Metal composite powder for additive manufacturing and preparation method thereof

By mixing and heating and melting aluminum ingots with porous graphene and nitrogen-doped graphene in additive manufacturing, aluminium-porous graphene composite powder is formed and mixed with aluminum alloy ingots, the poor mechanical properties of traditional aluminum alloy powder molded parts are solved. The problem of high density and mechanical properties have been improved.

CN118635513BActive Publication Date: 2024-11-15JIANGSU VILORY ADVANCED MATERIALS TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411111451.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-15
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

In additive manufacturing, the mechanical properties of molded parts are poor and cannot take into account both thermal conductivity and strength.

Method used

The aluminum ingot is heated and melted under an argon atmosphere, and the aluminum-porous graphene composite powder is formed by aerosolization method, and mixed with the aluminum alloy ingot for ball milling and screening. Prepare metal composite powders for additive manufacturing.

Benefits of technology

It improves the fluidity of the powder, the density and mechanical properties of the print parts, improves the thermal conductivity and strength of aluminum alloy powder, and meets the requirements of complex component molding of aluminum alloy materials in additive manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention relates to the field of additive manufacturing technology, and specifically to a metal composite powder for additive manufacturing and a preparation method thereof. The metal composite powder for additive manufacturing of the present invention is obtained by filling molten aluminum into the pores of porous graphene, adding the molten aluminum and nitrogen-doped graphene together into an aluminum alloy melt, and then sieving and drying after atomization treatment. The metal composite powder for additive manufacturing of the present invention has high powder fluidity, and the printed parts obtained by 3D printing have excellent densification and mechanical properties, and have good application prospects in the field of aluminum alloy powders used in additive manufacturing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of additive manufacturing, and in particular to a metal composite powder for additive manufacturing and a preparation method thereof. Background Art

[0002] Additive manufacturing technology, also known as 3D printing technology, is relative to traditional "subtractive manufacturing" technologies such as machining. It is based on the principle of accumulation. By accumulating two-dimensional cross-sections point by point to create a three-dimensional entity, this technology can realize the direct preparation of three-dimensional digital models to solid parts, making the part structure lightweight and the performance complex. Compared with traditional manufacturing technology, additive manufacturing technology has the advantages of no mold, high flexibility, short cycle, and no restrictions on part structure and materials. Additive manufacturing technology is expected to become a representative technology of the "third industrial revolution".

[0003] As a lightweight and high-strength material, aluminum alloy has always played a pivotal role in various fields due to its excellent specific strength. Especially in the field of aerospace, the requirements for aluminum alloy are increasing and becoming increasingly demanding. In addition to requiring lightweight materials, flexible and integrated component design is also required. The additive manufacturing process in the current processing method, especially the additive manufacturing process of aluminum alloy, needs to meet the requirements of lightweight and high-strength materials, as well as the design and molding requirements of complex components.

[0004] Patent technical document CN202011605054.2 discloses a rare earth aluminum alloy powder suitable for additive manufacturing and a preparation method thereof. The invention heats an aluminum ingot and melts it into aluminum liquid; adds the required alloy elements to the aluminum liquid to form an alloy liquid, uses a guide tube to guide the alloy liquid out, and uses a high-pressure airflow to impact the alloy liquid. The alloy liquid is atomized and forms fine droplets under the action of surface tension, and solidifies into spherical alloy powder; the spherical alloy powder is collected in a vacuum collector, screened, and dried to obtain a rare earth aluminum alloy powder. The present invention has the characteristics of high sphericity, less satellite powder and hollow powder, low oxygen content, and high bulk density, which can meet the use requirements of different printing conditions of additive manufacturing, but it ignores the problem of high reflectivity of aluminum alloy to laser.

