Functional aramid paper and preparation method thereof

By using functional aramid paper in flat wire motors, the problems of copper wire vibration and displacement are solved, the safety and stability of the motor are improved, and energy consumption is reduced through low-temperature calendering process, so as to realize the aramid paper. The effect of heat expansion and smooth surface and not easy to bleach solves the efficiency and energy consumption problems of traditional stator fixing methods.

CN118621625BActive Publication Date: 2024-11-26YANTAI TAYHO ADVANCED MATERIALS RES INST CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411095376.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-26
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

In traditional flat wire motors, the copper wire does not match the size of the silicon steel sheet, which causes the copper wire to vibrate and displace, affecting the safety, stability and service life of the motor. The stator impregnation resin process takes a long time and has high energy consumption, making it difficult to improve production efficiency. .

Method used

Functional aramid paper is used to disperse the chopped aramid fibers and precipitated fibers evenly in water, and add thermally expanded microspheres. After copying, pressing and drying, dimethylsiloxane slurry is coated and carried out. Low temperature calendering, aramid paper with heat expansion function was prepared to fix flat copper wires to reduce defective rate and leakage risk.

Benefits of technology

It has achieved the reduction in defective rate in the flat wire motor of new energy vehicles, improved the safety and stability of the motor, avoided fiber bleed and microspheres, reduced the risk of leakage, and replaced the traditional impregnated resin process and improved production. Efficiency and material fixation effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118621625B_ABST
    Figure CN118621625B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of manufacturing functional composite aramid paper materials, and specifically to a functional aramid paper and a preparation method thereof, wherein the preparation method is as follows: S1, dissociating and evenly dispersing aramid chopped fibers and aramid precipitated fibers in water; then adding heat-expandable microspheres, further evenly dispersing to obtain a mixed slurry; S2, obtaining a heat-expandable aramid base paper by papermaking, pressing, and drying the mixed slurry; S3, uniformly coating the two surfaces of the heat-expandable aramid base paper with a dimethylsiloxane-based slurry, then drying, and calendering to obtain the functional aramid paper. The functional aramid paper has a heat expansion function, effectively reduces the defective rate of flat wire motors for new energy vehicles, and improves the safety and stability of flat wire motors. Moreover, the functional aramid paper has the function of preventing fiber friction and fluffing, and the preparation process is simple and energy consumption is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to functional aramid paper and a preparation method thereof, belonging to the technical field of functional composite aramid paper material manufacturing. Background Art

[0002] As a "superpower" material, aramid paper has excellent performance characteristics such as high strength, high temperature resistance, light weight, and good insulation. It is widely used in military, aviation, and civil fields to help aircraft stealth, light weight, and high-speed flight. In the civil field, it is used for transformer insulation, consumer electronic high-temperature labels, environmentally friendly filter materials, medical devices, etc. With the vigorous development of new energy vehicles, the higher insulation and high-temperature resistance of aramid paper have been further explored and used in the motor insulation of new energy vehicles. For example: Chinese patent application CN116926982A discloses a composite meta-aramid paper and a preparation method thereof. The composite meta-aramid paper is prepared by directly spinning aramid ultrafine (nano to submicron) fibers on the surface of aramid base paper. The composite meta-aramid paper can be used as a high-grade insulating material in generators, motors, and transformers. Chinese patent application CN116497625A discloses a composite aramid paper and a preparation method thereof. The composite aramid paper includes: two aramid paper layers and a heat-conducting layer formed between the two aramid paper layers, and the heat-conducting layer contains resin and heat-conducting filler.

[0003] In traditional round wire motors, since the copper wire is cylindrical, there will be large gaps between the copper wires in the slots, resulting in a low slot fill rate and thus low overall power density of the motor. In order to improve the motor full slot rate and power density, flat wire motors have gradually developed. After the flat wire motor slots, there is still a certain air gap between the silicon steel sheet, which will cause the copper wire to vibrate or even shift when the motor is running, thereby affecting the safety, stability, service life of the motor and the NVH (noise-vibration-harshness) performance of the vehicle. In order to solve the above problems, the motor stator usually uses impregnation resin to fix the internal material. However, the stator impregnation process is time-consuming, will greatly reduce the production cycle, and generate high energy consumption. Therefore, it is of great importance to develop new ways to fix the internal material of the stator. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a functional aramid paper and a preparation method thereof. The functional aramid paper has the function of thermal expansion, which can effectively reduce the defective rate of flat wire motors for new energy vehicles and improve the safety and stability of flat wire motors. Moreover, the functional aramid paper can prevent fiber friction and fuzzing.

