A semiconductor structure and a method for manufacturing the same

By setting dense areas and sparse areas in the semiconductor structure and forming a sacrificial nitride layer on the sparse areas, isolation and connection between metal layers is achieved, and the problem of unconnected metal layers in the integrated circuit is solved, which improves the integrated circuit Yield and performance.

CN118629994BActive Publication Date: 2024-11-05NEXCHIP SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411110514.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-05
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

In integrated circuits, due to the different density of different semiconductor devices, the surface of the metal layer is not on the same plane, resulting in the metal layer in some areas being not connected, affecting the yield and performance of the integrated circuit.

Method used

By setting dense areas and sparse areas on the substrate, the first and second metal layers are formed respectively, and a sacrificial nitride layer is formed on the sparse areas, ensuring that the second metal layer is flush in the dense areas and sparse areas surfaces, realizing metals Isolation and connection between layers.

Benefits of technology

Effectively avoid circuit breakers caused by incomplete openings, improve the yield and performance of integrated circuits, meet the design requirements of metal wiring layers, and avoid the problem of metal layer unconnected due to uneven surfaces, without increasing production costs. and time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118629994B_ABST
    Figure CN118629994B_ABST
Patent Text Reader

Abstract

The present invention discloses a semiconductor structure and a manufacturing method thereof, belonging to the field of semiconductor technology. The semiconductor structure comprises: a substrate, comprising a dense area and a sparse area; a first dielectric layer, arranged on the substrate; a first metal layer, arranged in the first dielectric layer, the surface of the first dielectric layer and the first metal layer on the sparse area is lower than the surface on the dense area; a second dielectric layer, arranged on the first dielectric layer and the first metal layer, the surface of the second dielectric layer on the sparse area is lower than the surface on the dense area; a sacrificial nitride layer, arranged on the second dielectric layer in the sparse area, the surface of the sacrificial nitride layer is flush with the surface of the second dielectric layer on the dense area; a second metal layer, arranged in the second dielectric layer and the sacrificial nitride layer, the surface of the second metal layer on the sparse area and the dense area is flush. The semiconductor structure and the manufacturing method thereof provided by the present invention can improve the yield and performance of integrated circuits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of semiconductor technology, and in particular relates to a semiconductor structure and a manufacturing method thereof. Background Art

[0002] With the continuous development of integrated circuits, the critical dimension (CD) of semiconductor devices has been reduced, and the integration of integrated circuits has been continuously improved. In an integrated circuit, there are multiple different types of semiconductor devices, and the density of different semiconductor devices is different, and different semiconductor devices are connected through metal wiring layers. When forming the metal layer, due to the different densities of different semiconductor devices, the density of the metal layer on the semiconductor device is also different. In the process of forming the first metal layer, the load effect of the chemical mechanical polishing (CMP) process at different density positions causes the surface of the first metal layer to be not in the same plane. As a result, when forming subsequent metal layers, the metal layers in some areas are not connected, resulting in a short circuit, which affects the yield and performance of the integrated circuit. Summary of the invention

[0003] The object of the present invention is to provide a semiconductor structure and a method for manufacturing the same. The semiconductor structure and the method for manufacturing the same provided by the present invention can meet the isolation and connection between metal layers in different regions, avoid short circuits caused by incomplete openings, thereby improving the yield and performance of integrated circuits without increasing additional costs.

[0004] In order to solve the above technical problems, the present invention provides a semiconductor structure, comprising:

[0005] substrate, including dense and sparse regions;

[0006] A first dielectric layer is disposed on the substrate;

[0007] A first metal layer is disposed in the first dielectric layer, wherein surfaces of the first dielectric layer and the first metal layer on the sparse area are lower than surfaces on the dense area;

[0008] A second dielectric layer is disposed on the first dielectric layer and the first metal layer, wherein a surface of the second dielectric layer on the sparse area is lower than a surface of the second dielectric layer on the dense area;

[0009] a sacrificial nitride layer, disposed on the second dielectric layer in the sparse area, wherein a surface of the sacrificial nitride layer is flush with a surface of the second dielectric layer in the dense area; and

[0010] The second metal layer is disposed in the second dielectric layer and the sacrificial nitride layer, and the surface of the second metal layer on the sparse area and the dense area is flush.

[0011] In one embodiment of the present invention, a plurality of semiconductor devices are disposed in the substrate, and the density of the semiconductor devices in the dense area is greater than that in the sparse area.

[0012] In an embodiment of the present invention, the first metal layer is connected to the semiconductor device.

[0013] In one embodiment of the present invention, the second metal layer on the dense area is spaced apart from the first metal layer, and the second metal layer on the sparse area is connected to the first metal layer via a connection structure.

[0014] In one embodiment of the present invention, a cap layer is provided between the first dielectric layer and the substrate, and between the first dielectric layer and the second dielectric layer.

