A kind of transparent microcrystalline glass and preparation method thereof

By optimizing the component ratio and process flow of microcrystalline glass, the problems of complex preparation, high cost and difficult to take into account in the existing technology were solved, and high transparency and high hardness microcrystalline glass suitable for mobile terminal display field were successfully prepared. Excellent optical and mechanical properties are achieved.

CN118637832BActive Publication Date: 2024-11-15SICHUAN GLOBAL MICROCRYSTAL GLASS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411106082.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-15
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

The existing microcrystalline glass preparation process is complex, the cost is high, and it is difficult to mass-produce on a large scale, and it is difficult to take into account both optical and mechanical properties. Especially in the increasing demand in areas such as mobile terminal covers, existing materials cannot meet the high transparency, High toughness and high hardness requirements.

Method used

By optimizing the component design, including proportional control of components such as SiO2, Al2O3, Li2O, ZrO2, P2O5, CeO2, GeO2 and other components, alkali metal oxides such as Cs2O, Na2O, K2O are introduced, and presintering, melting, clarification, annealing and The segmented precision heat treatment process produces transparent microcrystalline glass with excellent optical and mechanical properties.

Benefits of technology

Achieve high transmittance and high hardness microcrystalline glass, suitable for display fields, especially mobile phone panels and other applications, has good optical and mechanical properties, and through fine regulation of crystallization dynamics and chemical stability, the glass is improved overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118637832B_ABST
    Figure CN118637832B_ABST
Patent Text Reader

Abstract

The present invention discloses a transparent microcrystalline glass and a preparation method thereof, belonging to the technical field of microcrystalline glass. The microcrystalline glass mainly contains, by weight percentage, SiO2: 65-80%, Al2O3: 5-10%, Li2O: 5-15%, ZrO2: 1-8%, and P2O5: 1-6%. In particular, by additionally introducing tetravalent oxides such as CeO2 and GeO2 and alkali metal oxides such as Cs2O, and by adjusting the ratio of the composite nucleating agent ZrO2 / P2O5 and the ratio of the glass network former to control the crystallization kinetics process, the type and size of the precipitated crystals are controlled, and microcrystalline glass with petalite, lithium disilicate, β-quartz, etc. as the main crystal phases and a crystal scale within 100nm is obtained. The microcrystalline glass has high visible transmittance and hardness, which meets the performance requirements of the panel in the display field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of microcrystalline glass, and in particular, relates to a transparent microcrystalline glass and a preparation method thereof. Background Art

[0002] In recent years, with the rapid development of the consumer electronics industry, people have put forward higher requirements for glass materials used in electronic devices / display devices. In particular, the requirements for the drop resistance, scratch resistance, and impact resistance of cover glass for mobile terminals are getting higher and higher.

[0003] As a special glass material that combines structural and functional properties, microcrystalline glass can obtain excellent properties such as high transparency, high toughness, and high hardness through reasonable component design and special preparation process. It has become a new type of display cover and backplane material with great potential and is the development trend of the future market.

[0004] However, at present, most panel glass materials on the market are still dominated by high-aluminum glass. This is mainly because the preparation process of microcrystalline glass is more complicated than that of high-aluminum glass, and it is difficult to mass-produce high-performance microcrystalline glass on a large scale, and the cost is high. Microcrystalline glass is composed of two phases, glass phase and crystal phase. The refractive index difference between the crystal phase and the glass phase is the main factor affecting the optical properties of microcrystalline glass. To obtain microcrystalline glass with high transmittance in the visible band, the refractive index of the glass phase and the precipitated crystal phase must match. Therefore, it is necessary to reasonably and finely design and optimize the components to finely control the type of crystalline phase, grain size and crystallinity. For example, some additives in the components, such as nucleating agents and glass network exosomes (modifiers), are selected and optimized. These additives often directly affect the uniformity and crystallization dynamics of microcrystalline glass, and thus affect the optical and mechanical properties of microcrystalline glass. Summary of the invention