[0005] The technical solution of the present invention to solve the above technical problem is as follows: a method for preparing functional aramid paper, the preparation method comprising:

[0006] S1. Dissociate and evenly disperse aramid chopped fibers and aramid fibrils in water; then add heat-expandable microspheres and further evenly disperse them to obtain a mixed slurry;

[0007] S2, obtaining heat-expandable aramid base paper by papermaking, pressing and drying the mixed slurry;

[0008] S3, evenly coating the two surfaces of the heat-expandable aramid base paper with a dimethylsiloxane-based slurry, then drying it, and performing low-temperature calendering to obtain the functional aramid paper.

[0009] Furthermore, the heat-expandable microspheres are hydrophilic heat-expandable microspheres.

[0010] Furthermore, the heat-expandable microspheres account for 0.2% to 2% of the dry weight of the functional aramid paper.

[0011] Furthermore, in step S3, the calendering is low-temperature calendering, and the temperature of the low-temperature calendering is lower than the optimal expansion temperature of the heat-expandable microspheres.

[0012] Furthermore, the temperature of the low-temperature calendering is 90-130°C.

[0013] Furthermore, the pressing pressure of the low-temperature calendering is 4~10MPa.

[0014] Furthermore, the coating thickness of the dimethylsiloxane-based slurry is 2 to 10 microns.

[0015] Furthermore, the dimethylsiloxane-based slurry is a mixture of dimethylsiloxane and an adhesive; in the dimethylsiloxane-based slurry, the mass fraction of dimethylsiloxane is 2-10%.

[0016] Furthermore, the adhesive is at least one of epoxy resin, polyurethane adhesive, acrylate adhesive, and cyanoacrylate adhesive.

[0017] The invention also discloses a functional aramid paper, and the functional aramid paper is prepared according to the preparation method of the invention.

[0018] The beneficial effects of the present invention are:

[0019] The functional aramid paper of the present invention is mainly used in the insulation of the stator slot of the flat wire motor of new energy vehicles. After being inserted into the copper wire slot of the stator of the flat wire motor, the functional aramid paper of the present invention can be heated to expand the aramid paper, which plays a role in further fixing the flat copper wire, solving the problem in the prior art that when the slot of the stator silicon steel sheet does not match the size of the copper wire, the copper wire is prone to displacement and vibration, which affects the performance, safety, stability and life of the entire motor. The functional aramid paper of the present invention can reduce the defective rate of the stator in the flat wire motor of new energy vehicles and improve the overall safety and stability of the motor.

[0020] At the same time, by coating dimethylsiloxane slurry and combining it with the calendering process, a dense coating can be formed on the surface of the aramid paper, which can solve the fiber fuzzing problem caused by inserting the aramid paper into the motor slot and the problem of powder falling due to external force after the microspheres expand, thereby reducing the risk of leakage of the motor.

[0021] The expanded microspheres are uniformly coated inside the aramid paper before being heated and expanded, and are fixed by the coating on the surface of the aramid paper after expansion, and are not easy to fall off. The invention realizes the efficiency characteristics of the aramid paper being able to expand when heated, having a smooth surface and not prone to fuzzing, and having a low energy consumption in the processing technology. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Optical photographs of the cross section of the functional aramid paper prepared in Example 1 before and after expansion;

[0023] Figure 2 This is the DSC curve of aramid fiber precipitation. DETAILED DESCRIPTION

[0024] The specific implementation of the present invention is described in detail below. The present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed.

[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used are only for describing specific embodiments and are not intended to limit the present invention.

[0026] A method for preparing functional aramid paper, the preparation method comprising:

[0027] S1. Dissociate and evenly disperse aramid chopped fibers and aramid fibrils in water; then add heat-expandable microspheres and further evenly disperse them to obtain a mixed slurry;

[0028] S2, obtaining heat-expandable aramid base paper by papermaking, pressing and drying the mixed slurry;

[0029] S3, evenly coating the two surfaces of the heat-expandable aramid base paper with a dimethylsiloxane-based slurry, then drying it, and calendering it to obtain the functional aramid paper.

