A direct-weldable polyurethane enameled copper rectangular wire and its preparation process

By adding rare earth elements, halloysite nanotubes, silicon carbide and graphene to polyurethane paint, and coating the outer layer with thermosetting polyamide resin paint, the problem of insufficient mechanical strength and heat resistance of polyurethane enameled copper flat wires is solved. Achieving higher mechanical strength and wear resistance, suitable for high-tech equipment.

CN118629703BActive Publication Date: 2024-10-29SHANGHAI SHENMAO MAGNET WIRE CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411110254.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-10-29
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The existing polyurethane enameled copper flat wires have poor mechanical strength, heat resistance and adhesion, and the flexibility and adhesion of large-size wires are poor, making them unable to meet the requirements of high-tech equipment.

Method used

Lanthanide rare earth elements, halloysite nanotubes, silicon carbide and graphene are added to the polyurethane paint to form a modified polyurethane paint, and the outer layer is coated with a thermosetting polyamide resin paint to improve mechanical strength and wear resistance.

Benefits of technology

It significantly improves the mechanical strength and wear resistance of polyurethane paint, enhances its performance stability and adhesion at high temperatures, extends its service life, and is suitable for welding and processing of high-tech equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to a direct-weldable polyurethane enameled copper flat wire and a preparation process thereof, and belongs to the technical field of enameled copper flat wires. The present invention modifies the intermediate layer polyurethane paint by adding rare earth elements, halloysite nanotubes, silicon carbide and graphene, thereby effectively improving the performance of the intermediate layer polyurethane paint. The addition of rare earth elements can refine the grains of the polyurethane paint, so that the polyurethane paint can be better coated on the copper flat wire; the addition of halloysite nanotubes can form a network structure of the polymer, so that the polyurethane paint has better mechanical strength; the addition of silicon carbide and graphene further improves the mechanical strength of the polyurethane paint, and at the same time enhances the barrier performance of the polyurethane paint, reduces the penetration of external substances such as moisture and oxygen into the polyurethane paint, which helps to improve the oxidation resistance of the polyurethane paint.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of enameled copper flat wires and relates to a direct-weldable polyurethane enameled copper flat wire and a preparation process thereof. Background Art

[0002] At present, the polyurethane enameled copper flat wire widely used in household appliances, precision instruments, telecommunications and instruments adopts ordinary polyurethane paint, which has direct solderability, good high-frequency resistance, easy coloring and good moisture resistance, but its mechanical strength and heat resistance are poor, and the flexibility and adhesion of large-size wires are also poor. Therefore, most of the specifications produced by this product are small-size round wires below Ф2.00mm; and the previous painting process of polyurethane enameled copper flat wire adopts felt painting, which has the disadvantage that the paint film thickness between wires is not easy to achieve consistency; high-viscosity insulating paint cannot be used, and more solvents are consumed. The painted felt is baked at high temperature at the lower furnace mouth, which makes the felt age and shortens its service life. High operating skills are required, and the product quality consistency is poor.

[0003] In addition, most of the existing ordinary enameled copper flat wires contain only one insulating layer. When making coils, a skeleton is required to fix and shape them. Moreover, their folding resistance, voltage resistance, wear resistance and heat resistance are poor. The paint film is easy to break and cannot be used directly for welding. The lubricity is also insufficient. Mechanical damage is easy to cause during the processing, which causes changes in the performance of the processed products. They are often used in ordinary motors, electrical appliances, instruments, transformers, etc., but are not suitable for high-tech computer monitors, color TV picture tube deflection coils, high-frequency inductors and high-frequency coils, telecommunication windings, high-speed variable frequency motors, etc., and cannot meet the requirements of the telecommunications and electronics industries.

