A 14.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod and a manufacturing method thereof

By using overeutectoid containing Cr, Mo chemical components and online molten salt secondary isotherm technology in 14.9-level fasteners, the microstructure of cold heading steel strips is regulated, and the high material cost and brittleness in fastener production is solved. Problem, high-efficiency and low-cost high-strength fastener manufacturing is achieved.

CN118621230BActive Publication Date: 2024-11-19JIANGSU YONGGANG GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411112679.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-19
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The production of existing 14.9-level fasteners requires multiple heat treatments, resulting in high material cost, low efficiency, high efficiency, increased brittleness of the strip, and easy to break, limiting the application of high-strength fasteners.

Method used

The microstructure of cold heading steel strips is controlled mainly by tempered cordite, containing a small amount of tempered bead light, and the microstructure of the cold heading steel strip is mainly tempered cordite, containing a small amount of tempered bead light. The body and fuse pearlite are prevented from the production of mesh carbides, and improve the utilization rate of carbon elements and the plasticity of the strips.

Benefits of technology

It significantly improves the tensile strength and plasticity of the strip, reduces material costs, simplifies the production process, reduces the risks of drawing and breaking wires and cold heading cracking, and is suitable for the manufacture of 14.9-level annealing-free fasteners.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118621230B_ABST
    Figure CN118621230B_ABST
Patent Text Reader

Abstract

The invention relates to a 14.9-grade annealing-free hot-rolled high-carbon cold-heading steel wire rod and a manufacturing method thereof. The invention comprises the following steps: based on a hypereutectoid Cr- and Mo-containing chemical composition, controlled rolling and spinning of a wire rod is performed, followed by online molten salt secondary isothermal treatment, wherein the wire rod first passes through a first stage of molten salt, and the wire rod is cooled to a pearlite phase region at a cooling rate of ≥40°C / s for isothermal phase transformation, and the wire rod is controlled to form most of troostite. The wire rod is then heated through a second stage of molten salt to promote isothermal transformation of the wire rod in the pearlite phase region, further tempering and melting of a new phase structure, and finally slowly cooled through a roller to form a cold-heading steel wire rod having a microstructure including most of tempered troostite and the rest of tempered pearlite and melted pearlite. The wire rod can realize organization control and strength-plasticity matching, and the tensile strength can reach 1260-1310MPa, and the cross-sectional shrinkage can reach 47%-52%. The wire rod is used for annealing-free processing of 14.9-grade fasteners, and is beneficial to reducing material costs, improving yield rate and production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hot-rolled cold-heading steel wire rods, and in particular relates to a 14.9-grade annealing-free hot-rolled high-carbon cold-heading steel wire rod and a manufacturing method thereof. Background Art

[0002] With the rapid development of my country's industry, various types of industrial machinery and equipment are gradually moving towards an environment with complex service conditions such as high power, high stress, and high speed. Fasteners, as important connecting components of various types of industrial machinery and equipment, are gradually developing from 8.8-grade fasteners to 12.9-grade fasteners. In recent years, China has carried out research on 13.9-grade fasteners and even 14.9-grade fasteners, but their applications are very limited, and the focus is on research and development based on low and medium carbon steels to reduce the difficulty of improving plasticity. The strengthening effect is achieved by increasing the alloy content, adding microalloy components, and combining the microstructure after controlled rolling and controlled cooling, including most of the bainite or a small amount of martensite. Due to the insufficient plasticity of the raw materials of the hot-rolled wire rods for 14.9-grade high-strength fasteners, production still needs to undergo multiple spheroidizing annealing and softening of the matrix structure to adapt to large deformation cold processing. For example: Patent CN118186298A discloses a high-plasticity delayed fracture resistant ultra-high-strength fastener steel wire rod and its manufacturing method, which adopts a medium C-Si-Mn-Cr-Mo-V-Al-Ni composition design, combined with air cooling + insulation cooling on the Stelmor air cooling line after rolling to obtain bainite. The main metallographic structure is obtained by isothermal heat treatment to obtain the lower bainite structure. However, on the one hand, increasing the alloy content and adding micro-alloy components will lead to higher material costs. Although multiple heat treatments can improve the cold processing performance of wire rods for high-strength fasteners, it also brings the disadvantages of many production processes, low efficiency, high energy consumption and high manufacturing cost. On the other hand, bainite or martensite, as hard and brittle phase structures with high distortion and high dislocation density, improves the strength of the wire rod, but increases the brittleness of the wire rod, which will cause the wire rod to be easily broken during the coiling, transportation and even uncoiling of downstream users in the steel plant, resulting in waste of raw materials and reduced yield, limiting production and application; therefore, it is necessary to develop a 14.9-grade annealing-free hot-rolled cold heading steel wire rod with relatively low cost and high yield and a manufacturing method thereof to meet the development of ultra-high strength annealing-free fastener bolts.

[0003] Carbon is a basic element that provides solid solution strengthening and precipitation strengthening to improve the strength of wire rods. It is cheaper than other alloying elements. Replacing strengthening alloys and micro-alloy components is expected to reduce material costs. However, the existing high-carbon steel wire rods suitable for drawing are mainly used in applications such as bridge cables, cords, and tire bead wires. The sorbite content is generally above 85%. The technical difficulties and causes of its application in 14.9-grade annealing-free fastener bolts are as follows:

[0004] (1) In order to increase the content of troostite in the microstructure, low-speed controlled cooling or delayed cooling is used after hot rolling to extend the time of the wire rod in the troostite phase region. However, during the controlled cooling process of the hypereutectoid steel on the Stelmor cooling line, the wire rod spends a long time in the secondary cementite precipitation zone, and the solubility of carbon in austenite decreases. The supersaturated carbon will precipitate from the austenite in the form of carbides along the austenite grain boundaries in a network, which will increase the inhomogeneity of the chemical composition in the steel, cause greater microstructure stress, and significantly increase the brittleness of the wire rod, leading to The contact fatigue strength is reduced during the drawing and cold heading process, while increasing the cooling rate will increase the temperature difference of the wire rod due to the different stacking thickness of the wire rod on the air cooling line and the increased difference in air volume between the windward side and the leeward side. This is not only not conducive to the troostite phase transformation, but also will cause abnormal bainite or martensite structure, resulting in increased mechanical fluctuations, and a significant decrease in drawing performance and yield rate. At the same time, due to the limited maximum cooling capacity of the Stelmor cooling line, the wire rod still has a high level of network carbide, resulting in uncontrollable deterioration, making it difficult to effectively utilize the carbon element.