[0005] The object of the present invention is to provide a transparent microcrystalline glass having excellent optical and mechanical properties and applied in the display field and a preparation method thereof.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A transparent microcrystalline glass, comprising the following components by weight percentage:

[0008] SiO2: 65~80%

[0009] Al2O3: 5~10%

[0010] Li2O: 5~15%

[0011] ZrO2: 1~8%

[0012] P2O5: 1~6%

[0013] Also includes CeO2 and / or GeO2;

[0014] Among them, the ratio of ZrO2 / P2O5: 1.5~3;

[0015] Ratio of (SiO2+Al2O3) / (ZrO2+P2O5): 7.5~17;

[0016] Ratio of (Li2O+Cs2O+Na2O+K2O) / (ZrO2+P2O5): 1~3;

[0017] CeO2: 0~0.5%, GeO2: 0~1% and GeO2+CeO2: 0~1%.

[0018] Furthermore, Cs2O and / or Na2O and / or K2O are introduced into the glass-ceramics components, Cs2O: 0~1%, Na2O: 0~3%, K2O: 0~1%, Na2O+K2O+Cs2O: 0~3%.

[0019] Furthermore, in terms of weight percentage, it may also selectively contain MgO: 0-5%, ZnO: 0-5%, Y2O3: 0-2%, La2O3: 0-2%, Gd2O3: 0-2%. Preferably, MgO: 0-3%, ZnO: 0-2%, Y2O3: 0-1%, La2O3: 0-1%, Gd2O3: 0-1%. More preferably, MgO: 0-2%, ZnO: 0-1%, Y2O3: 0-0.5%, La2O3: 0-0.5%, Gd2O3: 0-0.5%.

[0020] It also contains clarifiers Sb2O3: 0.1~1.0%, and / or NaNO3: 0.1~1.0%, and / or NaSbO3: 0.1~1.0%, and / or Na2SO4: 0.1~1.0%, and / or SnO2: 0.1~1.0%.

[0021] SiO2 and Al2O3 are the network formers of matrix glass, and are the main components of crystals such as petalite and lithium disilicate separated out by heat treatment.SiO2 content is lower than 60%, and the chemical stability of glass can deteriorate, but if its content is too high, it can cause the melting temperature to improve, and the glass viscosity increases, which is unfavorable for bubble removal, clarification and homogenization, and has increased the melting difficulty of glass, so SiO2 content should not exceed 80% at the highest.Al2O3 helps to improve glass structure and chemical stability, and reasonably introduces Al2O3 content that can control the speed of crystallization and the size of separated out crystal grains, thereby improving the transmittance and the hardness of microcrystalline glass.

[0022] Li2O is introduced into glass as the main alkali metal oxide, which can not only reduce the melting temperature of glass, but also is an indispensable component for the formation of crystals such as petalite and lithium disilicate, and is an important component for chemical strengthening. Therefore, the Li2O content cannot be less than 5%. However, if the Li2O content is too high, its corrosiveness to refractory bricks will increase. In addition, the chemical stability of high-Li glass will decrease, and high-concentration Li will cause the glass to be extremely easy to crystallize, making it difficult to obtain the target crystal phase.

[0023] Na2O, K2O and Cs2O alkali metal oxides are optional components in the present invention as network exosomes in the glass, and are mainly used for glass modification. The introduction of these alkali metal oxides can reduce the melting temperature and glass transition temperature of the glass. At the same time, the introduction of these alkali metal oxides will affect the crystallization kinetics of the glass, thereby regulating the crystal phase of the crystallization.

[0024] ZrO2 and P2O5 are necessary components in the present invention and are both used as nucleating agents. The combination of the two in a suitable ratio can achieve uniform crystallization of glass, refine the grain size of crystallization, and improve the transmittance of microcrystalline glass. In addition, ZrO2 also helps to improve the chemical stability and hardness of glass.