[0005] Patent technical document CN202111678901.2 discloses an aluminum alloy powder and a preparation method thereof, wherein the method comprises mixing aluminum alloy powder and second phase particles and subjecting the mixture to ball milling to obtain a primary mixed powder; subjecting the primary mixed powder to heat treatment to obtain a heat-treated primary mixed powder; subjecting the heat-treated primary mixed powder to plasma spheroidization to obtain an aluminum alloy powder containing second phase particles, which overcomes the technical difficulty in the prior art that the thermal conductivity and strength of aluminum alloy materials in additive manufacturing cannot be taken into account at the same time. The product has broad application prospects in the fields of automobiles, aerospace, electronic communications, etc., but it does not take into account the problem of poor interface compatibility between graphene and aluminum alloy matrix, which often has an adverse effect on the compactness and mechanical properties of the molded parts during additive manufacturing. Summary of the invention

[0006] In view of this, the purpose of the present invention is to propose a metal composite powder for additive manufacturing and a preparation method thereof, so as to solve the problem that traditional aluminum alloy powder has poor mechanical properties in 3D printed molded parts.

[0007] Based on the above purpose, the present invention provides a method for preparing a metal composite powder for additive manufacturing, comprising the following steps:

[0008] S1: In an argon atmosphere, an aluminum ingot is heated and melted into aluminum liquid at a temperature of 730°C-780°C, and then porous graphene is added to the aluminum liquid and stirred evenly to obtain a composite melt;

[0009] S2: The composite melt is discharged through a flow guide tube, broken into fine droplets by gas atomization, and low-energy ball milling is performed after solidification to obtain aluminum-porous graphene composite powder;

[0010] S3: Under an argon atmosphere, the aluminum alloy ingot is melted at 900° C.-1000° C. to form an aluminum alloy liquid, and then the aluminum-porous graphene composite powder and the nitrogen-doped graphene powder are added and stirred to obtain a composite alloy melt;

[0011] S4: The composite alloy melt is discharged through a flow guide tube, and is broken into fine droplets by a gas atomization method, and spherical aluminum alloy powder is obtained after solidification;

[0012] S5: Under an argon atmosphere, the spherical aluminum alloy powder is screened and dried to obtain a metal composite powder for additive manufacturing.

[0013] Preferably, the preparation steps of the porous graphene in step S1 are as follows:

[0014] In an ice water bath, graphite powder, concentrated sulfuric acid and potassium permanganate are mixed and reacted for 2-24 hours, then reacted at 35°C for 10-60 hours, then heated to 50-80°C, a pore-forming agent is added, and the reaction is continued for 2-8 hours. Finally, hydrogen peroxide is added to obtain a mixed solution; then a coagulant is added to the mixed solution, filtered, washed to make the pH of the filtrate 7, dried, and reduced at high temperature to obtain porous graphene.

[0015] Preferably, the weight ratio of the graphite powder, concentrated sulfuric acid, potassium permanganate, pore-forming agent, hydrogen peroxide and coagulation agent is 1:30-100:5-10:3-7:5-20:0.1-0.5.

[0016] Preferably, the graphite powder is expandable graphite with a diameter of 50-500 μm.

[0017] Preferably, the pore-forming agent is any one of potassium permanganate, potassium persulfate and potassium dichromate.

[0018] Preferably, the coagulation agent is any one of polyacrylic acid, polymethacrylic acid and polystyrene sulfonic acid.

[0019] Preferably, the washing is performed alternately using dilute hydrochloric acid and deionized water, and the volume fraction of the dilute hydrochloric acid is 10%.

[0020] Preferably, the drying temperature is 40-80° C. and the drying time is 24-48 hours.

[0021] Preferably, the temperature of the high-temperature reduction is 600-1200°C.

[0022] Preferably, in step S1, the weight ratio of the porous graphene to the aluminum ingot is 1:1-2.

[0023] Preferably, the ball-to-material ratio of the low-energy ball milling in step S2 is 8:1, the ball milling speed is 200-250 rpm, and the ball milling time is 1-2 h.

[0024] Preferably, the working parameters of the atomization method are: the gas flow is high-pressure argon gas, the pressure is 8MPa-10MPa, and the speed is 300-700 m / s.

[0025] Preferably, the particle size of the nitrogen-doped graphene powder in step S3 is 0.5-5 μm, and the nitrogen doping amount is 3 wt %.

[0026] Preferably, the aluminum alloy ingot in step S3 is any one of AlSi10Mg, AlSi7Mg, and AlSi12.

[0027] Preferably, in step S4, the weight ratio of the aluminum alloy ingot to the aluminum-porous graphene powder and the nitrogen-doped graphene powder is 94-98:1-4:1-2.