[0004] Therefore, in order to solve the above problems, the present invention modifies the polyurethane paint to improve its mechanical strength, and adds a layer of thermosetting polyamide resin paint on the outer layer to further improve the mechanical strength of the enameled copper rectangular wire. Summary of the invention

[0005] The invention aims to provide a direct-weldable polyurethane enameled copper rectangular wire and a preparation process thereof, which has the characteristics of high mechanical strength and not prone to aging.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A direct-weldable polyurethane enameled copper rectangular wire, comprising an inner copper round wire, an intermediate layer of modified polyurethane paint and an outer layer of thermosetting polyamide resin paint, wherein the preparation method of the intermediate layer of modified polyurethane paint is as follows:

[0008] S1: by weight percentage, polyester polyol resin 20-30%, blocked polyurethane resin 30-40%, inorganic filler 15-20%, titanium dioxide 1-5%, rare earth element 1-3%, halloysite nanotube 3-5%, silicon carbide 1-3%, graphene 1-2%, dispersant 1-2%, curing agent 1-2%, firstly mix the polyester polyol resin and the blocked polyurethane resin according to proportion, mix well and heat to 160°C to make the mixture molten, stir at a speed of 300 r / min for 2 h to obtain mixture A;

[0009] S2: Inorganic filler, titanium dioxide, rare earth element, halloysite nanotube, silicon carbide and graphene are mixed in proportion, and ground in a ball mill at a speed of 400 r / min under a nitrogen atmosphere for 4 h to obtain a mixture B;

[0010] S3: Add mixture B to mixture A under a nitrogen atmosphere, continue stirring at 160°C, add a dispersant, stir for 2 hours, cool to 100°C, add a curing agent and continue stirring for 2 hours. After stirring, slowly cool to room temperature at 2°C / min, let stand for 24 hours to obtain the modified polyurethane paint.

[0011] Furthermore, the polyester polyol resin in S1 is one of ethylene glycol dicarbonate, propylene glycol dicarbonate, and hexanediol dicarbonate.

[0012] Furthermore, the inorganic filler in S1 is one of bentonite, talcum powder, glass fiber, barium sulfate and calcium carbonate.

[0013] Furthermore, the rare earth element in S1 is one or more of La, Ce, and Pr.

[0014] Furthermore, the dispersant in S1 is one of sodium acrylate, water-based acrylic resin, and polyoxyethylene stearyl alcohol ether.

[0015] Furthermore, the curing agent in S1 is one of diisocyanate and triisocyanate.

[0016] A method for preparing a direct-weldable polyurethane enameled copper flat wire, the process of the method for preparing the direct-weldable polyurethane enameled copper flat wire is as follows:

[0017] S71: putting the round copper wire into a wire drawing machine for wire drawing, and the wire drawing oil temperature in the wire drawing machine is less than 40°C;

[0018] S72: transferring the drawn copper round wire into an annealing furnace, and annealing the wire at a speed of 150 m / min in a nitrogen atmosphere;

[0019] S73: applying the modified polyurethane paint on the surface of the copper round wire treated in S72, drying it by laser irradiation, and leaving it to stand for 12 hours after drying;

[0020] S74: Apply thermosetting polyamide resin paint to the surface of the product obtained in S73, dry at 60° C. for 12 hours, and stand for 24 hours to obtain a product, a direct-weldable polyurethane enameled copper rectangular wire.

[0021] Furthermore, in the S73, the laser power of the laser irradiation is 200 W, the temperature is 70° C., and the irradiation time is 30 min.

[0022] In the present invention, the crystal grains of the polyurethane paint are refined by adding lanthanide rare earth elements to the polyurethane paint, thereby increasing the number of grain boundaries and improving the mechanical strength of the polyurethane paint. This is because the rare earth elements can act as heterogeneous cores during the solidification process, increase the number of crystal cores, and hinder the growth of grains; the lanthanide rare earth elements also increase the bonding strength between the polyurethane paint and the copper round wire, so that the polyurethane paint is more firmly attached to the copper round wire, which effectively improves the mechanical properties and service life of the obtained product; in addition, the lanthanide rare earth elements can increase the hardness and wear resistance of the polyurethane paint, making it more resistant to external mechanical pressure and friction, which helps to improve the durability and use effect of the obtained product. In the present invention, the rare earth elements are added in the form of oxides.

[0023] In the present invention, the performance of polyurethane paint is improved by adding halloysite nanotubes into the polyurethane paint. Halloysite nanotubes have a large specific surface area and can form a network structure in the polymer matrix, thereby enhancing the mechanical properties of the polyurethane paint, such as hardness, wear resistance and tensile strength; the halloysite nanotubes can also reduce the penetration of water and other small molecules in the polyurethane paint, which helps to improve the barrier properties of the polyurethane paint and extend its service life; the addition of halloysite nanotubes can also improve the rheological properties of the polyurethane paint, making it easier to apply and level during the construction process.