[0005] (2) The cooling capacity of the Stelmor air-cooled wire is weak, and the diffusion capacity of carbon is strong, which can easily cause the precipitated phase particles to be coarse, forming a large amount of proeutectoid ferrite and soft pearlite with large interlamellar spacing. In addition, the undercooling is insufficient, which is not conducive to the formation of troostite with finer interlamellar spacing, which in turn leads to insufficient matrix strength. Even if insulation cooling is adopted, the wire rod is already in a low temperature state after the pearlite or troostite is inoculated during the continuous slow cooling process. The large thickness of the pearlite and cementite lamellae also increases the difficulty of softening, making the final structure stress and dislocation density of the wire rod high, resulting in increased drawing hardening and poor cold deformation ability. Therefore, increasing the ferrite content in the structure not only has limited effect on the improvement of the plasticity of the wire rod, but also causes a significant loss of strength of the wire rod. It is necessary to use large drawing to reduce the surface to increase the strength, which has a large loss of plasticity, further exacerbating the risk of wire breakage and cold heading cracking under annealing-free drawing. Summary of the invention

[0006] The present invention aims to solve at least one of the above-mentioned technical problems to a certain extent. The present invention provides a 14.9-grade annealing-free hot-rolled high-carbon cold-heading steel wire rod and a manufacturing method thereof, which can realize the microstructure regulation and strength-plasticity matching of the hot-rolled high-carbon cold-heading steel wire rod, and is used for annealing-free processing of 14.9-grade fasteners, which is beneficial to reducing material costs, improving yield rate and production efficiency.

[0007] The technical solution adopted by the present invention to solve its technical problem is:

[0008] A 14.9 grade annealing-free hot-rolled high-carbon cold-heading steel wire rod, the chemical composition and mass percentage of the cold-heading steel wire rod include: C: 0.78%-0.82%, Si: 0.20%-0.40%, Mn: 0.30%-0.50%, Cr: 0.20%-0.40%, Mo: 0.10%-0.35%, P≤0.015%, S≤0.015%, and the rest is Fe and unavoidable impurities; its microstructure includes tempered troostite accounting for 78%-83% by volume, and the rest is a mixed structure composed of tempered pearlite and fused pearlite.

[0009] The design basis of the chemical composition and mass percentage of the above-mentioned cold heading steel wire rod includes:

[0010] (1) Carbon: As the most economical and effective element for solid solution strengthening and precipitation strengthening, C is the main added element of the present invention, which is used to ensure the matrix strength of steel and to achieve a performance grade of 14.9 after annealing-free tempering. However, it also increases the risk of decarburization and the risk of cementite being distributed in a network along the grain boundaries. In addition, if the C content is too high, the bainite phase transformation temperature range will increase, which is not conducive to microstructure control. Therefore, in order to facilitate microstructure control and take into account the cold deformation performance and strength characteristics of cold heading steel wire rod without adding microalloy components, the mass percentage of C is controlled to be 0.78%~0.82%.

[0011] (2) Silicon: The Si element is often added to steel as a deoxidizer during the smelting process. It can improve the strength of austenite through substitutional solid solution strengthening and inhibit the grain coarsening of the first stage of molten salt treatment. However, excessive silicon will increase the risk of non-metallic inclusions and decarburization and reduce the cold heading forming performance of the material. Therefore, the mass percentage of Si is controlled to be 0.20%~0.40%.

[0012] (3) Manganese: Mn is often added to steel as a deoxidizer during the smelting process. It dissolves in austenite in the steel to form a substitutional solid solution, which can improve the strength of the steel. However, too high a Mn content will aggravate the segregation during the solidification of the steel billet, resulting in poor uniformity of the steel, increase the tendency of grain coarsening during the heating process of the material, increase the hardenability of the wire rod, and easily form a quenched structure. Too high a Mn content will also increase the material cost. Therefore, the mass percentage of Mn is controlled to be 0.30%~0.50%.

[0013] (4) Chromium: As a ferrite-forming element, Cr can greatly improve the hardenability of the material, shifting the transformation curve of the steel to the right. After secondary isothermal precipitation of the online molten salt, fine dispersed carbide particles are precipitated, which plays a role in dispersion strengthening to improve the strength of the material and is beneficial to the refinement of the pearlite lamellar spacing. However, if the Cr content is too high, quenching structure is likely to appear, which is not conducive to structure control and will increase the temper brittleness tendency of the steel. In addition, the precipitation and coarsening of Cr is not conducive to the strength and plasticity of the wire rod. Therefore, the mass percentage of Cr is controlled to be 0.20%~0.40%.

[0014] (5) Molybdenum: Mo can reduce the activity of C and inhibit the diffusion of carbon, thereby refining the precipitated phase particles and refining the thickness of pearlite and cementite lamellae, which is beneficial to the melting of pearlite and cementite lamellae at high temperatures. However, the cost of Mo is relatively high, which is not conducive to reducing material costs. Therefore, the mass percentage of Mo is controlled to be 0.10%~0.35%.

[0015] (6) Phosphorus and sulfur: P and S are impurity elements. The lower the better. Therefore, P is controlled to be ≤ 0.015% and S is ≤ 0.015%.

[0016] The cold heading steel wire rod is designed with a hypereutectoid chemical composition containing Cr and Mo, with relatively low Mn and Cr contents, and does not contain expensive microalloying components such as V and Nb, so that the material cost can be reduced. At the same time, compared with the high-strength fastener wire rod structure that is mainly bainite or contains a small amount of martensite after controlled rolling and controlled cooling, the structure of the cold heading steel wire rod is mainly tempered troostite, and the tempered troostite retains the characteristics that the troostite structure has finer interlamellar spacing than the pearlite structure, and has better strength and drawing properties. Combined with the solid solution and precipitation strengthening of the hypereutectoid Cr and Mo component system, it makes up for the strength loss caused by not adding high alloy content and microalloying components. At the same time, the troostite structure has smaller distortion and dislocation density than bainite or martensite structure, and better plasticity. After being tempered and softened and transformed into tempered troostite, the dislocation density is further reduced, making the toughness The plasticity and plasticity are further improved, which effectively alleviates the problem of drawing hardening. The organization also contains a small amount of tempered pearlite and fused pearlite. Compared with the existing wire rod organization with high troostite content, the tempered pearlite retains the characteristics of coarser pearlite interlamellar spacing and better matrix plasticity than troostite, and has better soft phase strength than ferrite. After the pearlite is softened by tempering and transformed into tempered pearlite, the organizational stress and dislocation density are further reduced. At the same time, the pearlite cementite lamellae are melted to form fused pearlite. The plasticity of the wire rod is further comprehensively improved through the tempering organizational state. On the basis of avoiding excessive loss of the wire rod, the plasticity and cold deformation properties of the wire rod are significantly improved, achieving strength-plasticity matching, reducing the risk of wire breakage and cold heading cracking under annealing-free treatment, and the strengthened component system is also suitable for the final performance level of fasteners reaching 14.9 after quenching and tempering.

