibing desorbent prepared according to the preparation method according to any one of claims 1 to 5 in coalbed methane fracturing.