[0028] Preferably, the guide tube is made of zirconium oxide and has an inner diameter of 4 mm-6 mm.

[0029] Preferably, the drying in step S5 is performed under a vacuum environment, the drying temperature is 105-115° C., and the drying time is 10-12 h.

[0030] Preferably, the particle size of the metal composite powder used for additive manufacturing in step S5 is 15-53 μm.

[0031] Furthermore, the present invention also provides a metal composite powder for additive manufacturing, and the metal composite powder for additive manufacturing is prepared by the above-mentioned preparation steps.

[0032] Beneficial effects of the present invention:

[0033] The metal composite powder for additive manufacturing of the present invention is prepared by adding N-doped graphene to an aluminum alloy matrix melt and introducing the N element, thereby improving the fluidity of the powder and the density and mechanical properties of the printed part.

[0034] The metal composite powder for additive manufacturing of the present invention adds aluminum-porous graphene composite powder to aluminum alloy matrix melt, thereby improving the compatibility of graphene with the matrix and enhancing the density of the printed part.

[0035] The metal composite powder for additive manufacturing of the present invention further improves the mechanical properties of additively manufactured printed parts by forming a ceramic reinforcement phase under high temperature conditions, and has a significant impact on the field of aluminum alloy powder for additive manufacturing. DETAILED DESCRIPTION

[0036] The sources or properties of the raw materials used in the examples and comparative examples of the present invention are as follows:

[0037] Graphite powder was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., with the catalog number E477901;

[0038] Nitrogen-doped graphene powder was purchased from Shanghai Jingkang Biological Co., Ltd. with the product number JK-R0802.

[0039] Example 1: A metal composite powder for additive manufacturing, the specific preparation steps are as follows:

[0040] (1) In an ice-water bath, 10 g of expandable graphite powder with a diameter of 50 μm, 300 g of concentrated sulfuric acid, and 50 g of potassium permanganate were mixed evenly, reacted in an ice-water bath for 2 h, then heated to 35 ° C, continued to react for 10 h, slowly added 1.5 L of deionized water, then heated to 50 ° C, added 30 g of potassium persulfate, continued to react for 2 h, and finally added 50 g of hydrogen peroxide to obtain a mixed solution; then 1 g of polyacrylic acid was added to the mixed solution, filtered, and washed alternately with 10% by volume dilute hydrochloric acid and deionized water until the pH of the filtrate was 7, dried at 40 ° C for 24 h, and reduced at 600 ° C to obtain porous graphene;

[0041] (2) In an argon atmosphere, 5 g of an aluminum ingot was heated and melted into aluminum liquid at a temperature of 730 °C, and then 5 g of porous graphene was added to the aluminum liquid and stirred evenly to obtain a composite melt;

[0042] (3) The composite melt was discharged through the zirconia flow guide tube, and was broken into fine droplets by gas atomization in an argon atmosphere. After solidification, low-energy ball milling was performed with a ball-to-material ratio of 8:1, a ball milling speed of 200 rpm, and a ball milling time of 1 h to obtain aluminum-porous graphene composite powder; wherein the pressure of the gas atomization method was 8 MPa and the speed was 300 m / s;

[0043] (4) Under an argon atmosphere, 94 g of AlSi10Mg alloy ingot was melted at 900 °C to form an aluminum alloy liquid, and then 1 g of aluminum-porous graphene composite powder and 1 g of nitrogen-doped graphene powder with a particle size of 0.5 μm were added and stirred evenly to obtain a composite alloy melt;

[0044] (5) The composite alloy melt is discharged through the zirconia flow guide tube, and is broken into fine droplets by a gas atomization method under an argon atmosphere, and spherical aluminum alloy powder is obtained after solidification; wherein the pressure of the gas atomization method is 8 MPa and the speed is 300 m / s;

[0045] (6) Under an argon atmosphere, the spherical aluminum alloy powder was sieved and dried under vacuum at 105 °C for 10 h to obtain a metal composite powder for additive manufacturing with a particle size of 15-53 μm.