[0017] In a preferred embodiment, the lamellar spacing of the tempered bainite is 60~100nm, the volume percentage of the tempered pearlite is 15%~20%, the lamellar spacing of the tempered pearlite is 160~195nm, and the lamellar spacing of the tempered bainite and tempered pearlite is relatively finer, which is beneficial to improving the matrix strength. The refined pearlite cementite lamellae thickness is also beneficial to the melting of the pearlite cementite lamellae at high temperature, thereby regulating the matrix plasticity.

[0018] In a preferred embodiment, the network carbide level of the cold heading steel wire rod is level 0, which effectively inhibits the generation of network carbides, eliminates uncontrollable deterioration factors caused by network carbides, and enhances the strengthening effect of carbon elements.

[0019] In a preferred embodiment, the diameter of the cold heading steel wire rod is 6.0~15.0mm, the tensile strength is 1260~1310MPa, the cross-sectional shrinkage rate is 47%~52%, and the wire rod diameter is relatively thinner, which is also suitable for simplifying the processing process of small-size fasteners. The wire rod after controlled rolling and controlled cooling has both high tensile strength and significantly improved wire rod plasticity. Its uses include manufacturing fasteners such as 14.9 grade bolts under annealing-free process.

[0020] A method for manufacturing a 14.9-grade annealing-free hot-rolled high-carbon cold-heading steel wire rod, the method comprising: producing a wire rod by controlled rolling according to the chemical composition of the above-mentioned 14.9-grade annealing-free hot-rolled high-carbon cold-heading steel wire rod, after the wire rod is spun into a wire rod at a spinning temperature of ≥915°C, performing online molten salt secondary isothermal treatment, allowing the wire rod to first pass through a first stage of molten salt, cooling the wire rod at a cooling rate of ≥40°C / s to a pearlite phase region for isothermal phase transformation, controlling the wire rod to form most of troostite, and then passing through a second stage of molten salt heating to promote the isothermal transformation of the wire rod in the pearlite phase region, further tempering and melting of the new phase structure, and finally slow cooling through a roller to produce a cold-heading steel wire rod having a microstructure including 78% to 83% by volume of tempered troostite and the rest being a mixed structure composed of tempered pearlite and fused pearlite.

[0021] The manufacturing method adopts a hypereutectoid chemical composition design containing Cr and Mo, combined with online molten salt secondary isothermal and roller slow cooling technology. On the one hand, compared with Stelmor fast cooling, the manufacturing method adopts the high-temperature wire rod after spinning through the first stage of molten salt controlled cooling, and utilizes the high-speed heat exchange capacity of the molten salt to quickly pass through the secondary network carbon precipitation interval into the pearlite phase region for isothermal phase transformation, effectively eliminating the deterioration effect of the network carbide, and at the same time, the wire rod is cooled at a faster cooling rate. As the cooling rate increases, the austenite transformation temperature decreases, and a higher degree of supercooling is conducive to the formation of troostite structure. Compared with the second stage molten salt, the temperature of the first stage molten salt is lower, which is also conducive to the formation of troostite lamella spacing. Finer, which is beneficial to improving the matrix strength and drawing performance, at the same time, when the wire rod passes through the molten salt, the molten salt can be wrapped on the surface of the wire rod, and there is no problem of wind volume difference and temperature difference between the windward side and the leeward side compared to wind cooling, and the wire rod can be controlled to undergo uniform isothermal phase transformation in the pearlite phase region to avoid the local generation of bainite or even martensite abnormal structure.

[0022] On the other hand, compared with the continuous cooling of Stelmor insulation, the online molten salt secondary isotherm adopts a control method of first cooling and then heating. After the austenite structure of the wire rod is transformed into the troostite structure with finer interlamellar spacing after the first stage of molten salt, the wire rod is heated by the second stage of molten salt with a higher temperature to promote the transformation of the residual austenite structure in the wire rod structure into the pearlite structure with coarser interlamellar spacing than the troostite, so as to control the plasticity of the matrix, which is more convenient for the control of the troostite and pearlite phase transformation. At the same time, Mo is used to inhibit the coarsening of the precipitated phase particles to avoid the deterioration of strength and plasticity caused by the coarsening of Cr at high temperature for a long time. The refined pearlite cementite lamellae are isothermally cooled rather than continuously at a higher temperature for a longer time, and are continuously melted to form melted pearlite, which is further tempered and softened, thereby reducing the organizational stress and dislocation density of the troostite structure and the new pearlite structure, and regulating the strength and plasticity of the matrix. In the further roller slow cooling step, the high temperature state of the wire rod after passing through the second stage of molten salt is continued by reducing the cooling rate, and further tempered and softened, and finally the wire rod structure and strength and plasticity are regulated, so that the plasticity of the wire rod after controlled cooling is greatly improved, and brittle fracture in the subsequent coiling process is avoided, so that the yield rate of cold heading steel wire rod is guaranteed.

[0023] In a preferred embodiment, during the controlled rolling, the heating furnace temperature is controlled to be ≤1120°C before rolling, the soaking time is 2-3h, and the time in the furnace is ≤5h. A lower heating furnace temperature and a shorter time in the furnace are selected to prevent the aggravation of high-temperature decarburization, and an appropriate soaking time is used to promote the homogenization of the billet composition and reduce segregation.

[0024] In a preferred embodiment, during the controlled rolling, the initial rolling temperature is controlled to be 1070~1100℃, the initial rolling reduction is 26~36%, and a lower initial rolling temperature and an appropriate initial rolling reduction are selected to control the temperature in the rolling stage in preparation for grain refinement.

[0025] In a preferred embodiment, during the controlled rolling, the final rolling temperature is controlled to be ≤950°C, the final rolling reduction is 35-45%, a lower final rolling temperature and a higher final rolling reduction are selected, the deformation amount is increased, the grain boundary area is increased, deformation bands are generated in the grains, carbides are precipitated and dispersed, and the overall grain refinement effect is improved.

[0026] In a preferred embodiment, the spinning temperature is 915-935°C. Selecting a higher spinning temperature is beneficial to controlling the precipitation of secondary carbon in the wire rod, improving the degree of supercooling and increasing the nucleation of sorbite, and avoiding grain coarsening caused by excessive temperature.

[0027] In a preferred embodiment, the molten salt temperature of the first stage molten salt is 505~555℃, and the processing time is 15~25s. The lower the molten salt temperature of the first stage molten salt and the longer the processing time, the more troostite structures are formed and the finer the spacing between troostite lamellae, which increases the proportion of tempered troostite in the wire rod structure, increases the strength of the wire rod and decreases the plasticity. However, if the molten salt temperature is too low, there is a risk of bainite appearing. Conversely, if the molten salt temperature is higher and the processing time is shorter, the proportion of tempered troostite in the structure decreases, the strength of the wire rod decreases and the plasticity increases. If the molten salt temperature is too high, it is not conducive to the refinement of the troostite lamellae and even affects the cooling rate, which is not conducive to the control of the network carbide and there is a risk of coarsening of the precipitate phase particles.