[0015] The present invention also provides a method for manufacturing a semiconductor structure, comprising the following steps:

[0016] Providing a substrate, the substrate comprising a dense area and a sparse area;

[0017] forming a first dielectric layer on the substrate;

[0018] forming a first metal layer in the first dielectric layer, wherein surfaces of the first dielectric layer and the first metal layer on the sparse area are lower than surfaces on the dense area;

[0019] forming a second dielectric layer on the first dielectric layer and the first metal layer, wherein a surface of the second dielectric layer on the sparse area is lower than a surface of the second dielectric layer on the dense area;

[0020] forming a sacrificial nitride layer on the second dielectric layer in the sparse area, wherein a surface of the sacrificial nitride layer is flush with a surface of the second dielectric layer in the dense area; and

[0021] A second metal layer is formed in the second dielectric layer and the sacrificial nitride layer, wherein the second metal layer has surfaces flush with the sparse area and the dense area.

[0022] In one embodiment of the present invention, the manufacturing method further includes:

[0023] forming a cap layer, a second dielectric layer, a sacrificial nitride layer, a sacrificial oxide layer and a hard mask layer in sequence on the first dielectric layer and the first metal layer, wherein the thickness of the sacrificial oxide layer on the dense area is greater than that on the sparse area;

[0024] forming a first photoresist layer on the hard mask layer, wherein the first photoresist layer comprises a first opening and a plurality of second openings, wherein the first opening is disposed on the dense region, the second opening is disposed on the sparse region, and an opening width of the second opening is smaller than an opening width of the first opening; and

[0025] Using the first photoresist layer as a mask, etching is performed toward the substrate to form a first groove at the first opening position and a second groove at the second opening position, wherein the bottom of the first groove is in the second dielectric layer and the bottom of the second groove is in the sacrificial oxide layer.

[0026] In one embodiment of the present invention, the manufacturing method further includes:

[0027] forming a first compensation layer in the first groove and the second groove;

[0028] Etching the first compensation groove to expose the sacrificial oxide layer; and

[0029] The etching conditions are changed to etch the cap layer from the bottom of the second groove to the first metal layer to form an opening, and the first compensation layer remains in the first groove.

[0030] In one embodiment of the present invention, the manufacturing method further includes:

[0031] forming a second compensation layer in the first compensation layer and the opening;

[0032] forming a second photoresist layer on the second compensation layer, wherein the second photoresist layer comprises a plurality of third openings arranged on the dense area and a fourth opening arranged on the sparse area, wherein the opening width of the third opening is smaller than the opening width of the first opening, and the fourth opening exposes the plurality of openings and the area between the openings;

[0033] Using the second photoresist layer as a mask, etching is performed, the third opening position forms a third recess, the fourth opening position forms a fourth recess, and the opening is etched to the first metal layer;

[0034] removing the second photoresist layer, the second compensation layer and the first compensation layer,

[0035] depositing a second metal layer in the third recess and the fourth recess;

[0036] The second metal layer is planarized until the second metal layer in the third recess and the fourth recess is flush.

[0037] In one embodiment of the present invention, after removing the second compensation layer and the first compensation layer, the tops of adjacent third recesses are connected, the opening width of the top connected parts of the third recesses is greater than the opening width of the fourth recess, and the surface of the second metal layer in the dense area is lower than the surface in the sparse area.

[0038] In summary, the present invention provides a semiconductor structure and a method for manufacturing the same. The unexpected technical effect of the present application is that it can meet the isolation and connection between metal layers in different regions, avoid short circuits caused by incomplete openings, and thus improve the yield and performance of integrated circuits. It can meet the design requirements of the metal wiring layer, while avoiding the lack of connection between metal layers that need to be connected due to uneven surfaces, thereby avoiding short circuit problems. It can solve the problem of openings not being etched to the first metal layer due to steps in sparse areas without increasing the photolithography procedure, solve the short circuit problem between metal layers, and does not increase the manufacturing cost or extend the manufacturing time. It can level the uneven surface caused by the formation of the first metal layer when forming the second metal layer, and when forming subsequent metal layers or other structures, it can be manufactured on a flat substrate, which can improve the yield of the process and improve the quality of the semiconductor structure.

[0039] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0041] Figure 1 FIG. 1 is a schematic diagram of forming a first recess and a second recess in a first dielectric layer according to an embodiment of the present invention.

[0042] Figure 2 It is a schematic diagram of depositing a first metal layer in a first recess and a second recess in one embodiment of the present invention.

[0043] Figure 3 FIG. 1 is a schematic diagram of a first metal layer after a planarization process in one embodiment of the present invention.

[0044] Figure 4 It is a schematic diagram of sequentially forming a second capping layer, a second dielectric layer, a sacrificial nitride layer, a sacrificial oxide layer and a hard mask layer on a first metal layer in one embodiment of the present invention.

[0045] Figure 5It is a schematic diagram of planarizing the sacrificial oxide layer after sequentially forming a second cap layer, a second dielectric layer, a sacrificial nitride layer and a sacrificial oxide layer in another embodiment of the present invention.