[0046] Example 2: A metal composite powder for additive manufacturing, the specific preparation steps are as follows:

[0047] (1) In an ice-water bath, 10 g of expandable graphite powder with a diameter of 350 μm, 730 g of concentrated sulfuric acid, and 80 g of potassium permanganate were mixed evenly, reacted in an ice-water bath for 15 h, then heated to 35 °C, continued to react for 35 h, slowly added 2 L of deionized water, then heated to 65 °C, added 50 g of potassium persulfate, continued to react for 5 h, and finally added 130 g of hydrogen peroxide to obtain a mixed solution; then 3 g of polyacrylic acid was added to the mixed solution, filtered, and washed alternately with 10% by volume dilute hydrochloric acid and deionized water until the pH of the filtrate was 7, dried at 60 °C for 36 h, and reduced at 900 °C to obtain porous graphene;

[0048] (2) In an argon atmosphere, 8 g of aluminum ingot was heated and melted into aluminum liquid at a temperature of 760 °C, and then 5 g of porous graphene was added to the aluminum liquid and stirred evenly to obtain a composite melt;

[0049] (3) The composite melt was discharged through the zirconia flow guide tube, and was broken into fine droplets by gas atomization in an argon atmosphere. After solidification, low-energy ball milling was performed with a ball-to-material ratio of 8:1, a ball milling speed of 230 rpm, and a ball milling time of 1 h to obtain aluminum-porous graphene composite powder; wherein the pressure of the gas atomization method was 9 MPa and the speed was 500 m / s;

[0050] (4) Under an argon atmosphere, 96 g of AlSi10Mg alloy ingot was melted at 950 °C to form an aluminum alloy liquid, and then 2.5 g of aluminum-porous graphene composite powder and 1.5 g of nitrogen-doped graphene powder with a particle size of 3 μm were added and stirred evenly to obtain a composite alloy melt;

[0051] (5) The composite alloy melt is discharged through the zirconia flow guide tube, and is broken into fine droplets by a gas atomization method under an argon atmosphere, and spherical aluminum alloy powder is obtained after solidification; wherein the pressure of the gas atomization method is 9 MPa and the speed is 500 m / s;

[0052] (6) Under an argon atmosphere, the spherical aluminum alloy powder was sieved and dried under vacuum at a temperature of 110 °C for 11 h to obtain a metal composite powder for additive manufacturing with a particle size of 15-53 μm.

[0053] Example 3: A metal composite powder for additive manufacturing, the specific preparation steps are as follows:

[0054] (1) In an ice-water bath, 10 g of expandable graphite powder with a diameter of 500 μm, 1000 g of concentrated sulfuric acid, and 100 g of potassium permanganate were mixed evenly, reacted in an ice-water bath for 24 h, then heated to 35 ° C, continued to react for 60 h, slowly added 2 L of deionized water, then heated to 80 ° C, added 70 g of potassium persulfate, continued to react for 8 h, and finally added 200 g of hydrogen peroxide to obtain a mixed solution; then 5 g of polyacrylic acid was added to the mixed solution, filtered, and washed alternately with 10% by volume dilute hydrochloric acid and deionized water until the pH of the filtrate was 7, dried at 80 ° C for 48 h, and reduced at 1200 ° C to obtain porous graphene;

[0055] (2) In an argon atmosphere, 10 g of an aluminum ingot was heated and melted into aluminum liquid at a temperature of 780 °C, and then 5 g of porous graphene was added to the aluminum liquid and stirred evenly to obtain a composite melt;

[0056] (3) The composite melt was discharged through the zirconia flow guide tube, and was broken into fine droplets by gas atomization in an argon atmosphere. After solidification, low-energy ball milling was performed with a ball-to-material ratio of 8:1, a ball milling speed of 250 rpm, and a ball milling time of 2 h to obtain aluminum-porous graphene composite powder; wherein the pressure of the gas atomization method was 10 MPa and the speed was 700 m / s;

[0057] (4) Under an argon atmosphere, 98 g of AlSi10Mg alloy ingot was melted at 1000 °C to form an aluminum alloy liquid, and then 1 g of aluminum-porous graphene composite powder and 1 g of nitrogen-doped graphene powder with a particle size of 5 μm were added and stirred evenly to obtain a composite alloy melt;

[0058] (5) The composite alloy melt is discharged through the zirconia flow guide tube, and is broken into fine droplets by a gas atomization method under an argon atmosphere, and spherical aluminum alloy powder is obtained after solidification; wherein the pressure of the gas atomization method is 10 MPa and the speed is 700 m / s;

[0059] (6) Under an argon atmosphere, the spherical aluminum alloy powder was sieved and dried under vacuum at a temperature of 115 °C for 12 h to obtain a metal composite powder for additive manufacturing with a particle size of 15-53 μm.