[0028] In a preferred embodiment, the molten salt circulation rate of the first stage molten salt is 500-700 t / h, and the molten salt temperature rise is ≤10°C. A higher molten salt circulation rate is used to reduce the molten salt temperature rise, control the temperature accuracy of the wire rod passing through the first stage molten salt, and promote uniform tissue transformation.

[0029] In a preferred embodiment, the molten salt temperature of the second-stage molten salt is 580~630℃, and the processing time is 400~600s. The lower the molten salt temperature of the second-stage molten salt, the finer the spacing between the pearlite lamellae formed, and refining the thickness of the pearlite and cementite lamellae is beneficial to melting at high temperature. However, too low a molten salt temperature is not conducive to the formation of a small amount of tempered pearlite. On the contrary, the higher the molten salt temperature, the coarser the spacing between the pearlite lamellae formed. If the molten salt temperature is too high, there is a risk of converting to ferrite to reduce the strength of the matrix. The longer the processing time, the more obvious the tempering and softening effect of troostite and pearlite, the more fused pearlite, the lower the strength of the wire rod and the higher the plasticity. However, if the processing time is too long, there is a risk of Cr precipitation coarsening and deterioration of the strength and plasticity. On the contrary, the shorter the processing time, the troostite and pearlite are not fully tempered, the organizational stress and dislocation density are high, and the matrix plasticity decreases.

[0030] In a preferred embodiment, the molten salt circulation rate of the second-stage molten salt is 300~400t / h, and the molten salt temperature rise is ≤3°C. The molten salt temperature rise is reduced by using an appropriate molten salt circulation rate, and the temperature accuracy of the wire rod passing through the second-stage molten salt is controlled to promote uniform tempering and melting of the tissue, while avoiding unnecessary increase in production energy consumption caused by excessive molten salt circulation rate.

[0031] In a preferred embodiment, the roller slow cooling adopts closing the insulation cover, controlling the wire rod to be cooled at a slow cooling rate of 0.5~0.8℃ / s, and the slow cooling time is ≥300s. A lower slow cooling rate and a longer slow cooling time are used to extend the high temperature state of the wire rod, promote further tempering and softening of the wire rod structure, and regulate the strength and plasticity of the matrix.

[0032] In a preferred embodiment, the roller is slowly cooled and then coiled, and the coiling temperature is below 350°C.

[0033] Compared with the prior art, the beneficial effects of the present invention are at least:

[0034] (1) There is little research and application of 14.9 grade fasteners in China. At the same time, its production undergoes multiple heat treatments, which brings about the disadvantages of low production efficiency, high energy consumption and high manufacturing cost. The 14.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod of the present invention is designed based on the hypereutectoid chemical composition containing Cr and Mo combined with microstructure control to obtain a mixed microstructure composed of tempered troostite as the main component and a small amount of tempered pearlite and fused pearlite, which can significantly improve the strength and plasticity of the wire rod. The tensile strength of the product after controlled rolling and controlled cooling can reach 1260~1310MPa, the cross-sectional shrinkage rate can reach 47%~52%, and the network carbide level is 0, which breaks the application restriction of hypereutectoid steel on high-strength cold heading steel wire rod, is conducive to reducing material cost and improving yield rate, and can be used in the manufacture of 14.9 grade bolts and other application fields to save spheroidizing annealing processing, reduce the risk of wire breakage and cold heading cracking, and is conducive to simplifying the production process, reducing production energy consumption, improving production efficiency, and alleviating cost pressure. It has good market application prospects.

[0035] (2) The manufacturing method of the present invention is based on the design of hypereutectoid chemical composition containing Cr and Mo, combined with online molten salt secondary isothermal and roller slow cooling technology. After spinning, it is directly in an online salt bath. First, the high-speed heat exchange capacity of the first-stage molten salt is used to quickly pass through the secondary network carbon precipitation zone to enter the pearlite phase region for isothermal phase transformation. Through the rapid cooling technology, the uncontrollable deterioration factors caused by the network carbide are eliminated, the strengthening effect of the carbon element is enhanced, and most of the troostite structure is formed with a higher supercooling degree. Then, the second-stage molten salt with a higher temperature than the first-stage molten salt is selected to promote the isothermal transformation of the pearlite phase region of the wire rod structure and the further tempering of the new phase structure. Mo is used to refine the thickness of the pearlite cementite lamellae, which is beneficial to the melting of the pearlite cementite lamellae at high temperature and the strong plasticity of the matrix is ​​regulated. Finally, it is further softened by roller slow cooling, and 14.9 grade annealing-free hot-rolled high-carbon cold heading steel wire rod is successfully manufactured. The obtained wire rod has high plastic toughness and is not easy to be brittle during the steel plant coiling, transportation and downstream user uncoiling, and has good industrial adaptability. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0037] Figure 1 is a metallographic structure diagram of Example 1 of the present invention;

[0038] Figure 2 is the metallographic structure diagram of Example 2 of the present invention;

[0039] Figure 3 It is the metallographic structure diagram of Example 3 of the present invention. DETAILED DESCRIPTION

[0040] The embodiments described below with reference to the accompanying drawings are exemplary and are only for the purpose of illustration and do not limit the description of the features and characteristics of the present invention. They are intended to be used to explain the present invention and are sufficient to enable those skilled in the art to implement the present invention, but should not be construed as limiting the scope of the present invention. Embodiment 1:

[0041] A preferred embodiment of the manufacturing method of the 14.9 grade annealing-free hot-rolled high-carbon cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.8%, Si: 0.28%, Mn: 0.3%, Cr: 0.26%, Mo: 0.27%, P: 0.015%, S: 0.014%, and the rest is Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of controlled rolling → wire laying → online molten salt secondary isothermal → roller slow cooling → coiling, specifically:

[0042] The controlled rolling is used to heat the steel billet with a specification of 180mm×180mm through a heating furnace to achieve a high-temperature steel billet that can be rolled into plastic. A lower heating furnace temperature and a shorter furnace time are selected to prevent the high-temperature decarburization from being aggravated. The steel billet coming out of the heating furnace is rolled into a wire with a diameter of 8mm through a rolling line. Low-temperature controlled rolling is used to prevent the coarsening of recrystallized grains, improve the overall grain refinement effect, and strengthen the wire rod matrix. Specifically, the heating procedure of the heating furnace is a preheating section, a heating section, and a soaking section that are heated up in sequence. The soaking section is controlled. The heating furnace temperature of the hot section is 1105°C, the soaking time is 2.5h, the time in the furnace is 4.5h, the initial rolling temperature is 1080°C, the initial rolling reduction is 32%, the final rolling temperature is 930°C, and the final rolling reduction is 40%; the wire-spinning process is used to make the wire rods coming out of the rolling line into wire rods through a wire-spinning mechanism, and the wire rods are spread on the rollers and transported along the rollers. A higher wire-spinning temperature is selected to control the precipitation of secondary carbon in the wire rods and form a larger degree of supercooling, thereby promoting the nucleation of sorbite. Specifically, the wire-spinning temperature is controlled to be 920°C.