[0030] Specifically, the heat-expandable microspheres can be uniformly dispersed in water, and the dispersion method includes intrinsic hydrophilicity or dispersion assisted by adding hydrophilic fillers.

[0031] More specifically, the heat-expandable microspheres are hydrophilic heat-expandable microspheres, and the hydrophilic heat-expandable microspheres can be evenly dispersed in water by means of intrinsic hydrophilicity.

[0032] Specifically, the heat-expandable microspheres account for 0.2% to 2% of the dry weight of the functional aramid paper.

[0033] Preferably, the heat-expandable microspheres account for 1% to 1.5% of the dry weight of the functional aramid paper.

[0034] Specifically, in step S3, the calendering is low-temperature calendering, and the temperature of the low-temperature calendering is lower than the optimal expansion temperature of the heat-expandable microspheres.

[0035] Specifically, the temperature of the low-temperature calendering is 90-130°C.

[0036] Preferably, the temperature of the low-temperature calendering is 100-110°C.

[0037] Specifically, the pressing pressure of the low-temperature calendering is 4-10 MPa.

[0038] Preferably, the pressing pressure of the low-temperature calendering is 6~8MPa.

[0039] Specifically, the coating thickness of the dimethylsiloxane-based slurry is 2 to 10 microns.

[0040] Preferably, the coating thickness of the dimethylsiloxane slurry is 2 to 5 microns.

[0041] Specifically, the dimethylsiloxane-based slurry is a mixture of dimethylsiloxane and an adhesive; in the dimethylsiloxane-based slurry, the mass fraction of dimethylsiloxane is 2-10%.

[0042] Specifically, the adhesive is at least one of epoxy resin, polyurethane adhesive, acrylate adhesive, and cyanoacrylate adhesive.

[0043] Preferably, the adhesive is acrylic adhesive.

[0044] Specifically, the dimethylsiloxane slurry is coated by scraping or spraying.

[0045] More specifically, the method adopted in the embodiment of the present invention is scraping.

[0046] Specifically, the drying temperature of step S2 is: 110°C;

[0047] The drying temperature of step S3 is 110° C. and the drying time is 3 min.

[0048] Specifically, when preparing the functional aramid paper, the usage ratio of the aramid chopped fibers to the aramid fibrids can be set according to actual needs. In the embodiment of the present invention, the weight ratio of the aramid chopped fibers to the aramid fibrids is 5:5.

[0049] The raw materials used in the embodiments of the present invention are specifically:

[0050] Aramid chopped fiber: Taimei Da 2D 7mm;

[0051] Aramid fiber: beating degree 60°SR;

[0052] Hydrophilic thermal expansion microspheres: thermal expansion temperature range is 130-160℃;

[0053] Epoxy resin: 3M DP460;

[0054] Polyurethane adhesive: 3M 6316;

[0055] Acrylate glue: Henkel 8097;

[0056] Cyanoacrylate glue: Henkel 8400.

[0057] Example 1

[0058] A preparation method of functional aramid paper comprises the following steps:

[0059] (1) Dissociate and disperse aramid short fibers and aramid fibrils uniformly in water; add hydrophilic heat-expandable microspheres, wherein the hydrophilic heat-expandable microspheres account for 1.2% of the dry weight of the entire heat-expandable aramid base paper, and further disperse uniformly at high speed to obtain a mixed slurry (wherein the high-speed dispersion process is carried out in a high-speed mixer, and the speed of the high-speed mixer is 50,000 revolutions per minute);

[0060] (2) The dispersed mixed slurry is paper-made, pressed and dried to obtain heat-expandable aramid base paper;

[0061] (3) Dimethylsiloxane-based slurry is uniformly coated on both surfaces of the heat-expandable aramid base paper, and the paper is dried in an oven at 110° C. for 3 minutes, and then calendered. The hot pressing temperature of the calendering operation is 110° C. and the pressing pressure is 5 MPa, thereby obtaining the functional aramid paper.