[0046] Figure 6 It is a schematic diagram of the first etching process when forming the first groove and the second groove in one embodiment of the present invention.

[0047] Figure 7 It is a schematic diagram of the second etching process when forming the first groove and the second groove in one embodiment of the present invention.

[0048] Figure 8 FIG. 4 is a schematic diagram of forming a first compensation layer in one embodiment of the present invention.

[0049] Fig. 9 It is a schematic diagram of etching the first compensation layer and the bottom of the second groove to form an opening in one embodiment of the present invention.

[0050] Fig.10 FIG. 4 is a schematic diagram of forming a second compensation layer and a second photoresist layer in one embodiment of the present invention.

[0051] Fig.11 FIG. 4 is a schematic diagram of forming a third recess and a fourth recess in one embodiment of the present invention.

[0052] Fig.12 It is a schematic diagram after removing the second photoresist layer and the compensation layer in one embodiment of the present invention.

[0053] Fig.13 FIG. 1 is a schematic diagram of a second metal layer after being deposited in one embodiment of the present invention.

[0054] Fig.14 FIG. 4 is a schematic diagram of a semiconductor structure after a second metal layer planarization process according to an embodiment of the present invention.

[0055] Description of labels:

[0056] 10. substrate; 100. dense area; 200. sparse area; 101. semiconductor device; 102. conductive plug; 11. interlayer dielectric layer; 12. first cap layer; 13. first dielectric layer; 131. first recess; 132. second recess; 14. first metal layer; 141. first subdivision; 142. second subdivision; 15. second cap layer; 16. second dielectric layer; 17. sacrificial nitride layer; 18. sacrificial oxide layer; 19. hard mask Layer; 20, first photoresist layer; 201, first opening; 202, second opening; 211, first groove; 212, second groove; 21, first compensation layer; 22, second compensation layer; 221, opening; 23, second photoresist layer; 231, third opening; 232, fourth opening; 241, third recess; 242, fourth recess; 25, second metal layer; 251, third subdivision; 252, fourth subdivision; 253, connection structure. DETAILED DESCRIPTION

[0057] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0058] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0059] In the description of this specification, it should be understood that the directions or positional relationships indicated by the terms "center", "upper", "lower", "front", "back", "left", "right", etc. are based on the directions or positional relationships shown in the drawings, and are only for the convenience of describing this solution and simplifying the description, rather than indicating or implying that the device or component referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on this solution. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0060] See also Fig.14As shown, the present invention provides a semiconductor structure, including a substrate 10 and a multi-layer metal layer arranged on the substrate 10, wherein the substrate 10 includes a dense area 100 and a sparse area 200, and the first metal layer is arranged in the first dielectric layer 13. When the first metal layer is formed, the surface of the first dielectric layer 13 and the first metal layer on the sparse area 200 is lower than the surface on the dense area 100 due to the different pattern densities. The second dielectric layer 16 and the sacrificial nitride layer 17 are arranged on the first metal layer and the first dielectric layer 13, so that the surface of the formed second metal layer can be flush, and the surface of the sacrificial nitride layer 17 is flush with the surface of the second dielectric layer 16 on the dense area 100, while ensuring the connection between the metal layers on the sparse area. Through the semiconductor structure of the present application, the isolation and connection between the metal layers in different regions are met, and the circuit break caused by incomplete opening is avoided, thereby improving the yield and performance of the integrated circuit. At the same time, the uneven surface caused by the formation of the first metal layer is leveled on the surface of the second metal layer, thereby improving the yield of the subsequent manufacturing process.

[0061] See also Figure 1As shown, in one embodiment of the present invention, a substrate 10 is first provided. The substrate 10 can be any material suitable for forming a semiconductor device, such as silicon carbide (SiC), gallium nitride (GaN), aluminum nitride (AlN), indium nitride (InN), indium phosphide (InP), gallium arsenide (GaAs), silicon germanium (GeSi), sapphire, silicon wafer or other semiconductor materials formed by III / V compounds, etc., and also includes a stacked structure composed of these semiconductor materials, or silicon on insulator, stacked silicon on insulator, silicon germanium on insulator, and germanium on insulator, etc. Among them, a plurality of semiconductor devices 101 are formed on the substrate 10, and the substrate 10 includes a dense area 100 and a sparse area 200, and the density of the semiconductor devices 101 on the dense area 100 is greater than the density of the semiconductor devices 101 on the sparse area 200. The present invention does not limit the type of semiconductor device 101. The semiconductor device 101 is, for example, a field effect transistor (FET), a metal-oxide-semiconductor field-effect transistor (MOSFET), a complementary metal oxide semiconductor (CMOS), an insulated gate bipolar transistor (IGBT), a fast recovery diode (FRD), a high-speed and high-efficiency rectifier diode (HED), a constant voltage diode, a high-frequency diode, a light-emitting diode (LED), a gate turn off thyristor (GTO), a light triggered thyristor (LTT), a thyristor, a charge coupled device (CCD image sensor), a digital signal processor (DSP), a photo relay or a microprocessor (MCU). One or more of the semiconductor devices such as processors and the like can be manufactured according to the manufacturing requirements of the semiconductor structure.