[0043] The online molten salt secondary isothermal method adopts a two-stage salt bath tank with molten salt inside. The wire rod after spinning is first conveyed by a roller to pass through the first stage salt bath tank, and is quickly cooled to the temperature of the first stage molten salt, so that the wire rod is cooled at a cooling rate of 41°C / s, and quickly passes through the secondary carbon precipitation interval to enter the pearlite phase region for isothermal phase transformation. A higher degree of supercooling is used to control the wire rod to form most of the troostite. The wire rod coming out of the first stage molten salt is then conveyed by a roller to pass through the second stage salt bath tank, and is quickly transformed to the second stage molten salt. Temperature, promote isothermal transformation of the wire rod in the pearlite phase region, further tempering and melting of the new phase structure, namely, sorbite and pearlite structure, and avoid the precipitation and coarsening of Cr. Specifically: the molten salt temperature of the first stage molten salt is 520°C, the processing time is 20s, the molten salt circulation volume is 600t / h, and the molten salt temperature rise is ≤10°C; the molten salt temperature of the second stage molten salt is 610°C, the processing time is 555s, the molten salt circulation volume is 400t / h, and the molten salt temperature rise is ≤3°C.

[0044] The roller slow cooling process adopts closing the insulation cover, and conveying the wire rod coming out of the second salt bath tank into the insulation cover by rollers for slow cooling treatment to promote further tempering and softening of the wire rod structure. Specifically: the wire rod is controlled to be cooled at a slow cooling rate of 0.7°C / s, and the slow cooling time is 420s until coiling; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 316°C. After packaging and storage, the cold heading steel wire rod product is obtained, and its metallographic structure diagram is as follows Figure 1 shown.

[0045] Comparative Example 1:

[0046] A method for manufacturing wire rod, which differs from Example 1 in that the method is manufactured according to the process flow of controlled rolling → low-temperature wire drawing → Stelmor insulation and slow cooling → coiling. Specifically: the heating furnace temperature of the equalizing section is controlled to be 1070°C, the equalizing time is 3h, the time in the furnace is 5h, the initial rolling temperature is 1050°C, the final rolling temperature is 900°C, and the wire drawing temperature is 885°C. The Stelmor insulation and slow cooling adopts the method of shutting down all fans and insulation covers, and conveying the wire rod with rollers. The wire rod completes phase change at a cooling rate of 1.5°C / s in the cover, and the finished wire rod is obtained after coiling off the line.

[0047] Comparative Example 2:

[0048] A method for manufacturing wire rod, which differs from Example 1 in that the method is manufactured according to the process flow of controlled rolling → low-temperature wire spinning → Stelmor rapid cooling + insulation slow cooling → coiling, specifically: the temperature of the heating furnace in the soaking section is controlled to be 1075°C, the soaking time is 3h, the time in the furnace is 5h, the initial rolling temperature is 1055°C, the final rolling temperature is 905°C, the wire spinning temperature is 890°C, the Stelmor rapid cooling + insulation slow cooling adopts 1~6# fans to be opened at 60%, so that the wire rod is cooled to 675°C at a cooling rate of 4.1°C / s, then the rear fan and the insulation cover are closed, the wire rod is conveyed by a roller, the wire rod completes phase change in the cover at a cooling rate of 0.5°C / s, and the finished wire rod is obtained after the coil is rolled off the line.

[0049] Comparative Example 3:

[0050] A method for manufacturing wire rod, which differs from Example 1 in that the method is manufactured according to a process flow of controlled rolling → spinning → Stelmor rapid cooling + thermal insulation slow cooling. Specifically: the Stelmor rapid cooling + thermal insulation slow cooling adopts 1~7# fans opened at 95%, so that the wire rod is cooled to 680°C at a cooling rate of 10.2°C / s, and then the rear fan and the thermal insulation cover are turned off, and the wire rod is conveyed by a roller. The wire rod completes a phase change in the cover at a cooling rate of 0.8°C / s, and the finished wire rod is obtained after it comes off the line.

[0051] The wire rods obtained in the above-mentioned Example 1 and Comparative Examples 1 to 3 were subjected to organization and performance testing: the tensile test was conducted using "GB-T228.1-2021 Metal Material Tensile Test Part 1: Room Temperature Test Method" to obtain tensile strength and cross-sectional shrinkage, and the organization was tested according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 1 below:

[0052] Table 1. Comparison of wire rod structure and properties by different manufacturing methods

[0053]

[0054] From the comparison results of Example 1 and Comparative Example 1, it can be seen that the hypereutectoid chemical composition design containing Cr and Mo, compared with the troostite + ferrite microstructure obtained under low-temperature spinning and Stelmor insulation cooling, although the strength is higher, the network carbide level is higher, the dislocation density of the troostite structure is higher, and the plasticity of the obtained wire rod is insufficient. The cold heading steel wire rod of the present invention can quickly pass through the secondary network carbon precipitation zone into the pearlite phase zone for isothermal phase transformation, effectively eliminating the deterioration effect of the network carbide and enhancing the strengthening effect of the carbon element.

[0055] From the comparison results of Example 1 with Comparative Example 2 and Comparative Example 3, it can be seen that compared with increasing the cooling rate of the Stelmor air-cooled line after spinning, the network carbide is improved but the level is still high, and the hard-brittle phase structure of bainite or even martensite is obtained, which increases the brittleness of the wire rod, and causes the wire rod to be easily broken during coiling, transportation and even uncoiling by downstream users, resulting in waste of raw materials and reduced yield rate. The cold heading steel wire rod of the present invention is based on the hypereutectoid chemical composition design containing Cr and Mo combined with tissue regulation to obtain a mixed structure composed of mainly tempered troostite and a small amount of tempered pearlite and fused pearlite, which can significantly improve the strength and plasticity of the wire rod, breaking the application restriction of hypereutectoid steel to high-strength cold heading steel wire rod, which is beneficial to reducing material costs and improving the yield rate. Embodiment 2:

[0056] A preferred embodiment of the manufacturing method of the 14.9 grade annealing-free hot-rolled high-carbon cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.82%, Si: 0.4%, Mn: 0.5%, Cr: 0.4%, Mo: 0.33%, P: 0.013%, S: 0.012%, and the rest is Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of controlled rolling → wire laying → online molten salt secondary isothermal → roller slow cooling → coiling, specifically:

[0057] The controlled rolling is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to achieve a high-temperature steel billet that can be rolled into plastic. A lower heating furnace temperature and a shorter furnace time are selected to prevent the high-temperature decarburization from being aggravated. The steel billet coming out of the heating furnace is then rolled into a wire with a diameter of 15mm through a rolling line. Low-temperature controlled rolling is used to prevent the recrystallization grains from coarsening, improve the overall grain refinement effect, and strengthen the wire rod matrix. Specifically, the heating procedure of the heating furnace is a preheating section, a heating section, and a soaking section that are heated up in sequence. The heating furnace temperature of the soaking section is controlled to be 1120°C, the soaking time is 3h, the time in the furnace is 5h, the initial rolling temperature is 1000°C, the initial rolling reduction is 26%, the final rolling temperature is 950°C, and the final rolling reduction is 35%; the wire-spinning process is used to make the wire rods exiting the rolling line into wire rods through a wire-spinning mechanism, and the wire rods are spread on the rollers and transported along the rollers. A higher wire-spinning temperature is selected to control the precipitation of secondary carbon in the wire rods and form a larger degree of supercooling, thereby promoting the nucleation of sorbite. Specifically, the wire-spinning temperature is controlled to be 935°C.

[0058] The online molten salt secondary isothermal method adopts a two-stage salt bath tank with molten salt inside. The wire rod after spinning is first conveyed by a roller to pass through the first stage salt bath tank, and is quickly cooled to the temperature of the first stage molten salt, so that the wire rod is cooled at a cooling rate of 41°C / s, and quickly passes through the secondary carbon precipitation interval to enter the pearlite phase region for isothermal phase transformation. A higher degree of supercooling is used to control the wire rod to form most of the troostite. The wire rod coming out of the first stage molten salt is then conveyed by a roller to pass through the second stage salt bath tank, and is quickly transformed to the second stage molten salt. Temperature, promote isothermal transformation of the wire rod in the pearlite phase region, further tempering and melting of the new phase structure, namely, sorbite and pearlite structure, and avoid precipitation and coarsening of Cr. Specifically: the molten salt temperature of the first stage molten salt is 530°C, the processing time is 18s, the molten salt circulation volume is 620t / h, and the molten salt temperature rise is ≤10°C; the molten salt temperature of the second stage molten salt is 595°C, the processing time is 600s, the molten salt circulation volume is 300t / h, and the molten salt temperature rise is ≤3°C.

[0059] The roller slow cooling process adopts closing the insulation cover, and conveying the wire rod coming out of the second salt bath tank into the insulation cover by rollers for slow cooling treatment to promote further tempering and softening of the wire rod structure. Specifically: the wire rod is controlled to be cooled at a slow cooling rate of 0.6°C / s, and the slow cooling time is 440s until coiling; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 331°C. After packaging and storage, the cold heading steel wire rod product is obtained, and its metallographic structure diagram is as follows Figure 2 shown.

[0060] Comparative Example 4:

[0061] A method for manufacturing a wire rod, which differs from that of Example 2 in that the temperature of the heating furnace in the soaking section is controlled to be 1075°C, the soaking time is 3 hours, the time in the furnace is 5 hours, the initial rolling temperature is 1055°C, the final rolling temperature is 905°C, the spinning temperature is 895°C, the wire rod is cooled at a cooling rate of 38°C / s through the first section of molten salt, and the finished wire rod is obtained after being rolled off the line.

[0062] Comparative Example 5:

[0063] A method for manufacturing wire rod, which differs from that of Example 2 in that the molten salt temperature of the first stage molten salt is 480°C, the processing time is 30s, the wire rod is cooled at a cooling rate of 43°C / s through the first stage molten salt, the molten salt circulation rate is 750t / h, and the finished wire rod is obtained after the coil is rolled off the line.

[0064] Comparative Example 6:

[0065] A method for manufacturing wire rod, which differs from Example 2 in that the molten salt temperature of the first stage molten salt is 560°C, the processing time is 10s, the wire rod is cooled at a cooling rate of 40°C / s after passing through the first stage molten salt, and the finished wire rod is obtained after being rolled off the line. Embodiment 3:

[0066] A preferred embodiment of the manufacturing method of the 14.9 grade annealing-free hot-rolled high-carbon cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.78%, Si: 0.2%, Mn: 0.45%, Cr: 0.2%, Mo: 0.1%, P: 0.012%, S: 0.012%, and the rest is Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of controlled rolling → wire laying → online molten salt secondary isothermal → roller slow cooling → coiling, specifically:

[0067] The controlled rolling is used to heat the steel billet with a specification of 180mm×180mm through a heating furnace to achieve a high-temperature steel billet that can be rolled into plastic. A lower heating furnace temperature and a shorter furnace time are selected to prevent the high-temperature decarburization from being aggravated. The steel billet coming out of the heating furnace is then rolled into a wire with a diameter of 6mm through a rolling line. Low-temperature controlled rolling is used to prevent the recrystallization grains from coarsening, improve the overall grain refinement effect, and strengthen the wire rod matrix. Specifically: the heating procedure of the heating furnace is a preheating section, a heating section, and a soaking section that are heated up in sequence. The controlled rolling is controlled to The heating furnace temperature of the soaking section is 1095°C, the soaking time is 2h, the time in the furnace is 4.5h, the initial rolling temperature is 1070°C, the initial rolling reduction is 36%, the final rolling temperature is 925°C, and the final rolling reduction is 45%; the wire-spinning process is used to make the wire rods coming out of the rolling line into wire rods through a wire-spinning mechanism, and the wire rods are spread on the rollers and transported along the rollers. A higher wire-spinning temperature is selected to control the precipitation of secondary carbon in the wire rods and form a larger degree of supercooling, thereby promoting the nucleation of sorbite. Specifically, the wire-spinning temperature is controlled to be 915°C.

[0068] The online molten salt secondary isothermal method adopts a two-stage salt bath tank with molten salt inside. The wire rod after spinning is first conveyed by a roller to pass through the first salt bath tank, and is quickly cooled to the temperature of the first molten salt. The wire rod is cooled at a cooling rate of 42°C / s, and quickly passes through the secondary carbon precipitation interval to enter the pearlite phase region for isothermal phase transformation. A high degree of supercooling is used to control the wire rod to form most of the troostite. The wire rod coming out of the first molten salt is then conveyed by a roller to pass through the second salt bath tank, and is quickly transformed to the second molten salt. Temperature, promote isothermal transformation of the wire rod in the pearlite phase region, further tempering and melting of the new phase structure, namely, sorbite and pearlite structure, and avoid precipitation and coarsening of Cr. Specifically: the molten salt temperature of the first stage molten salt is 505°C, the processing time is 25s, the molten salt circulation volume is 700t / h, and the molten salt temperature rise is ≤10°C; the molten salt temperature of the second stage molten salt is 580°C, the processing time is 475s, the molten salt circulation volume is 330t / h, and the molten salt temperature rise is ≤3°C.