[0062] The thickness of the dimethylsiloxane-based slurry coated on each surface of the thermal expansion aramid base paper is 2 microns, and the adhesive of the dimethylsiloxane-based slurry is acrylate glue; in the dimethylsiloxane-based slurry, the mass fraction of the dimethylsiloxane is 10%.

[0063] Example 2

[0064] A preparation method of functional aramid paper comprises the following steps:

[0065] (1) Dissociating and uniformly dispersing aramid short-cut fibers and aramid fibrils in water; adding hydrophilic heat-expandable microspheres, wherein the hydrophilic heat-expandable microspheres account for 0.2% of the dry weight of the entire heat-expandable aramid base paper, and further uniformly dispersing at a high speed of 50,000 r / min to obtain a mixed slurry;

[0066] (2) The dispersed mixed slurry is paper-made, pressed and dried to obtain heat-expandable aramid base paper;

[0067] (3) Dimethylsiloxane-based slurry is uniformly coated on both surfaces of the heat-expandable aramid base paper, and the paper is dried in an oven at 110° C. for 3 minutes, and then calendered. The hot pressing temperature of the calendering operation is 110° C. and the pressing pressure is 5 MPa, thereby obtaining the functional aramid paper.

[0068] The thickness of the dimethylsiloxane-based slurry coated on each surface of the thermal expansion aramid base paper is 3 microns, and the adhesive of the dimethylsiloxane-based slurry is polyurethane glue; in the dimethylsiloxane-based slurry, the mass fraction of the dimethylsiloxane is 8%.

[0069] Example 3

[0070] A preparation method of functional aramid paper comprises the following steps:

[0071] (1) Dissociating and uniformly dispersing aramid short-cut fibers and aramid fibrils in water; adding hydrophilic heat-expandable microspheres, wherein the hydrophilic heat-expandable microspheres account for 1.2% of the dry weight of the entire heat-expandable aramid base paper, and further uniformly dispersing at high speed to obtain a mixed slurry;

[0072] (2) The dispersed mixed slurry is paper-made, pressed and dried to obtain heat-expandable aramid base paper;

[0073] (3) Dimethylsiloxane-based slurry is uniformly coated on both surfaces of the heat-expandable aramid base paper, and the paper is dried in an oven at 110° C. for 3 minutes, and then calendered. The hot pressing temperature of the calendering operation is 110° C. and the pressing pressure is 8 MPa, thereby obtaining the functional aramid paper.

[0074] The thickness of the dimethylsiloxane-based slurry coated on each surface of the thermal expansion aramid base paper is 5 microns, and the adhesive of the dimethylsiloxane-based slurry is epoxy resin glue; in the dimethylsiloxane-based slurry, the mass fraction of the dimethylsiloxane is 3%.

[0075] Example 4

[0076] A preparation method of functional aramid paper comprises the following steps:

[0077] (1) Dissociating and uniformly dispersing aramid short-cut fibers and aramid fibrils in water; adding hydrophilic heat-expandable microspheres, wherein the hydrophilic heat-expandable microspheres account for 1.5% of the dry weight of the entire heat-expandable aramid base paper, and further uniformly dispersing at high speed to obtain a mixed slurry;

[0078] (2) The dispersed mixed slurry is paper-made, pressed and dried to obtain heat-expandable aramid base paper;

[0079] (3) The two surfaces of the heat-expandable aramid base paper are uniformly coated with a dimethylsiloxane-based slurry, and the paper is dried in an oven at 110° C. for 3 minutes, and then calendered. The hot pressing temperature of the calendering operation is 100° C. and the pressing pressure is 9 MPa, thereby obtaining the functional aramid paper.

[0080] The thickness of the dimethylsiloxane-based slurry coated on each surface of the thermal expansion aramid base paper is 5 microns, and the adhesive of the dimethylsiloxane-based slurry is cyanoacrylate adhesive; in the dimethylsiloxane-based slurry, the mass fraction of the dimethylsiloxane is 4%.