[0062] See also Figure 1As shown, in one embodiment of the present invention, an interlayer dielectric layer 11 is provided on the substrate 10, and a plurality of conductive plugs 102 are provided in the interlayer dielectric layer 11, and the conductive plugs 102 are connected to the semiconductor device 101 in the substrate 10. The interlayer dielectric layer 11 is, for example, an insulating material such as silicon dioxide (SiO2) or silicon nitride (SiN), which can isolate the semiconductor device 101 from the metal layer, prevent the diffusion of the metal, and protect the semiconductor device 101 when preparing the metal layer to prevent the semiconductor device 101 from being damaged. In this embodiment, the conductive plug 102 is, for example, a low-resistance material such as metal tungsten, metal silver or metal gold, to ensure that the conductive plug 102 has a small resistance when connected to the metal layer prepared later, thereby improving the performance of the semiconductor structure.

[0063] See also Figure 1 As shown, in one embodiment of the present invention, a first capping layer 12 and a first dielectric layer 13 are formed on the interlayer dielectric layer 11. The first capping layer 12 is disposed on the interlayer dielectric layer 11, and the first dielectric layer 13 is disposed on the first capping layer 12, and the first capping layer 12 is, for example, silicon carbide nitride (SiCN) or silicon nitride, etc., to prevent metal ions in the metal layer from diffusing to the interlayer dielectric layer 11, and the first capping layer 12 can be, for example, deposited by chemical vapor deposition (CVD) or plasma enhanced chemical vapor deposition (PECVD). The first dielectric layer 13 is, for example, made of a low dielectric constant (Low-K) material such as silicon dioxide or silicon fluoride (SiF), silicon oxycarbide (SiOC) or silicon oxyfluoride (SiOF) to improve the reliability of the semiconductor structure, and the first dielectric layer 13 can be deposited by chemical vapor deposition or low pressure chemical vapor deposition (LPCVD). The present invention does not limit the thickness of the first capping layer 12 and the first dielectric layer 13 , that is, the thickness of the first capping layer 12 and the first dielectric layer 13 can be selected according to the preparation requirements of the semiconductor structure.

[0064] See also Figure 1As shown, in one embodiment of the present invention, a patterned photoresist layer (not shown in the figure) is formed on the first dielectric layer 13, and the patterned photoresist layer is used as a mask to etch the first dielectric layer 13 and the first cap layer 12, and the etching is stopped until the interlayer dielectric layer 11 is reached to form a concave portion, and after the concave portion is formed, the patterned photoresist layer is removed by wet etching or ashing. In this embodiment, the concave portion is formed, for example, by a dry etching process, and the etching gas can be, for example, one or a combination of trifluoromethane (CHF3), difluoromethane (CH2F2), nitrogen trifluoride (NF3), sulfur hexafluoride (SF6) or nitrogen (N2), or a mixture of them and oxygen (O2). The recesses include a first recess 131 and a second recess 132 . The first recess 131 is disposed on the semiconductor device 101 in the dense area 100 , and the second recess 132 is disposed on the semiconductor device 101 in the sparse area 200 . The density of the first recess 131 is greater than that of the second recess 132 .

[0065] See also Figure 1 to Figure 2 As shown, in one embodiment of the present invention, after the recess is formed, a first metal layer 14 is deposited on the recess and the first dielectric layer 13 until the first metal layer 14 completely fills the recess. In the present application, before the first metal layer 14 is deposited, a barrier layer (not shown in the figure) can be formed on the sidewalls and bottom of the first recess 131 and the second recess 132, and the barrier layer is formed, for example, by physical vapor deposition (PVD) and the like. The barrier layer is, for example, tantalum (Ta) or tantalum nitride (TaN) and the like, and the thickness of the barrier layer is, for example, 2nm to 5nm. To enhance the adhesion of the metal to the sidewalls of the first recess 131 and the second recess 132, and improve the electrical properties of the semiconductor structure. Among them, the deposited first metal layer 14 is, for example, a metal copper layer, a metal aluminum layer or a metal tungsten layer. In the present embodiment, the first metal layer 14 is, for example, a metal copper layer, and the metal copper layer is, for example, formed by physical vapor deposition or electroplating.

[0066] See also Figures 2 to 3 As shown, in one embodiment of the present invention, after the first metal layer 14 is deposited, a first planarization process is performed, such as a planarization process performed by chemical mechanical polishing, until the metal in the first recess 131 is flush with the first dielectric layer 13 on both sides. The first metal layer 14 finally formed includes a first sub-portion 141 and a second sub-portion 142, wherein the first sub-portion 141 is formed in the first recess 131, and the second sub-portion 142 is formed in the second recess 132. During the planarization process, since the polishing speed of the sparse area 200 is fast, the surfaces of the first dielectric layer 13 and the first metal layer on the sparse area 200 are lower than those on the dense area 100, forming a height difference.