[0024] In the present invention, the performance of the polyurethane paint is further improved by adding silicon carbide and graphene. Both silicon carbide and graphene have extremely high hardness and strength. Their addition can significantly improve the hardness and wear resistance of the polyurethane paint. Both silicon carbide and graphene have excellent thermal stability and can maintain structural stability at high temperatures. Their addition can increase the thermal decomposition temperature of the polyurethane paint, so that it can still maintain good performance under high temperature conditions. The addition of silicon carbide and graphene can enhance the barrier performance of the polyurethane paint and reduce the penetration of external substances such as moisture and oxygen into the polyurethane paint, which helps to improve the oxidation resistance of the polyurethane paint and slow down the aging of the obtained enameled copper flat wire.

[0025] Beneficial effects of the present invention:

[0026] The present invention modifies the middle layer polyurethane paint by adding rare earth elements, halloysite nanotubes, silicon carbide and graphene, thereby effectively improving the performance of the middle layer polyurethane paint. The addition of rare earth elements can refine the grains of the polyurethane paint, so that the polyurethane paint can be better coated on the copper flat wire; the addition of halloysite nanotubes can make the polymer form a network structure, so that the polyurethane paint has better mechanical strength; the addition of silicon carbide and graphene further improves the mechanical strength of the polyurethane paint, and at the same time enhances the barrier performance of the polyurethane paint, reduces the penetration of external substances such as moisture and oxygen into the polyurethane paint, which helps to improve the oxidation resistance of the polyurethane paint. DETAILED DESCRIPTION

[0027] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.

[0028] Ratio 1: ethylene glycol dicarbonate 30%, blocked polyurethane resin 30%, bentonite 20%, titanium dioxide 5%, rare earth element Ce 3%, halloysite nanotube 5%, silicon carbide 3%, graphene 2%, water-based acrylic resin 1%, diisocyanate 1%;

[0029] Ratio 2: ethylene glycol dicarbonate 20%, blocked polyurethane resin 40%, bentonite 20%, titanium dioxide 5%, rare earth element Ce 3%, halloysite nanotube 5%, silicon carbide 3%, graphene 2%, water-based acrylic resin 1%, diisocyanate 1%;

[0030] Ratio 3: ethylene glycol dicarbonate 25%, blocked polyurethane resin 40%, bentonite 15%, titanium dioxide 5%, rare earth element Ce 3%, halloysite nanotube 3%, silicon carbide 3%, graphene 2%, water-based acrylic resin 2%, diisocyanate 2%;

[0031] Ratio 4: ethylene glycol dicarbonate 25%, blocked polyurethane resin 40%, bentonite 15%, titanium dioxide 5%, rare earth element Ce 3%, halloysite nanotube 3%, silicon carbide 3%, graphene 2%, water-based acrylic resin 2%, diisocyanate 2%;

[0032] The blocked polyurethane resin of the present invention was purchased from Shanghai Kangming Chemical Co., Ltd., with the product number being NL7130M.

[0033] The thermosetting polyamide resin paint of the present invention is Versamid115.

[0034] The preparation process of the intermediate layer modified polyurethane paint is as follows:

[0035] S1: First, ethylene glycol dicarbonate and blocked polyurethane resin are mixed in proportion, and after being evenly mixed, they are heated to 160° C. to make the mixture molten, and stirred at a speed of 300 r / min for 2 h to obtain a mixture A;

[0036] S2: Mix bentonite, titanium dioxide, rare earth element Ce, halloysite nanotubes, silicon carbide and graphene in proportion, grind them in a ball mill at a speed of 400 r / min under a nitrogen atmosphere for 4 hours to obtain a mixture B;

[0037] S3: Add mixture B to mixture A under a nitrogen atmosphere, continue stirring at 160°C, add water-based acrylic resin, stir for 2 hours, cool to 100°C, add diisocyanate and continue stirring for 2 hours. After stirring, slowly cool to room temperature at 2°C / min, let stand for 24 hours to obtain the modified polyurethane paint.