[0081] Example 5

[0082] A preparation method of functional aramid paper comprises the following steps:

[0083] (1) Dissociate and evenly disperse aramid short-cut fibers and aramid fibrils in water; add hydrophilic heat-expandable microspheres, wherein the hydrophilic heat-expandable microspheres account for 1% of the dry weight of the entire heat-expandable aramid base paper, and further disperse evenly at high speed to obtain a mixed slurry;

[0084] (2) The dispersed mixed slurry is paper-made, pressed and dried to obtain heat-expandable aramid base paper;

[0085] (3) Dimethylsiloxane-based slurry is uniformly coated on both surfaces of the heat-expandable aramid base paper, and the paper is dried in an oven at 110° C. for 3 minutes, and then calendered. The hot pressing temperature of the calendering operation is 130° C. and the pressing pressure is 4 MPa, thereby obtaining the functional aramid paper.

[0086] The thickness of the dimethylsiloxane-based slurry coated on each surface of the thermal expansion aramid base paper is 2 microns, and the adhesive of the dimethylsiloxane-based slurry is acrylate glue; in the dimethylsiloxane-based slurry, the mass fraction of the dimethylsiloxane is 10%.

[0087] Example 6

[0088] A preparation method of functional aramid paper comprises the following steps:

[0089] (1) Dissociate and evenly disperse aramid short-cut fibers and aramid fibrils in water; add hydrophilic heat-expandable microspheres, wherein the hydrophilic heat-expandable microspheres account for 2% of the dry weight of the entire heat-expandable aramid base paper, and further disperse evenly at high speed to obtain a mixed slurry;

[0090] (2) The dispersed mixed slurry is paper-made, pressed and dried to obtain heat-expandable aramid base paper;

[0091] (3) Dimethylsiloxane-based slurry is uniformly coated on both surfaces of the heat-expandable aramid base paper, and the paper is dried in an oven at 110° C. for 3 minutes, and then calendered. The hot pressing temperature of the calendering operation is 90° C. and the pressing pressure is 10 MPa, thereby obtaining the functional aramid paper.

[0092] The thickness of the dimethylsiloxane-based slurry coated on each surface of the thermal expansion aramid base paper is 10 microns, and the adhesive of the dimethylsiloxane-based slurry is acrylate glue; in the dimethylsiloxane-based slurry, the mass fraction of the dimethylsiloxane is 2%.

[0093] Comparative Example 1

[0094] The functional aramid paper was prepared by the same method as in Example 1, except that the hot pressing temperature of the heat-expandable aramid base paper was 150° C. (higher than the temperature range specified in the present invention). The specific operation process is as follows:

[0095] (1) Dissociating and uniformly dispersing aramid short-cut fibers and aramid fibrils in water; adding hydrophilic heat-expandable microspheres, wherein the hydrophilic heat-expandable microspheres account for 1.2% of the dry weight of the entire heat-expandable aramid base paper, and further uniformly dispersing at high speed to obtain a mixed slurry;

[0096] (2) The dispersed mixed slurry is paper-made, pressed and dried to obtain heat-expandable aramid base paper;

[0097] (3) The two surfaces of the heat-expandable aramid base paper are uniformly coated with a dimethylsiloxane-based slurry, and the paper is dried in an oven at 110° C. for 3 minutes, and then calendered. The hot pressing temperature of the calendering operation is 150° C. and the pressing pressure is 8 MPa, thereby obtaining the functional aramid paper.

[0098] The thickness of the dimethylsiloxane-based slurry coated on each surface of the thermal expansion aramid base paper is 2 microns, and the adhesive of the dimethylsiloxane-based slurry is acrylate glue; in the dimethylsiloxane-based slurry, the mass fraction of the dimethylsiloxane is 10%.

[0099] Comparative Example 2

[0100] The functional aramid paper was prepared by the same method as in Example 1, except that the pressing pressure of the heat-expanded aramid base paper was 20 MPa (higher than the pressing pressure defined in the present invention). The specific operation process is as follows:

[0101] (1) Dissociating and uniformly dispersing aramid short-cut fibers and aramid fibrils in water; adding hydrophilic heat-expandable microspheres, wherein the hydrophilic heat-expandable microspheres account for 1.2% of the dry weight of the entire heat-expandable aramid base paper, and further uniformly dispersing at high speed to obtain a mixed slurry;

[0102] (2) The dispersed mixed slurry is paper-made, pressed and dried to obtain heat-expandable aramid base paper;

[0103] (3) Dimethylsiloxane-based slurry is uniformly coated on both surfaces of the heat-expandable aramid base paper, and the paper is dried in an oven at 110° C. for 3 minutes, and then calendered. The hot pressing temperature of the calendering operation is 110° C. and the pressing pressure is 20 MPa, thereby obtaining the functional aramid paper.