[0067] See also Figures 3 to 5 As shown, in one embodiment of the present invention, after the first metal layer is planarized, a second capping layer 15, a second dielectric layer 16, a sacrificial nitride layer 17, a sacrificial oxide layer 18 and a hard mask layer 19 are sequentially formed on the first dielectric layer 13 and the first metal layer. The material of the second capping layer 15 is, for example, silicon carbide nitride or silicon nitride, the second dielectric layer 16 is, for example, a low dielectric constant material such as silicon dioxide or silicon fluoride, silicon oxycarbide or silicon oxyfluoride, the sacrificial nitride layer 17 is, for example, a silicon nitride layer or silicon carbide nitride, the sacrificial oxide layer 18 is, for example, a silicon oxide layer, and the hard mask layer 19 is, for example, a material such as titanium nitride. The sacrificial nitride layer 17 and the sacrificial oxide layer 18 are used to ensure complete contact and surface flatness between the metal layers when the second metal layer and the connection structure are subsequently formed, and the hard mask layer 19 plays a role in transferring the pattern in the subsequent manufacturing process. When forming the second metal layer, the sacrificial nitride layer and the sacrificial oxide layer can ensure that the opening is exposed to the first metal layer, and can level the second metal layer, thereby improving the quality of the semiconductor structure.

[0068] See also Figures 4 to 5As shown, in one embodiment of the present invention, the present invention does not limit the thickness and deposition method of the second cap layer 15, the second dielectric layer 16 and the sacrificial nitride layer 17, and can be selected according to the preparation requirements of the semiconductor structure. When forming the second cap layer 15, the second dielectric layer 16 and the sacrificial nitride layer 17, due to the height difference between the dense area 100 and the sparse area 200, the formed second cap layer 15, the second dielectric layer 16 and the sacrificial nitride layer 17 will inherit this height difference in the sparse area 200. In one embodiment of the present invention, the sacrificial oxide layer 18 is formed by chemical vapor deposition process and using Tetraethyl Orthosilicate (TEOS). Due to the fluidity of Tetraethyl Orthosilicate, the thickness of the sacrificial oxide layer 18 on the sparse area 200 is greater than the thickness of the sacrificial oxide layer 18 on the dense area 100. In another embodiment of the present invention, when forming the sacrificial oxide layer 18, the deposition time is extended to increase the deposition thickness of the sacrificial oxide layer 18, and then chemical mechanical polishing is performed for flattening to make the surface of the sacrificial oxide layer 18 flat. After forming the sacrificial oxide layer 18, a hard mask layer 19 is formed on the sacrificial oxide layer 18. The present invention does not limit the thickness and deposition method of the hard mask layer 19, which can be selected according to the preparation requirements of the semiconductor structure. After forming the hard mask layer 19, a first photoresist layer 20 is formed on the hard mask layer 19, and the first photoresist layer 20 is exposed and developed to form a first opening 201 and a plurality of second openings 202, wherein the first opening 201 is arranged on the dense area 100 and covers at least two first sections 141, and the second opening 202 is arranged on the sparse area 200, and the opening width of the second opening 202 is smaller than the width of the second section 142, that is, much smaller than the width of the first opening 201, and two second openings are arranged on a single second section 142, for example.

[0069] See also Figures 4 to 7 As shown, in one embodiment of the present invention, after forming the first photoresist layer 20, the first photoresist layer 20 is used as a mask to perform etching in the direction of the substrate 10. In the present application, the etching is performed in two steps, for example, to form a first groove 211 and a second groove 212, wherein the first opening 201 defines the position of the first groove 211, and the second opening 202 locates the position of the second groove 212. Figure 6As shown, during the first etching, since the thickness of the sacrificial oxide layer 18 on the sparse area 200 is greater than the thickness of the sacrificial oxide layer 18 on the dense area 100, when the first groove 211 is etched to the sacrificial nitride layer 17, the second groove 212 is still located in the sacrificial oxide layer 18. Therefore, with the sacrificial nitride layer 17 on the dense area 100 as the etching stop layer, when the first groove 211 is etched to the sacrificial nitride layer 17, the second groove 212 is located in the sacrificial oxide layer 18. Then, the etching conditions are changed, and the second etching is performed, and the sacrificial nitride layer 17 and part of the second dielectric layer 16 exposed by the first groove 211 are removed by selective etching. Since the etching selectivity of the sacrificial nitride layer 17 and the sacrificial oxide layer 18 is relatively large, after the second etching is completed, the first groove 211 stops in the second dielectric layer 16, and the second groove 212 stops in the sacrificial oxide layer 18. In this embodiment, the groove is formed by, for example, dry etching, and after the etching is completed, the first photoresist layer 20 is removed by wet etching or ashing. By forming the first opening 201 with a larger opening width, the stop positions of the first groove and the second groove can be controlled, thereby ensuring the contact of the subsequently formed openings in the subsequent process.