[0025] CeO2 and GeO2 are optional components in the present invention as network exosomes in glass, and are mainly used to regulate the crystallization process of glass, while increasing the refractive index of the glass body, so that the refractive index of the precipitated crystals is more matched with the residual glass, thereby improving the transmittance of the glass. In addition, the introduction of CeO2 can increase the hardness of the glass, and can also be used as a clarifier to improve the quality of glass melting. However, the amount of CeO2 introduced should not exceed 2%, preferably, should not exceed 1%, and more preferably, should not exceed 0.5%. Too high will cause glass coloring. The introduction of CeO2 in the present invention will not cause a significant decrease in the transmittance of the glass material in the visible light band.

[0026] MgO and ZnO are optional components in the present invention, which can improve the material properties of the glass and participate in the crystallization process to form Zn 0.5 AlSi2O6 or Mg 0.5 AlSi2O6.

[0027] Ln2O3 is a rare earth oxide, which is an optional component in the present invention. It is one or more of Y2O3, La2O3, and Gd2O3, and is mainly used to regulate the crystallization process of glass and the refractive index of the glass itself.

[0028] Sb2O3, NaNO3, NaSbO3, Na2SO4, SnO2 are used as clarifiers, and one or more of them can be selected.

[0029] The method for preparing the above-mentioned glass-ceramics comprises the following steps:

[0030] (1) Weigh the raw materials according to the proportion, grind and mix them thoroughly, and then put them into a platinum crucible;

[0031] (2) placing the platinum crucible containing the mixed raw materials into a furnace at 1550-1650°C for pre-sintering, and then grinding the pre-sintered glass clinker to obtain uniform glass powder;

[0032] (3) The glass powder is melted, stirred, clarified, and other operations are performed in a platinum crucible;

[0033] (4) After clarification, the glass is cast into a preheated mold;

[0034] (5) The formed glass is quickly transferred to an annealing furnace and heated to a temperature of 100 °C at the glass transition temperature (T g ) and then cool down naturally after annealing.

[0035] (6) The glass is subjected to segmented precision heat treatment to ultimately obtain glass-ceramics.

[0036] Furthermore, in step (3), the glass powder is melted at 1550-1650°C for 2-5 hours, during which time it is stirred 2-3 times using a platinum stirring rod, each stirring lasting about 30 minutes, and the clarification process is carried out at 1550-1600°C for 0.5-2 hours.

[0037] Furthermore, the stepwise precision heat treatment process in step (6) is as follows: the nucleation temperature of the base glass heat treatment is controlled to be higher than the glass transition temperature (T g ) between 50℃ and 100℃, the nucleation time is 1~6h, and the crystallization temperature is controlled at the crystallization starting temperature (T x ), the crystallization time is 0.5~1h; such segmented operation can improve the comprehensive performance of the glass.

[0038] In the above preparation method, the microcrystalline glass is subjected to a pre-sintering process, a grinding process, and then melted again to improve the uniformity of glass melting.

[0039] The crystals precipitated by the above preparation method mainly include one or more crystal phases such as petalite, lithium disilicate, β-quartz, etc., with a crystallinity of more than 60% and a grain size of less than 100nm.

[0040] The obtained microcrystalline glass has a transmittance of 90% or more in the 550nm band when the thickness is 0.7mm, and a Vickers hardness of 720kgf / mm 2 .

[0041] The obtained microcrystalline glass can be applied to display fields such as mobile phone panels.

[0042] Beneficial effects of the present invention:

[0043] (1) The kinetics of glass crystallization can be finely controlled by controlling the ratio of the composite nucleating agents ZrO2 / P2O5, the ratio of the glass network formers SiO2 and Al2O3 SiO2 / Al2O3, and the ratio of the sum of SiO2 and Al2O3 to the nucleating agents (SiO2+Al2O3) / (ZrO2+P2O5).