[0104] The thickness of the dimethylsiloxane-based slurry coated on each surface of the thermal expansion aramid base paper is 2 microns, and the adhesive of the dimethylsiloxane-based slurry is acrylate glue; in the dimethylsiloxane-based slurry, the mass fraction of the dimethylsiloxane is 10%.

[0105] Comparative Example 3

[0106] The functional aramid paper was prepared by the same method as in Example 1, except that the hydrophilic heat-expandable microspheres accounted for 8% of the dry weight of the entire heat-expandable aramid base paper (higher than the percentage of hydrophilic heat-expandable microspheres specified in the present invention). The specific operation process is as follows:

[0107] (1) Dissociate and evenly disperse aramid short fibers and aramid fibrils in water; add hydrophilic heat-expandable microspheres, wherein the hydrophilic heat-expandable microspheres account for 8% of the dry weight of the entire heat-expandable aramid base paper, and further disperse evenly at high speed to obtain a mixed slurry;

[0108] (2) The dispersed mixed slurry is paper-made, pressed and dried to obtain heat-expandable aramid base paper;

[0109] (3) Dimethylsiloxane-based slurry is uniformly coated on both surfaces of the heat-expandable aramid base paper, and the paper is dried in an oven at 110° C. for 3 minutes, and then calendered. The hot pressing temperature of the calendering operation is 110° C. and the pressing pressure is 8 MPa, thereby obtaining the functional aramid paper.

[0110] The thickness of the dimethylsiloxane-based slurry coated on each surface of the thermal expansion aramid base paper is 2 microns, and the adhesive of the dimethylsiloxane-based slurry is acrylate glue; in the dimethylsiloxane-based slurry, the mass fraction of the dimethylsiloxane is 10%.

[0111] Comparative Example 4

[0112] The functional aramid paper was prepared by the same method as in Example 1, except that the dimethylsiloxane-based slurry was not coated in this comparative example 4. The specific operation process is as follows:

[0113] (1) Dissociating and uniformly dispersing aramid short-cut fibers and aramid fibrils in water; adding hydrophilic heat-expandable microspheres, wherein the hydrophilic heat-expandable microspheres account for 1.2% of the dry weight of the entire heat-expandable aramid base paper, and further uniformly dispersing at high speed to obtain a mixed slurry;

[0114] (2) The dispersed mixed slurry is paper-made, pressed and dried to obtain heat-expandable aramid base paper;

[0115] (3) Calendering the heat-expanded aramid base paper, wherein the hot pressing temperature of the calendering operation is 110° C. and the pressing pressure is 8 MPa, to obtain the functional aramid paper.

[0116] Comparative Example 5

[0117] The functional aramid paper was prepared by the same method as in Example 1, except that the coating slurry did not contain dimethylsiloxane. The specific operation process was as follows:

[0118] (1) Dissociating and uniformly dispersing aramid short-cut fibers and aramid fibrils in water; adding hydrophilic heat-expandable microspheres, wherein the hydrophilic heat-expandable microspheres account for 1.2% of the dry weight of the entire heat-expandable aramid base paper, and further uniformly dispersing at high speed to obtain a mixed slurry;

[0119] (2) The dispersed mixed slurry is paper-made, pressed and dried to obtain heat-expandable aramid base paper;

[0120] (3) The slurry is evenly coated on both surfaces of the heat-expandable aramid base paper, and the paper is dried in an oven at 110° C. for 3 minutes, and then calendered. The hot pressing temperature of the calendering operation is 110° C. and the pressing pressure is 8 MPa, thereby obtaining the functional aramid paper.

[0121] The thickness of the slurry coated on each surface of the thermal expansion aramid base paper is 2 microns, and the coating slurry is an adhesive acrylate glue.

[0122] Comparative Example 6

[0123] This comparative example 6 is a preparation process of conventional aramid paper, which specifically includes the following steps:

[0124] (1) dissociating and uniformly dispersing aramid short fibers and aramid fibrids (the mass ratio of aramid short fibers to aramid fibrids is 5:5) in water to obtain a mixed slurry;

[0125] (2) The dispersed mixed slurry is subjected to papermaking, pressing and drying to obtain aramid base paper; the base paper is subjected to high-temperature hot pressing at 290°C (with a counter-pressing pressure of 8 MPa) to obtain calendered aramid paper.