[0070] See also Figures 7 and 8 As shown, in one embodiment of the present invention, after removing the first photoresist layer 20, a first compensation layer 21 is deposited on the groove and the hard mask layer 19, and the first compensation layer 21 is, for example, an organic dielectric layer (ODL) material. Specifically, the first compensation layer 21 can be formed by a spin coating process, and after the organic dielectric layer is spin-coated, the height of the first compensation layer 21 on the dense area 100 is slightly greater than the height of the first compensation layer 21 on the sparse area 200.

[0071] See also Figures 7 to 9 As shown, in one embodiment of the present invention, after the first compensation layer 21 is formed, the first compensation layer 21 is directly etched. During the etching process, since the first groove 211 is deeper than the second groove 212 and the thickness of the first compensation layer 21 on the dense area 100 is greater, when the first compensation layer 21 in the second groove 212 is completely removed, part of the first compensation layer 21 remains in the first groove 211. During the etching process, when the sacrificial oxide layer 18 in the second groove 212 is detected, the etching conditions are changed, and the sacrificial oxide layer 18, the sacrificial nitride layer 17, the second dielectric layer 16 and part of the second cap layer 15 at the bottom of the second groove 212 are removed by selective etching to form an opening 221. In this embodiment, the opening 221 is formed by dry etching, for example. By forming the first compensation layer 21, the opening 221 can be etched to form the opening without setting a photoresist layer, thereby ensuring contact between metal layers.

[0072] See also Figures 9 and 10As shown, in one embodiment of the present invention, after the opening 221 is formed, a second compensation layer 22 is formed on the surface of the substrate 10, and the second compensation layer 22 is, for example, an organic dielectric layer material. Specifically, the second compensation layer 22 can be formed by a spin coating process, and after the organic dielectric layer is spin-coated, the thickness of the second compensation layer 22 on the dense area 100 is slightly greater than the thickness of the second compensation layer 22 on the sparse area 200. A second photoresist layer 23 is formed on the second compensation layer 22, and the second photoresist layer 23 is exposed and developed to form a plurality of third openings 231 and fourth openings 232. The third opening 231 is disposed on the dense area 100, and the third opening 231 is disposed on the first subsection 141, the number of the third openings 231 is the same as the number of the first subsection 141, the fourth opening 232 is disposed on the sparse area 200, and the fourth opening 232 exposes a plurality of openings 221 and the area between the openings 221, that is, the fourth opening 232 is located on the second subsection 142, and exposes all the openings 221 on the second subsection 142. In this embodiment, the opening width of the fourth opening 232 is greater than the opening width of the third opening 231.

[0073] See also Figure 10 to Figure 11 As shown, in one embodiment of the present invention, after forming the second photoresist layer 23, the second photoresist layer 23 is used as a mask to etch in the direction of the substrate 10 to remove the compensation layer, part of the second dielectric layer 16 and the second cap layer 15 in the opening 221, so as to form the third recess 241 and the fourth recess 242. In this embodiment, etching is performed, for example, by a dry etching process. During the etching process, since the opening width of the fourth opening 232 is greater than the opening width of the third opening 231, and the surface of the second compensation layer 22 on the sparse area 200 is lower than the surface of the second compensation layer 22 on the dense area 100, when etching to the opening 221 in the fourth recess 242 to expose the second sub-portion 142, the third recess 241 is etched into the second dielectric layer 16, and the etching stops. That is, the bottom of the third recess 241 is at a preset distance from the first sub-portion 141, and the bottom of the fourth recess 242 between the openings 221 is flush with the bottom of the third recess 241. In the present application, in the process of forming the opening 221, the fourth recess 242 and the third recess 241, it is only necessary to optimize the opening position of the photolithography plate. Without increasing the photolithography procedure, the problem of the opening not being etched to the first metal layer due to the steps in the sparse area is solved, and the problem of short circuit between the metal layers is solved without increasing the production cost or extending the production time.

[0074] See also Figure 11 to Figure 12As shown, in one embodiment of the present invention, after the recess etching is completed, the second photoresist layer 23 is removed by ashing, and the second compensation layer 22 and the first compensation layer 21 are removed by ashing. After the second compensation layer 22 and the first compensation layer 21 are removed, the tops of the adjacent third recesses 241 are connected, and the opening width of the connected portion of the top of the third recess 241 is greater than the opening width of the fourth recess 242.