[0069] The roller slow cooling process adopts closing the insulation cover, and conveying the wire rod coming out of the second salt bath tank into the insulation cover by rollers for slow cooling treatment to promote further tempering and softening of the wire rod structure. Specifically: the wire rod is controlled to be cooled at a slow cooling rate of 0.5°C / s, and the slow cooling time is 480s until coiling; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 340°C. After packaging and storage, the cold heading steel wire rod product is obtained, and its metallographic structure diagram is as follows Figure 3 shown.

[0070] Comparative Example 7:

[0071] A method for manufacturing a wire rod, which differs from that of Example 3 in that the molten salt temperature of the second-stage molten salt is 560° C., the processing time is 350 s, and the finished wire rod is obtained after the coil is rolled off the production line.

[0072] Comparative Example 8:

[0073] A method for manufacturing wire rod, which differs from Example 3 in that the molten salt temperature of the second-stage molten salt is 640°C, the processing time is 630s, the molten salt circulation rate is 500t / h, the wire rod is controlled to be cooled at a slow cooling rate of 0.8°C / s, the slow cooling time is 370s, and the finished wire rod is obtained after coiling off the line.

[0074] Comparative Example 9:

[0075] A method for manufacturing wire rod, which differs from Example 3 in that the molten salt temperature of the second-stage molten salt is 640°C, the processing time is 700s, the molten salt circulation rate is 500t / h, the wire rod is controlled to be cooled at a slow cooling rate of 0.8°C / s, the slow cooling time is 370s, and the finished wire rod is obtained after coiling off the line. Embodiment 4:

[0076] A preferred embodiment of the manufacturing method of the 14.9 grade annealing-free hot-rolled high-carbon cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.81%, Si: 0.36%, Mn: 0.39%, Cr: 0.38%, Mo: 0.35%, P: 0.012%, S: 0.015%, and the rest is Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of controlled rolling → wire laying → online molten salt secondary isothermal → roller slow cooling → coiling, specifically:

[0077] The controlled rolling is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to achieve a high-temperature steel billet that can be rolled into plastic. A lower heating furnace temperature and a shorter furnace time are selected to prevent the high-temperature decarburization from being aggravated. The steel billet coming out of the heating furnace is rolled into a wire with a diameter of 12mm through a rolling line. Low-temperature controlled rolling is used to prevent the coarsening of recrystallized grains, improve the overall grain refinement effect, and strengthen the wire rod matrix. Specifically: the heating procedure of the heating furnace is a preheating section, a heating section and a soaking section that are heated in sequence. The controlled rolling The heating furnace temperature of the soaking section is 1110°C, the soaking time is 2.5h, the time in the furnace is 5h, the initial rolling temperature is 1090°C, the initial rolling reduction is 29%, the final rolling temperature is 940°C, and the final rolling reduction is 37%; the wire-spinning process is used to make the wire rods coming out of the rolling line into wire rods through a wire-spinning mechanism, and the wire rods are spread on the rollers and transported along the rollers. A higher wire-spinning temperature is selected to control the precipitation of secondary carbon in the wire rods and form a larger degree of supercooling, thereby promoting the nucleation of sorbite. Specifically, the wire-spinning temperature is controlled to be 930°C.

[0078] The online molten salt secondary isothermal method adopts a two-stage salt bath tank with molten salt inside. The wire rod after spinning is first conveyed by a roller to pass through the first salt bath tank, and is quickly cooled to the temperature of the first molten salt. The wire rod is cooled at a cooling rate of 40°C / s, and quickly passes through the secondary carbon precipitation interval to enter the pearlite phase region for isothermal phase transformation. A high degree of supercooling is used to control the wire rod to form most of the troostite. The wire rod coming out of the first molten salt is then conveyed by a roller to pass through the second salt bath tank, and is quickly transformed to the second molten salt. Temperature, promote isothermal transformation of the wire rod in the pearlite phase region, further tempering and melting of the new phase structure, namely, sorbite and pearlite structure, and avoid the precipitation and coarsening of Cr. Specifically: the molten salt temperature of the first stage molten salt is 555°C, the processing time is 15s, the molten salt circulation volume is 500t / h, and the molten salt temperature rise is ≤10°C; the molten salt temperature of the second stage molten salt is 630°C, the processing time is 400s, the molten salt circulation volume is 320t / h, and the molten salt temperature rise is ≤3°C.

[0079] The roller slow cooling process adopts closing the insulation cover and conveying the wire rod coming out of the second salt bath tank into the insulation cover by rollers for slow cooling treatment to promote further tempering and softening of the wire rod structure. Specifically: the wire rod is controlled to be cooled at a slow cooling rate of 0.8°C / s, and the slow cooling time is 355s until it is coiled; the coiling process is used to coil the wire rod into a coil by a coiling drum, and the coiling temperature is 346°C. After packaging and warehousing, the finished cold heading steel wire rod is obtained.

[0080] Comparative Example 10:

[0081] A method for manufacturing a wire rod, which differs from Example 4 in that the method is manufactured according to a process flow of controlled rolling → spinning → online molten salt secondary isothermal → air cooling → coiling. Specifically: the air cooling is performed by opening a heat preservation cover, using a roller to transport the wire rod coming out of the second salt bath tank, controlling the wire rod to be cooled to 318°C at 2.6°C / s, and then coiling it off the line to obtain a finished wire rod.

[0082] The wire rods obtained in the above-mentioned Examples 2 to 4 and Comparative Examples 4 to 10 were subjected to organization and performance testing: the tensile test was conducted using "GB-T 228.1-2021 Metallic Material Tensile Test Part 1: Room Temperature Test Method" to obtain tensile strength and cross-sectional shrinkage, and the organization was tested according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 2 below:

[0083] Table 2. Comparison of the microstructure and properties of cold heading steel wire rods with different compositions and manufacturing methods

[0084]

[0085] It can be seen from the results of Examples 1 to 4 that the tensile strength of the product after controlled rolling and controlled cooling of the present invention can reach 1260 to 1310 MPa, the cross-sectional shrinkage rate can reach 47% to 52%, and the network carbide grade is grade 0. It can be used in the manufacture of 14.9 grade bolts and other application fields to save spheroidizing annealing processing, reduce the risk of wire breakage during drawing and cracking during cold heading, which is conducive to simplifying the production process, reducing production energy consumption, improving production efficiency, and alleviating cost pressure, and has good market application prospects.