[0060] Comparative Example 1: A metal composite powder, the specific preparation steps are as follows:

[0061] (1) In an ice-water bath, 10 g of expandable graphite powder with a diameter of 350 μm, 730 g of concentrated sulfuric acid, and 80 g of potassium permanganate were mixed evenly, reacted in an ice-water bath for 15 h, then heated to 35 °C, continued to react for 35 h, slowly added 2 L of deionized water, then heated to 65 °C, added 50 g of potassium persulfate, continued to react for 5 h, and finally added 130 g of hydrogen peroxide to obtain a mixed solution; then 3 g of polyacrylic acid was added to the mixed solution, filtered, and washed alternately with 10% by volume dilute hydrochloric acid and deionized water until the pH of the filtrate was 7, dried at 60 °C for 36 h, and reduced at 900 °C to obtain porous graphene;

[0062] (2) In an argon atmosphere, 8 g of aluminum ingot was heated and melted into aluminum liquid at a temperature of 760 °C, and then 5 g of porous graphene was added to the aluminum liquid and stirred evenly to obtain a composite melt;

[0063] (3) The composite melt was discharged through the zirconia flow guide tube, and was broken into fine droplets by gas atomization in an argon atmosphere. After solidification, low-energy ball milling was performed with a ball-to-material ratio of 8:1, a ball milling speed of 230 rpm, and a ball milling time of 1 h to obtain aluminum-porous graphene composite powder; wherein the pressure of the gas atomization method was 9 MPa and the speed was 500 m / s;

[0064] (4) Under an argon atmosphere, 96 g of AlSi10Mg alloy ingot was melted at 950 °C to form an aluminum alloy liquid, and then 2.5 g of aluminum-porous graphene composite powder and 1.5 g of graphene powder with a particle size of 3 μm were added and stirred evenly to obtain a composite alloy melt;

[0065] (5) The composite alloy melt is discharged through the zirconia flow guide tube, and is broken into fine droplets by a gas atomization method under an argon atmosphere, and spherical aluminum alloy powder is obtained after solidification; wherein the pressure of the gas atomization method is 9 MPa and the speed is 500 m / s;

[0066] (6) Under an argon atmosphere, the spherical aluminum alloy powder was sieved and dried under vacuum at a temperature of 110 °C for 11 h to obtain a metal composite powder for additive manufacturing with a particle size of 15-53 μm.

[0067] Comparative Example 2: A metal composite powder, the specific preparation steps are as follows:

[0068] (1) In an ice-water bath, 10 g of expandable graphite powder with a diameter of 350 μm, 730 g of concentrated sulfuric acid, and 80 g of potassium permanganate were mixed evenly, reacted in an ice-water bath for 15 h, then heated to 35 °C, continued to react for 35 h, slowly added 2 L of deionized water, then heated to 65 °C, added 50 g of potassium persulfate, continued to react for 5 h, and finally added 130 g of hydrogen peroxide to obtain a mixed solution; then 3 g of polyacrylic acid was added to the mixed solution, filtered, and washed alternately with 10% by volume dilute hydrochloric acid and deionized water until the pH of the filtrate was 7, dried at 60 °C for 36 h, and reduced at 900 °C to obtain porous graphene;

[0069] (2) In an argon atmosphere, 96 g of AlSi10Mg alloy ingot was melted at 950 °C to form an aluminum alloy liquid, and then 2.5 g of porous graphene powder and 1.5 g of nitrogen-doped graphene powder with a particle size of 3 μm were added and stirred evenly to obtain a composite alloy melt;

[0070] (3) The composite alloy melt is discharged through the zirconia flow guide tube, and is broken into fine droplets by gas atomization in an argon atmosphere, and spherical aluminum alloy powder is obtained after solidification; wherein the pressure of the gas atomization method is 9 MPa and the speed is 500 m / s;

[0071] (4) Under an argon atmosphere, the spherical aluminum alloy powder was sieved and dried under vacuum at a temperature of 110°C for 11 h to obtain a metal composite powder for additive manufacturing with a particle size of 15-53 μm.