[0075] See also Figure 12 to Figure 13 As shown, in one embodiment of the present invention, after removing the compensation layer, a second metal layer 25 is deposited in the third recess 241 and the fourth recess 242 until the second metal layer 25 completely fills the recess. In the present application, before depositing the second metal layer 25, a barrier layer (not shown in the figure) can be formed on the sidewalls and bottom of the third recess 241 and the fourth recess 242, and the barrier layer is formed, for example, by physical vapor deposition, etc., and the barrier layer is, for example, tantalum or tantalum nitride, etc., and the thickness of the barrier layer is, for example, 2nm~5nm. To enhance the adhesion of the metal to the sidewalls of the third recess 241 and the fourth recess 242, and improve the electrical properties of the semiconductor structure. Among them, the deposited second metal layer 25 is, for example, a metal copper layer, a metal aluminum layer or a metal tungsten layer. In this embodiment, the second metal layer 25 is, for example, a metal copper layer, and the metal copper layer is, for example, formed by physical vapor deposition or electroplating. In this embodiment, for example, an electrochemical plating method is selected to form the second metal layer 25. Since the opening width of the top connecting portion of the third recess 241 is greater than the opening width of the fourth recess 242, the deposition speed of the second metal layer 25 in the fourth recess 242 is greater than the deposition speed in the third recess 241, and the surface of the second metal layer 25 in the sparse area 200 protrudes from the surface of the second metal layer 25 in the dense area 100.

[0076] See also Figure 13 to Figure 14As shown, in one embodiment of the present invention, after the second metal layer 25 is deposited, a second planarization process is performed, such as a planarization process performed by chemical mechanical polishing, to remove the second metal layer 25 in the top connecting portion of the third recess, until the metal layers in the third recess and the fourth recess are flush. The second metal layer 25 finally formed includes a third subdivision 251 and a fourth subdivision 252, wherein the third subdivision 251 is formed in the third recess, and the fourth subdivision 252 is formed in the fourth recess, wherein the second metal layer in the bottom opening of the fourth recess is defined as a connection structure 253. The third subdivision 251 is isolated from the first subdivision 141, and the fourth subdivision 252 and the second subdivision 142 are connected by the connection structure 253, which can ensure good contact between the metal layers in the sparse area 200. Through the present application, the isolation and connection between the metal layers in different regions can be met to meet the design requirements of the metal wiring layer, while avoiding the non-connection between the metal layers that need to be connected in the sparse area due to the uneven surface, thereby avoiding the problem of short circuit and improving the yield and performance of the integrated circuit.

[0077] See also Figure 13 to Figure 14 As shown, in one embodiment of the present invention, during the planarization process, since the second metal layer 25 on the sparse area 200 is higher than the dense area 100, the grinding speed of the second metal layer 25 in the sparse area 200 is greater than the grinding speed of the dense area 100. After the grinding stops, the surfaces of the third section 251 and the fourth section 252 are flush, the third section 251 is flush with the second dielectric layer 16 on both sides, and the fourth section 252 is flush with the sacrificial nitride layer 17 on both sides. The sacrificial nitride layer 17 on the sparse area 200 is flush with the second dielectric layer 16 on the dense area 100, that is, after the second planarization process, it can ensure that the surface of the second metal layer is flush, that is, when the second metal layer is formed, the uneven surface caused by the formation of the first metal layer can be leveled, and when the subsequent metal layer or other structure is formed, it can be manufactured on a flat substrate, which can improve the yield of the process and improve the quality of the semiconductor structure. After the second metal layer is formed, the subsequent metal layer or other structure is manufactured, which will not be elaborated here.

[0078] In summary, the present invention provides a semiconductor structure and a method for manufacturing the same. By improving the semiconductor structure and the method for manufacturing the same, the unexpected technical effect of the present application is that the isolation and connection between metal layers in different regions can be met, and the short circuit caused by incomplete openings can be avoided, thereby improving the yield and performance of the integrated circuit. It can meet the design requirements of the metal wiring layer, while avoiding the non-connection between metal layers that need to be connected due to uneven surfaces, thereby avoiding the short circuit problem. It can solve the problem of the opening not being etched to the first metal layer due to the height difference in the sparse area on the basis of not increasing the photolithography procedure, solve the short circuit problem between the metal layers, and does not increase the production cost or extend the production time. It can level the uneven surface caused by the formation of the first metal layer when forming the second metal layer, and when forming subsequent metal layers or other structures, it can be manufactured on a flat substrate, which can improve the yield of the process and improve the quality of the semiconductor structure.

[0079] The above description of the illustrated embodiments of the present invention (including the contents described in the Abstract) is not intended to be an exhaustive list or to limit the present invention to the precise form disclosed herein. Although specific embodiments of the present invention and examples of the present invention are described herein for illustrative purposes only, various equivalent modifications are possible within the spirit and scope of the present invention as will be recognized and appreciated by those skilled in the art. As noted, these modifications may be made to the present invention in accordance with the above description of the embodiments described in the present invention, and these modifications will be within the spirit and scope of the present invention.

[0080] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the inventive concept, such as the technical solution formed by replacing the above features with the technical features with similar functions disclosed in this application (but not limited to). In addition to the technical features described in the specification, the remaining technical features are known technologies to those skilled in the art. In order to highlight the innovative features of the present invention, the remaining technical features will not be described in detail here.