[0086] From the comparison results of Example 2 and Comparative Example 4, it can be seen that the use of a higher spinning temperature is beneficial to controlling the precipitation of secondary carbon in the wire rod, improving the degree of supercooling and increasing the nucleation of troostite, and avoiding grain coarsening caused by excessive temperature.

[0087] From the comparison results of Example 2 and Comparative Example 5, it can be seen that the lower the molten salt temperature of the first stage molten salt and the longer the treatment time, the more troostite structure is formed and the finer the spacing between the troostite lamellae, which increases the proportion of tempered troostite in the wire rod structure, increases the strength of the wire rod, and decreases the plasticity; from the comparison results of Example 2 and Comparative Example 6, it can be seen that the higher the molten salt temperature and the shorter the treatment time, the smaller the proportion of tempered troostite in the structure, decreases the strength of the wire rod, and increases the plasticity, and the molten salt temperature and treatment time of the first stage molten salt can be further controlled to control the proportion of tempered troostite in the structure.

[0088] From the comparison results of Example 3 and Comparative Example 7, it can be seen that the lower the molten salt temperature of the second-stage molten salt, the finer the spacing between the pearlite lamellae formed, and the shorter the treatment time, the troostite and pearlite are not fully tempered, the microstructure stress and dislocation density are high, and the matrix plasticity decreases; from the comparison results of Example 3 and Comparative Example 8, it can be seen that the longer the treatment time, the more obvious the tempering and softening effect of troostite and pearlite; from the comparison results of Example 3 and Comparative Example 9, it can be seen that if the treatment time is too long, there is a risk of Cr precipitation coarsening and deterioration of strength and plasticity properties, so the molten salt temperature and treatment time of the second-stage molten salt can be further controlled to further regulate the microstructure and strength and plasticity matching.

[0089] From the comparison results of Example 4 and Comparative Example 10, it can be seen that using a lower slow cooling rate and a longer slow cooling time to prolong the high temperature state of the wire rod can promote further tempering and softening of the wire rod structure and regulate the strength and plasticity of the matrix.

[0090] The series of detailed descriptions listed above are only specific descriptions of feasible embodiments of the present invention, and they are not intended to limit the scope of protection of the present invention. For example, steel billets can be obtained by sequentially performing converter smelting, refining, and continuous casting processes on steelmaking raw materials. Any equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.

Claims

1. A 14.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod, characterized in that: The chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.78% to 0.82%, Si: 0.20% to 0.40%, Mn: 0.30% to 0.50%, Cr: 0.20% to 0.40%, Mo: 0.10% to 0.35%, P≤0.015%, S≤0.015%, and the rest are Fe and unavoidable impurities; its microstructure includes tempered troostite accounting for 78% to 83% by volume, and the rest is a mixed structure composed of tempered pearlite and fused pearlite; The method comprises: producing a wire rod by controlled rolling according to the chemical composition of the 14.9 grade annealing-free hot-rolled high-carbon cold heading steel wire rod, after the wire rod is spun into a wire rod at a spinning temperature of ≥915°C, performing online molten salt secondary isothermal treatment, making the wire rod first pass through a first stage of molten salt, cooling the wire rod to a pearlite phase region at a cooling rate of ≥40°C / s for isothermal phase transformation, controlling the wire rod to form most of troostite, and then passing through a second stage of molten salt heating to promote isothermal transformation of the wire rod in the pearlite phase region, further tempering and melting of the new phase structure, and finally passing through a roller for slow cooling to produce a cold heading steel wire rod with a microstructure including a mixed structure composed of tempered troostite, tempered pearlite and fused pearlite, the molten salt temperature of the first stage of molten salt is 505-555°C, and the treatment time is 15-25s; the molten salt temperature of the second stage of molten salt is 580-630°C, and the treatment time is 400-600s.

2. The 14.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod according to claim 1, characterized in that: The interlamellar spacing of the tempered bainite is 60-100 nm, the volume percentage of the tempered pearlite is 15%-20%, the interlamellar spacing of the tempered pearlite is 160-195 nm, and the network carbide level of the cold heading steel wire rod is level 0.

3. The 14.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod according to claim 1 or 2, characterized in that: The cold heading steel wire rod has a diameter of 6.0-15.0 mm, a tensile strength of 1260-1310 MPa, and a cross-sectional shrinkage of 47%-52%.

4. A method for manufacturing 14.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod, characterized in that: The method comprises: producing a wire rod by controlled rolling according to the chemical composition of the 14.9 grade annealing-free hot-rolled high-carbon cold heading steel wire rod as claimed in claim 1, after the wire rod is spun into a wire rod at a spinning temperature of ≥915°C, performing online molten salt secondary isothermal treatment, allowing the wire rod to first pass through a first stage of molten salt, cooling the wire rod at a cooling rate of ≥40°C / s to a pearlite phase region for isothermal phase transformation, controlling the wire rod to form a majority of troostite, and then passing through a second stage of molten salt heating to promote the wire rod to be isothermal in the pearlite phase region. The steel wire rod is transformed, further tempered and melted through the new phase structure, and finally slowly cooled through a roller to obtain a cold heading steel wire rod whose microstructure includes 78% to 83% tempered troostite by volume and the rest is a mixed structure composed of tempered pearlite and melted pearlite. The molten salt temperature of the first stage molten salt is 505 to 555°C and the processing time is 15 to 25s; the molten salt temperature of the second stage molten salt is 580 to 630°C and the processing time is 400 to 600s.

5. The method for manufacturing 14.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod according to claim 4, characterized in that: During the controlled rolling, the temperature of the heating furnace is controlled to be ≤1120°C before rolling, the soaking time is 2-3h, and the time in the furnace is ≤5h.

6. The method for manufacturing 14.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod according to claim 4, characterized in that: During the controlled rolling, the initial rolling temperature is controlled to be 1070-1100° C., the initial rolling reduction is 26-36%, the final rolling temperature is ≤950° C., and the final rolling reduction is 35-45%.

7. The method for manufacturing 14.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod according to claim 4, characterized in that: The molten salt circulation rate of the first stage molten salt is 500-700 t / h, and the temperature rise of the molten salt is ≤10°C.

8. The method for manufacturing 14.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod according to claim 4, characterized in that: The molten salt circulation rate of the second-stage molten salt is 300-400t / h, and the temperature rise of the molten salt is ≤3°C.

9. The method for manufacturing 14.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod according to claim 4, characterized in that: The roller slow cooling adopts closing the heat preservation cover, controlling the wire rod to be cooled at a slow cooling speed of 0.5-0.8°C / s, and the slow cooling time is ≥300s.