[0072] Comparative Example 3: A metal composite powder, the specific preparation steps are as follows:

[0073] (1) In an argon atmosphere, 8 g of aluminum ingot was heated and melted into aluminum liquid at a temperature of 760 °C, and then 5 g of graphene was added to the aluminum liquid and stirred evenly to obtain a composite melt;

[0074] (2) The composite melt was discharged through the zirconia flow guide tube, and was broken into fine droplets by gas atomization in an argon atmosphere. After solidification, low-energy ball milling was performed with a ball-to-material ratio of 8:1, a ball milling speed of 230 rpm, and a ball milling time of 1 h to obtain aluminum-graphene composite powder; wherein the pressure of the gas atomization method was 9 MPa and the speed was 500 m / s;

[0075] (3) Under an argon atmosphere, 96 g of AlSi10Mg alloy ingot was melted at 950 °C to form an aluminum alloy liquid, and then 2.5 g of aluminum-graphene composite powder and 1.5 g of nitrogen-doped graphene powder with a particle size of 3 μm were added and stirred evenly to obtain a composite alloy melt;

[0076] (4) The composite alloy melt is discharged through the zirconia flow guide tube, and is broken into fine droplets by a gas atomization method under an argon atmosphere, and spherical aluminum alloy powder is obtained after solidification; wherein the pressure of the gas atomization method is 9 MPa and the speed is 500 m / s;

[0077] (5) Under an argon atmosphere, the spherical aluminum alloy powder was sieved and dried under vacuum at a temperature of 110°C for 11 h to obtain a metal composite powder for additive manufacturing with a particle size of 15-53 μm.

[0078] Performance Testing

[0079] Fluidity: The powder fluidity test of the embodiment and the comparative example was carried out according to the "GB / T 1482-2010 Metal Powder Fluidity Determination Standard Funnel Method (Hall Rheometer)", and the test results are shown in Table 1

[0080] The sample powders obtained in the embodiment and the comparative example were subjected to SLM printing using an additive manufacturing device under the following parameters: the preheating temperature of the printer plate was 100-190°C, the laser power was 260-270W, the scanning speed was 1000-1200mm / s, the scanning spacing was 0.1-0.15mm, the scanning layer thickness was 0.03-0.06mm, and the area overlap was 0.15mm; the powder printed parts were annealed to obtain powder molded parts; the annealing treatment included: heating the powder molded parts to 300-350°C in a vacuum environment, keeping the temperature for 4-6h, and finally cooling them to room temperature in air to finally obtain powder printed parts, and the powder printed parts were subjected to performance tests:

[0081] Density: The obtained powder print was cleaned with anhydrous ethanol to remove the oil and impurities on the surface, and the true density (d e ), and calculate the theoretical density of the composite material (d t ), the density D calculation formula is as follows:

[0082] ;

[0083] According to the national standard GB / T228.1-2010 “Tensile test of metallic materials Part 1 Room temperature test method”, the mechanical properties of the powder printed parts were tested, including yield strength and tensile strength. The test results are shown in Table 1.

[0084]

[0085] Data analysis: It can be seen from Examples 1-3 that the metal composite powder for additive manufacturing of the present invention has good fluidity and high sphericity, and the densification degree and mechanical properties of the printed parts obtained by 3D printing of the powder are relatively excellent, among which the density can reach 99.79%, the tensile strength can reach 547MPa, and the yield strength can reach 378MPa, which can meet the requirements of traditional additive manufacturing for aluminum alloy powder.

[0086] It can be seen from Example 2 and Comparative Examples 1-3 that the metal composite powder for additive manufacturing of the present invention, by adding nitrogen-doped graphene powder and aluminum-porous graphene composite powder to aluminum alloy melt, makes the performance of the obtained powder after printing is relatively excellent. The reason may be that the aluminum liquid is filled into the porous graphene, which on the one hand avoids the problem of poor interface compatibility between graphene and the aluminum alloy matrix, and at the same time, the aluminum liquid filling will also improve the density; N-doped graphene solves the problem of easy agglomeration of graphene itself, and at the same time, the doped N element provides more active sites on the graphene surface. Under high temperature conditions, it can generate a ceramic reinforcement phase in situ with aluminum filled with porous graphene, which is beneficial to the improvement of the interface compatibility between graphene and the aluminum alloy matrix, so that the density and mechanical properties of the printed parts are further improved.