Claims

1. A semiconductor structure, characterized in that: include: substrate, including dense and sparse regions; A first dielectric layer is disposed on the substrate; A first metal layer is disposed in the first dielectric layer, wherein surfaces of the first dielectric layer and the first metal layer on the sparse area are lower than surfaces on the dense area; A second dielectric layer is disposed on the first dielectric layer and the first metal layer, wherein a surface of the second dielectric layer on the sparse area is lower than a surface of the second dielectric layer on the dense area; A sacrificial nitride layer, disposed on the second dielectric layer in the sparse area, wherein a surface of the sacrificial nitride layer is flush with a surface of the second dielectric layer in the dense area; as well as A second metal layer is arranged in the second dielectric layer and the sacrificial nitride layer, the surfaces of the second metal layer on the sparse area and the dense area are flush, the second metal layer on the dense area is spaced apart from the first metal layer, and the second metal layer on the sparse area is connected to the first metal layer via a connecting structure.

2. The semiconductor structure according to claim 1, characterized in that: A plurality of semiconductor devices are arranged in the substrate, and the density of the semiconductor devices in the dense area is greater than that in the sparse area.

3. The semiconductor structure according to claim 2, characterized in that: The first metal layer is connected to the semiconductor device.

4. The semiconductor structure according to claim 1, characterized in that: A cap layer is disposed between the first dielectric layer and the substrate, and between the first dielectric layer and the second dielectric layer.

5. A method for manufacturing a semiconductor structure, characterized in that: The following steps are involved: Providing a substrate, the substrate comprising a dense area and a sparse area; forming a first dielectric layer on the substrate; forming a first metal layer in the first dielectric layer, wherein surfaces of the first dielectric layer and the first metal layer on the sparse area are lower than surfaces on the dense area; forming a second dielectric layer on the first dielectric layer and the first metal layer, wherein a surface of the second dielectric layer on the sparse area is lower than a surface of the second dielectric layer on the dense area; forming a sacrificial nitride layer on the second dielectric layer in the sparse area, wherein a surface of the sacrificial nitride layer is flush with a surface of the second dielectric layer in the dense area; as well as A second metal layer is formed in the second dielectric layer and the sacrificial nitride layer, the surfaces of the second metal layer on the sparse area and the dense area are flush, the second metal layer on the dense area is spaced apart from the first metal layer, and the second metal layer on the sparse area is connected to the first metal layer via a connecting structure.

6. The method for manufacturing a semiconductor structure according to claim 5, characterized in that: The production method further comprises: forming a cap layer, a second dielectric layer, a sacrificial nitride layer, a sacrificial oxide layer and a hard mask layer in sequence on the first dielectric layer and the first metal layer, wherein the thickness of the sacrificial oxide layer on the dense area is greater than that on the sparse area; forming a first photoresist layer on the hard mask layer, wherein the first photoresist layer comprises a first opening and a plurality of second openings, wherein the first opening is disposed on the dense region, the second opening is disposed on the sparse region, and an opening width of the second opening is smaller than an opening width of the first opening; and Using the first photoresist layer as a mask, etching is performed toward the substrate to form a first groove at the first opening position and a second groove at the second opening position, wherein the bottom of the first groove is in the second dielectric layer and the bottom of the second groove is in the sacrificial oxide layer.

7. The method for manufacturing a semiconductor structure according to claim 6, characterized in that: The production method further comprises: forming a first compensation layer in the first groove and the second groove; Etching the first compensation groove to expose the sacrificial oxide layer; and The etching conditions are changed to etch the cap layer from the bottom of the second groove to the first metal layer to form an opening, and the first compensation layer remains in the first groove.

8. The method for manufacturing a semiconductor structure according to claim 7, characterized in that: The production method further comprises: forming a second compensation layer in the first compensation layer and the opening; forming a second photoresist layer on the second compensation layer, wherein the second photoresist layer comprises a plurality of third openings arranged on the dense area and a fourth opening arranged on the sparse area, wherein the opening width of the third opening is smaller than the opening width of the first opening, and the fourth opening exposes the plurality of openings and the area between the openings; Using the second photoresist layer as a mask, etching is performed, the third opening position forms a third recess, the fourth opening position forms a fourth recess, and the opening is etched to the first metal layer; removing the second photoresist layer, the second compensation layer and the first compensation layer, depositing a second metal layer in the third recess and the fourth recess; The second metal layer is planarized until the second metal layer in the third recess and the fourth recess is flush.

9. The method for manufacturing a semiconductor structure according to claim 8, characterized in that: After removing the second compensation layer and the first compensation layer, the tops of the adjacent third recesses are connected, the opening width of the top connected parts of the third recesses is greater than the opening width of the fourth recess, and the surface of the second metal layer on the dense area is lower than the surface on the sparse area.