[0038] Example 1

[0039] S71: putting the round copper wire into a wire drawing machine for wire drawing, and the wire drawing oil temperature in the wire drawing machine is less than 40°C;

[0040] S72: transferring the drawn copper round wire into an annealing furnace, and annealing the wire at a speed of 150 m / min in a nitrogen atmosphere;

[0041] S73: applying the modified polyurethane paint prepared according to the ratio 1 on the surface of the copper round wire treated in S72, drying it by laser irradiation, the laser power is 200W, the temperature is 70°C, the irradiation time is 30min, and it is left to stand for 12h after drying;

[0042] S74: Apply thermosetting polyamide resin paint to the surface of the product obtained in S73, dry at 60° C. for 12 hours, and stand for 24 hours to obtain a product, a direct-weldable polyurethane enameled copper rectangular wire.

[0043] Example 2

[0044] S71: putting the round copper wire into a wire drawing machine for wire drawing, and the wire drawing oil temperature in the wire drawing machine is less than 40°C;

[0045] S72: transferring the drawn copper round wire into an annealing furnace, and annealing the wire at a speed of 150 m / min in a nitrogen atmosphere;

[0046] S73: applying the modified polyurethane paint prepared according to the ratio 2 on the surface of the copper round wire treated in S72, drying it by laser irradiation, the laser power is 200W, the temperature is 70°C, the irradiation time is 30min, and it is left to stand for 12h after drying;

[0047] S74: Apply thermosetting polyamide resin paint to the surface of the product obtained in S73, dry at 60° C. for 12 hours, and stand for 24 hours to obtain a product, a direct-weldable polyurethane enameled copper rectangular wire.

[0048] Example 3

[0049] S71: putting the round copper wire into a wire drawing machine for wire drawing, and the wire drawing oil temperature in the wire drawing machine is less than 40°C;

[0050] S72: transferring the drawn copper round wire into an annealing furnace, and annealing the wire at a speed of 150 m / min in a nitrogen atmosphere;

[0051] S73: applying the modified polyurethane paint prepared according to the ratio 3 on the surface of the copper round wire treated in S72, drying it by laser irradiation, the laser power is 200W, the temperature is 70°C, the irradiation time is 30min, and it is left to stand for 12h after drying;

[0052] S74: Apply thermosetting polyamide resin paint to the surface of the product obtained in S73, dry at 60° C. for 12 hours, and stand for 24 hours to obtain a product, a direct-weldable polyurethane enameled copper rectangular wire.

[0053] Example 4

[0054] S71: putting the round copper wire into a wire drawing machine for wire drawing, and the wire drawing oil temperature in the wire drawing machine is less than 40°C;

[0055] S72: transferring the drawn copper round wire into an annealing furnace, and annealing the wire at a speed of 150 m / min in a nitrogen atmosphere;

[0056] S73: applying the modified polyurethane paint prepared according to the ratio 4 on the surface of the copper round wire treated in S72, drying it by laser irradiation, the laser power is 200W, the temperature is 70°C, the irradiation time is 30min, and it is left to stand for 12h after drying;

[0057] S74: Apply thermosetting polyamide resin paint to the surface of the product obtained in S73, dry at 60° C. for 12 hours, and stand for 24 hours to obtain a product, a direct-weldable polyurethane enameled copper rectangular wire.

[0058] Comparative Example 1

[0059] S71: putting the round copper wire into a wire drawing machine for wire drawing, and the wire drawing oil temperature in the wire drawing machine is less than 40°C;

[0060] S72: transferring the drawn copper round wire into an annealing furnace, and annealing the wire at a speed of 150 m / min in a nitrogen atmosphere;

[0061] S73: applying unmodified polyurethane paint on the surface of the copper round wire treated in S72, drying it by laser irradiation, the laser power is 200W, the temperature is 70℃, the irradiation time is 30min, and it is left to stand for 12h after drying;

[0062] S74: Apply thermosetting polyamide resin paint to the surface of the product obtained in S73, dry at 60° C. for 12 hours, and stand for 24 hours to obtain a product, a direct-weldable polyurethane enameled copper rectangular wire.

[0063] This comparative example uses unmodified polyurethane paint, to which rare earth element Ce, halloysite nanotubes, silicon carbide and graphene are not added, and other proportions are the same as those of proportion 2.

[0064] The mechanical strength test of the prepared direct-weldable polyurethane enameled copper flat wire was carried out according to the ISO 527 tensile test method. The specific test method is as follows:

[0065] Install the test sample on the tensile testing machine, making sure that the installation direction of the sample is consistent with the tensile direction;

[0066] Set the stretching speed to 2 mm / s, the stretching force to 200 N, and the stretching time to 20 s;

[0067] The stretching was recorded and the sample tensile strength was analyzed.