[0126] Comparative Example 7

[0127] Comparative Example 7 is a preparation process of conventional aramid paper according to the low temperature calendering process of this embodiment, which specifically includes the following steps:

[0128] (1) dissociating and uniformly dispersing aramid short fibers and aramid fibrids (the mass ratio of aramid short fibers to aramid fibrids is 5:5) in water to obtain a mixed slurry;

[0129] (2) The dispersed mixed slurry is subjected to papermaking, pressing and drying to obtain aramid base paper; the base paper is subjected to low-temperature hot pressing at 110°C (with a counter-pressing pressure of 8 MPa) to obtain calendered aramid paper.

[0130] The aramid paper samples prepared in the above embodiments and comparative examples were subjected to performance tests. The specific data results are shown in Table 1 below. The measurement methods involved refer to GB / T5591.2-2017. The thickness change rate test method is as follows: the sample is measured at 5 points and the average thickness is recorded as h1. Then, the sample is placed in a 150°C oven for 3 minutes. After being taken out, the average thickness of the sample after heating is measured by the same method as above and recorded as h2. The thickness change rate ( Δ ) is calculated as: Δ =h2 / h1; The method for determining the appearance of the surface after friction is: rub the sample on 1000-mesh gauze paper with the same force (5N) for 3 times, and observe the surface fuzzing phenomenon. The specific measurement results are shown in Table 1.

[0131] Table 1 Aramid paper performance test results

[0132]

[0133] Example 1-Example 6 The functional aramid paper was prepared by the preparation method of the present invention, and the heat-expandable microspheres were successfully introduced into the aramid paper, so that the aramid paper had excellent thermal expansion performance. The thermal expansion multiple can be adjusted according to the mass fraction of the added microspheres in the dry weight of the aramid paper. The expansion effect of the functional aramid paper prepared in Example 1 is as follows: Figure 1 As shown. In addition, the functional aramid paper prepared by the preparation method of the present invention has not only excellent expansion performance, but also good strength performance and insulation performance. Moreover, the introduction of thermal expansion microspheres will not affect the flame retardant properties of the aramid paper. The flame retardant grade of the aramid paper prepared by the preparation method of the present invention is not lower than V-1.

[0134] The invention provides an aramid paper that can expand when heated. After the flat copper wire is inserted into the motor, it can expand at a low temperature of 150°C to achieve the effect of fixing the copper wire. It can replace the traditional method of fixing by impregnating resin, reduce raw material costs, and improve production efficiency.

[0135] From the comparison of the data of Example 1 and Comparative Example 1, it can be seen that if the temperature of hot pressing is too high, the thermal expansion temperature range of the heat-expandable microspheres will be easily reached, and the material will expand prematurely, affecting the subsequent use effect.

[0136] From the data comparison of Example 1 and Comparative Example 2, it can be seen that if the hot pressing pressure is too large, the aramid paper is easily crushed. Therefore, the calendering conditions defined in the present invention are more conducive to obtaining functional aramid paper with excellent performance.

[0137] From the data comparison of Example 1 and Comparative Example 3, it can be seen that if too many heat-expandable microspheres are introduced, the effect of the coating will be weakened, and the heat-expandable microspheres are prone to fall off under external forces such as friction; at the same time, if too many small balls are accumulated, they are prone to uneven expansion at the expansion temperature, which in turn affects the expansion effect.

[0138] From the data comparison of Example 1 and Comparative Example 4, it can be seen that if the dimethylsiloxane-based slurry is not coated during the preparation process, the performance of the aramid paper will also deteriorate. The microspheres in Comparative Example 4 are only modified on the aramid fibers of the aramid paper through van der Waals force, that is, weak intermolecular interaction. The interaction force is weak and it is easy to fall off when subjected to external force, thereby affecting the final use effect. However, the present invention coats the dimethylsiloxane-based slurry on the aramid base paper and introduces an adhesive to allow the microspheres to be tightly bonded to the fibers, thereby preventing the problem of the microspheres falling off due to external force.