[0044] (2) By introducing additional alkali metal oxides other than Li2O, including Cs2O, Na2O and K2O, the ratio of alkali metal oxides to nucleating agents (Li2O+Cs2O+Na2O+K2O) / (ZrO2+P2O5) is adjusted to control the number of non-bridging oxygen bonds in the glass, thereby regulating the crystallization kinetics, chemical stability, hardness and other properties of the glass.

[0045] (3) The additional introduction of tetravalent oxides such as CeO2 and GeO2 can improve the chemical stability and hardness of the glass, regulate the crystallization process of the glass, and increase the refractive index of the glass itself, so that the refractive index of the precipitated crystals is more matched with the residual glass, thereby improving the transmittance of the glass. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] The present invention will be further described below in conjunction with the accompanying drawings.

[0047] Figure 1 is the XRD pattern of the glass-ceramics of Example 13;

[0048] Figure 2 This is the SEM spectrum of the glass-ceramics of Example 13;

[0049] Figure 3 This is the transmittance spectrum of the microcrystalline glass of Example 13. DETAILED DESCRIPTION

[0050] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0051] The preparation method of microcrystalline glass includes the following specific steps:

[0052] (1) Quartz sand, aluminum oxide, lithium oxide, zirconium oxide, phosphorus pentoxide, sodium oxide, cerium oxide and other additives are weighed according to the ratio, ground and mixed thoroughly, and then placed in a platinum crucible.

[0053] (2) The platinum crucible containing the mixed raw materials is placed in a furnace at 1550~1650℃ for pre-sintering, and then the pre-sintered glass clinker is ground to obtain uniform glass powder.

[0054] (3) The glass powder is melted, stirred, and clarified in a platinum crucible. The glass is melted at 1550-1650°C for about 2-5 hours, during which it is stirred 2-3 times with a platinum stirring rod, each stirring lasting about 30 minutes. The clarification process is carried out at 1550-1600°C and lasts for about 0.5-2 hours.

[0055] (4) After clarification, the glass is cast into a preheated mold.

[0056] (5) The formed glass is quickly transferred to an annealing furnace and heated to a temperature of 100 °C at the glass transition temperature (T g ) and the temperature is naturally lowered after annealing.

[0057] (6) The glass is subjected to segmented precision heat treatment, and the nucleation temperature of the basic glass heat treatment is controlled to be higher than the glass transition temperature (T g ) between 50℃ and 100℃, the nucleation time is 1~6h, and the crystallization temperature is controlled at the crystallization starting temperature (T x ), the crystallization time is 0.5~1h, and finally microcrystalline glass is obtained.

[0058] The present invention is described in detail below through specific examples. The raw materials, component ratios and performance indicators of the finished glass products used in the following examples are shown in the following table:

[0059] Component / weight percentage (%) Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Example 8 <![CDATA[SiO2]]> 68.2 71.5 69.4 71.7 70.5 71.5 71.5 69.5 <![CDATA[Al2O3]]> 7.9 8.5 8 8 8 8 8.5 8 <![CDATA[Li2O]]> 11 7.3 10.4 10.4 10.3 10.3 10.3 10.3 <![CDATA[ZrO2]]> 4.5 4.5 4.5 4.5 6 5 5 5.5 <![CDATA[P2O5]]> 2 2 2 2 3 2 1.5 3.5 <![CDATA[Na2O]]> 4.5 3.8 3.3 2 2 2 2 2 <![CDATA[Cs2O]]> 1 0.7 0.5 0.5 0.5 0.5 0.5 0.5 <![CDATA[K2O]]> 0 0.8 1 0 0 0 0 0 <![CDATA[CeO2]]> 0.2 0.2 0.2 0.2 0.2 0.2 0.2 0.2 <![CDATA[GeO2]]> 0 0 0 0 0 0 0 0 MgO 0.1 0.1 0.1 0.1 0 0 0 0 ZnO 0.1 0.1 0.1 0.1 0 0 0 0 <![CDATA[Y2O3]]> 0 0 0 0 0 0 0 0 <![CDATA[La2O3]]> 0 0 0 0 0 0 0 0 <![CDATA[Gd2O3]]> 0 0 0 0 0 0 0 0 <![CDATA[Sb2O3+NaNO3+NaSbO3+Na2SO4+SnO2]]> 0.5 0.5 0.5 0.5 0.5 0.5 0.5 0.5 <![CDATA[ZrO2 / P2O5]]> 2.25 2.25 2.25 2.25 2 2.5 3.33 1.57 <![CDATA[SiO2 / Al2O3]]> 8.63 8.41 8.68 8.96 8.81 8.94 8.41 8.69 <![CDATA[(SiO2+Al2O3) / (ZrO2+P2O5)]]> 11.71 12.31 11.91 12.26 8.72 11.36 12.31 8.61 <![CDATA[(Li2O+Na2O+K2O+Cs2O) / (ZrO2+P2O5)]]> 2.54 1.94 2.34 1.98 1.42 1.83 1.97 1.42 <![CDATA[GeO2+CeO2]]> 0.2 0.2 0.2 0.2 0.2 0.2 0.2 0.2 Precipitation crystal size (nm) <100 <100 <80 <50 <50 <50 <100 <100 Crystal phase Petalite, lithium disilicate Petalite, lithium disilicate Petalite, lithium disilicate Petalite, lithium disilicate Petalite, lithium disilicate Petalite, lithium disilicate, β-quartz Petalite, lithium disilicate Petalite, lithium disilicate, β-quartz Transmittance at 550nm with a thickness of 0.7mm (%) 81 83 85 89 90 91 83 80 <![CDATA[Vickers hardness (kgf / mm 2 )]]> 689 684 682 702 706 709 703 711

[0060] Component / weight percentage (%) Example 9 Example 10 Embodiment 11 Example 12 Example 13 Embodiment 14 Embodiment 15 Example 16 <![CDATA[SiO2]]> 71 70.5 70.6 70.5 71.7 74.5 75 69.9 <![CDATA[Al2O3]]> 8 9 9 9 9 5.5 7 12 <![CDATA[Li2O]]> 10.3 10.3 10.5 10.3 11 10.3 9.7 10.3 <![CDATA[ZrO2]]> 4 4.5 4.5 4.5 4.5 5.5 4.5 4 <![CDATA[P2O5]]> 3.5 2 2 2 2 2 1 2 <![CDATA[Na2O]]> 2 1.5 1.5 1.5 0.5 0 0.5 0.5 <![CDATA[Cs2O]]> 0.5 0.5 0.5 0.5 0.5 0.5 0.5 0.5 <![CDATA[K2O]]> 0 0 0 0 0 0 0 0 <![CDATA[CeO2]]> 0.2 0.2 0.4 0.5 0.2 0.2 0.2 0.2 <![CDATA[GeO2]]> 0 1 0.5 0.7 0 1 1 0 MgO 0 0 0 0 0 0 0 0 ZnO 0 0 0 0 0 0 0 0 <![CDATA[Y2O3]]> 0 0 0 0 0.1 0 0 0 <![CDATA[La2O3]]> 0 0 0 0 0 0 0.1 0 <![CDATA[Gd2O3]]> 0 0 0 0 0 0 0 0.1 <![CDATA[Sb2O3+NaNO3+NaSbO3+Na2SO4+SnO2]]> 0.5 0.5 0.5 0.5 0.5 0.5 0.5 0.5 <![CDATA[ZrO2 / P2O5]]> 1.14 2.25 2.25 2.25 2.25 2.75 4.5 2 <![CDATA[SiO2 / Al2O3]]> 8.88 7.83 7.84 7.83 7.97 13.55 10.71 5.83 <![CDATA[(SiO2+Al2O3) / (ZrO2+P2O5)]]> 10.53 12.23 12.25 12.23 12.42 10.67 14.91 13.65 <![CDATA[(Li2O+Na2O+K2O+Cs2O) / (ZrO2+P2O5)]]> 1.71 1.89 1.92 1.89 1.85 1.44 1.95 1.88 <![CDATA[GeO2+CeO2]]> 0.2 1.2 0.9 1.2 0.2 1.2 1.2 0.2 Precipitation crystal size (nm) <100 <60 <60 <70 <50 <80 <100 <80 Crystal phase Petalite, lithium disilicate Petalite, lithium disilicate, β-quartz Petalite, lithium disilicate Petalite, lithium disilicate Petalite, lithium disilicate, β-quartz Petalite, lithium disilicate Petalite, lithium disilicate, β-quartz Petalite, lithium disilicate Transmittance at 550nm with a thickness of 0.7mm (%) 83 89 89 86 91 87 81 85 <![CDATA[Vickers hardness (kgf / mm 2 )]]> 689 701 704 691 721 682 719 693