[0068] The experimental results of the embodiments and comparative examples are summarized in the following table:

[0069]

[0070] It can be seen from the experimental results that the modification of the polyurethane paint effectively improves the mechanical strength of the obtained product, the direct-weldable polyurethane enameled copper rectangular wire, among which Example 2 is the best example.

[0071] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A direct-weldable polyurethane enameled copper rectangular wire, It is characterized in that The direct-weldable polyurethane enameled copper rectangular wire comprises an inner copper round wire, an intermediate layer of modified polyurethane paint and an outer layer of thermosetting polyamide resin paint, wherein the preparation method of the intermediate layer of modified polyurethane paint is as follows: S1: by weight percentage, polyester polyol resin 20-30%, blocked polyurethane resin 30-40%, inorganic filler 15-20%, titanium dioxide 1-5%, rare earth element 1-3%, halloysite nanotube 3-5%, silicon carbide 1-3%, graphene 1-2%, dispersant 1-2%, curing agent 1-2%, firstly mix the polyester polyol resin and the blocked polyurethane resin according to proportion, mix well and heat to 160°C to make the mixture molten, stir at a speed of 300 r / min for 2 h to obtain mixture A; S2: Inorganic filler, titanium dioxide, rare earth element, halloysite nanotube, silicon carbide and graphene are mixed in proportion, and ground in a ball mill at a speed of 400 r / min under a nitrogen atmosphere for 4 h to obtain a mixture B; S3: Add mixture B to mixture A under a nitrogen atmosphere, continue stirring at 160°C, add a dispersant, stir for 2 hours, cool to 100°C, add a curing agent and continue stirring for 2 hours. After stirring, slowly cool to room temperature at 2°C / min, let stand for 24 hours to obtain the modified polyurethane paint.

2. A directly weldable polyurethane enameled rectangular copper wire according to claim 1, It is characterized in that The polyester polyol resin in S1 is one of ethylene glycol dicarbonate, propylene glycol dicarbonate and hexanediol dicarbonate.

3. The directly weldable polyurethane enameled rectangular copper wire according to claim 1, It is characterized in that The inorganic filler in S1 is one of bentonite, talcum powder, glass fiber, barium sulfate and calcium carbonate.

4. The directly weldable polyurethane enameled rectangular copper wire according to claim 1, It is characterized in that The rare earth element in S1 is one or more of La, Ce and Pr.

5. The directly weldable polyurethane enameled rectangular copper wire according to claim 1, It is characterized in that The dispersant in S1 is one of sodium acrylate, water-based acrylic resin, and polyoxyethylene stearyl alcohol ether.

6. The directly weldable polyurethane enameled rectangular copper wire according to claim 1, It is characterized in that The curing agent in S1 is one of diisocyanate and triisocyanate.

7. A method for preparing a directly solderable polyurethane enameled copper flat wire, based on the directly solderable polyurethane enameled copper flat wire according to any one of claims 1 to 6, It is characterized in that The process of preparing the direct-weldable polyurethane enameled copper flat wire is as follows: S71: putting the round copper wire into a wire drawing machine for wire drawing, and the wire drawing oil temperature in the wire drawing machine is less than 40°C; S72: transferring the drawn copper round wire into an annealing furnace, and annealing the wire at a speed of 150 m / min in a nitrogen atmosphere; S73: applying the modified polyurethane paint on the surface of the copper round wire treated by S72, drying it by laser irradiation, and standing it for 12 hours after drying; S74: Apply thermosetting polyamide resin paint to the surface of the product obtained in S73, dry at 60° C. for 12 hours, and stand for 24 hours to obtain a product, a direct-weldable polyurethane enameled copper rectangular wire.

8. The method for preparing the directly weldable polyurethane enameled rectangular copper wire according to claim 7, It is characterized in that The laser power of the laser irradiation in S73 is 200 W, the temperature is 70° C., and the irradiation time is 30 min.

Citation Information

Patent Citations

  • Coated overhead conductor

    CN106062896A

  • Antiskid wear-resistant polyurethane deck paint and preparation method thereof

    CN112430424A