[0139] From the data comparison of Example 1 and Comparative Example 5, it can be seen that if the coating slurry is only an adhesive and does not contain dimethylsiloxane, the performance of aramid paper will also deteriorate. Because aramid paper is composed of aramid fibers, there are inevitably small gaps between the fibers. Therefore, when the slurry is coated, the adhesive will penetrate into the aramid paper through the gaps, and the ability to fix the microspheres on the surface of the aramid paper will be weakened. The use of dimethylsiloxane in the preparation method of the present invention to cooperate with oven curing can quickly form a protective film on the paper surface, making the surface bright and dense. At the same time, the introduction of dimethylsiloxane makes the surface of aramid paper smooth, and the slot process in the oil-cooled motor terminal application is smoother, which promotes the improvement of production rhythm.

[0140] From the data comparison of Example 1 and Comparative Example 6, it can be seen that the thermal expansion aramid paper is basically consistent with the conventional aramid paper in terms of mechanical properties; the breakdown voltage that can be sustained is higher than that of the conventional aramid paper, because the addition of slurry such as adhesive fills the gaps between the aramid fibers, and the thickness increases after expansion, so the breakdown voltage that can be sustained is higher; in addition, the embodiments of the present invention also increase the thermal expansion performance that the conventional aramid paper does not have.

[0141] From the data comparison of Example 1 and Comparative Example 7, it can be seen that: under the same low-temperature hot pressing process, due to the presence of adhesive in the coating slurry, the aramid fibers can be pressed very tightly under low temperature conditions, and the performance in all aspects is excellent. However, the initial glass transition temperature of conventional aramid paper is about 273°C (such as Figure 2 As shown in the figure), low-temperature pressing does not reach the softening temperature of the precipitated fibers, so the aramid fibers cannot be pressed densely, the interaction between the fibers is reduced, and various performance indicators deteriorate.

[0142] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are exhaustively listed. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0143] For those skilled in the art, several modifications and improvements may be made without departing from the concept of the present invention, all of which belong to the protection scope of the present invention. The protection scope of the present invention shall be based on the attached claims.

Claims

1. A method for preparing functional aramid paper, characterized in that: The preparation method is: S1. Dissociate and evenly disperse aramid chopped fibers and aramid fibrils in water; then add heat-expandable microspheres and further evenly disperse them to obtain a mixed slurry; S2, obtaining heat-expandable aramid base paper by papermaking, pressing and drying the mixed slurry; S3, uniformly coating the two surfaces of the heat-expandable aramid base paper with a dimethylsiloxane-based slurry, then drying it, and calendering it to obtain the functional aramid paper; The heat-expandable microspheres account for 0.2% to 2% of the dry weight of the functional aramid paper; In step S3, the calendering is low-temperature calendering, the temperature of the low-temperature calendering is lower than the optimal expansion temperature of the heat-expandable microspheres; the pressing pressure of the low-temperature calendering is 4-10 MPa; The dimethylsiloxane-based slurry is a mixture of dimethylsiloxane and an adhesive; in the dimethylsiloxane-based slurry, the mass fraction of the dimethylsiloxane is 2-10%.

2. The method for preparing a functional aramid paper according to claim 1, characterized in that: The heat-expandable microspheres are hydrophilic heat-expandable microspheres.

3. The method for preparing a functional aramid paper according to claim 1, characterized in that: The temperature of the low temperature calendering is 90-130°C.

4. The method for preparing a functional aramid paper according to claim 1, characterized in that: The coating thickness of the dimethylsiloxane-based slurry is 2 to 10 microns.

5. The method for preparing functional aramid paper according to claim 1, characterized in that: The adhesive is at least one of epoxy resin, polyurethane adhesive, acrylate adhesive and cyanoacrylate adhesive.

6. A functional aramid paper, characterized in that: The functional aramid paper is prepared according to any one of the preparation methods of claims 1-5.

Citation Information

Patent Citations

  • Composite aramid paper and preparation method thereof

    CN116497625A

  • Composite meta-aramid paper and preparation method thereof

    CN116926982A

  • Aramid insulation paper-based material for motor slot insulation and preparation method of aramid insulation paper-based material

    CN115506176A

  • Insulation paper and motor stator

    CN116505690A

  • Insulating sheet and preparation method thereof

    CN116581919A