[0087] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

Claims

1. A method for preparing a metal composite powder for additive manufacturing, It is characterized in that The following steps are involved: S1: In an argon atmosphere, an aluminum ingot is heated and melted into aluminum liquid at a temperature of 730°C-780°C, and then porous graphene is added to the aluminum liquid and stirred evenly to obtain a composite melt; S2: The composite melt is discharged through a flow guide tube, broken into fine droplets by gas atomization, and low-energy ball milling is performed after solidification to obtain aluminum-porous graphene composite powder; S3: Under an argon atmosphere, the aluminum alloy ingot is melted at 900° C.-1000° C. to form an aluminum alloy liquid, and then the aluminum-porous graphene composite powder and the nitrogen-doped graphene powder are added and stirred to obtain a composite alloy melt; S4: The composite alloy melt is discharged through a flow guide tube, and is broken into fine droplets by a gas atomization method, and spherical aluminum alloy powder is obtained after solidification; S5: Under an argon atmosphere, the spherical aluminum alloy powder is screened and dried to obtain a metal composite powder for additive manufacturing; The preparation steps of the porous graphene in step S1 are as follows: In an ice water bath, graphite powder, concentrated sulfuric acid and potassium permanganate are mixed and reacted for 2-24 hours, then reacted at 35°C for 10-60 hours, then heated to 50-80°C, a pore-forming agent is added, and the reaction is continued for 2-8 hours. Finally, hydrogen peroxide is added to obtain a mixed solution; then a coagulant is added to the mixed solution, filtered, washed to make the pH of the filtrate 7, dried, and reduced at high temperature to obtain porous graphene.

2. The method for preparing the metal composite powder for additive manufacturing according to claim 1, It is characterized in that The weight ratio of the graphite powder, concentrated sulfuric acid, potassium permanganate, pore-forming agent, hydrogen peroxide and coagulation agent is 1:30-100:5-10:3-7:5-20:0.1-0.

5.

3. The method for preparing the metal composite powder for additive manufacturing according to claim 1, It is characterized in that The graphite powder is expandable graphite with a diameter of 50-500 μm.

4. The method for preparing metal composite powder for additive manufacturing according to claim 1, It is characterized in that The weight ratio of the porous graphene to the aluminum ingot in step S1 is 1:1-2.

5. The method for preparing metal composite powder for additive manufacturing according to claim 1, It is characterized in that The ball-to-material ratio of the low-energy ball milling in step S2 is 8:1, the ball milling speed is 200-250 rpm, and the ball milling time is 1-2 h.

6. The method for preparing metal composite powder for additive manufacturing according to claim 1, It is characterized in that The particle size of the nitrogen-doped graphene powder in step S3 is 0.5-5 μm, and the nitrogen doping amount is 3 wt %.

7. The method for preparing metal composite powder for additive manufacturing according to claim 1, It is characterized in that The aluminum alloy ingot in step S3 is one of AlSi10Mg, AlSi7Mg, and AlSi12.

8. The method for preparing metal composite powder for additive manufacturing according to claim 1, It is characterized in that The weight ratio of the aluminum alloy ingot to the aluminum-porous graphene composite powder and the nitrogen-doped graphene powder in step S4 is 94-98:1-4:1-2.

9. A metal composite powder for additive manufacturing, It is characterized in that The method for preparing the metal composite powder for additive manufacturing according to any one of claims 1 to 8 is used.

Citation Information

Patent Citations

  • Rare earth aluminum alloy powder suitable for additive manufacturing and preparation method of rare earth aluminum alloy powder

    CN112831694A

  • Aluminum alloy powder and preparation method thereof

    CN114293049A

  • The Method for improving elastic modulus of particle reinforced aluminum-based composite material

    AU2020101927A4

  • Nanocarbon-reinforced aluminium composite materials and method for manufacturing the same

    CN104975201A

  • Preparation method for composite aluminium alloy material

    CN106756176A