[0061] As can be seen from the above table data, when the ZrO2 / P2O5 ratio is relatively low and close to 1.5 or even lower than 1.5, such as Example 8 and Example 9, the higher P2O5 content causes the glass network structure to change greatly, more Si-O bonds inside the glass are interrupted, the glass crystallization temperature is reduced, and the glass shows the performance of easy crystallization, so it is difficult to finely control the crystallization process, resulting in the crystal size being larger and the size distribution range being wide. At the same time, more P2O5 will consume more Li in the glass in the initial stage of nucleation, forming Li3PO4 crystals, resulting in the precipitation of lithium disilicate and petalite in the glass being restricted, thereby further affecting the overall performance of the glass. But if ZrO2 is introduced too much, it will lead to the increase of the glass melting temperature, which is not conducive to the processes such as glass bubbling and clarification, and at the same time, more ZrO2 will also affect the crystallization dynamics. In the present invention, we find that the ZrO2 / P2O5 ratio is a more reasonable range of 1.5~3, and the crystallization process can be easily controlled, thereby obtaining a highly transparent and high hardness microcrystalline glass.

[0062] The ratio of SiO2 and Al2O3 in the glass network formers, SiO2 / Al2O3, and the ratio of the sum of SiO2 and Al2O3 to the nucleating agent (SiO2+Al2O3) / (ZrO2+P2O5) can also finely control the dynamics of glass crystallization. SiO2 / Al2O3 determines the internal network structure of the glass and the amount of non-bridging oxygen in the glass, which has a significant impact on the glass melting temperature, crystallization range, etc. When the SiO2 / Al2O3 ratio is between 5 and 10, and the (SiO2+Al2O3) / (ZrO2+P2O5) ratio is between 7.5 and 17, a transmittance of more than 80% and a hardness of more than 680 kgf / mm can be obtained. 2 Furthermore, it can be further concluded from Examples 1-16 that when the ratio of (SiO2+Al2O3) / (ZrO2+P2O5) is controlled at 10-13, generally better transmittance and hardness performance can be obtained.

[0063] In addition, by introducing a small amount of alkali metal oxides other than Li2O, including Cs2O, Na2O and K2O, and adjusting the ratio between alkali metal oxides and nucleating agents (Li2O+Cs2O+Na2O+K2O) / (ZrO2+P2O5) to 1~3, the crystallization kinetics, chemical stability, hardness and other properties of the glass can also be further regulated. More preferably, the ratio of (Li2O+Cs2O+Na2O+K2O) / (ZrO2+P2O5) should be controlled at 1.8~2. Note that the amount of Cs2O, Na2O and K2O introduced here needs to be controlled. Excessive introduction will greatly affect the thermal expansion and chemical strengthening process of the glass, resulting in the overall performance of the glass being affected. In terms of weight percentage, the content of the introduced components should be controlled at Cs2O: 0~1%, Na2O: 0~3%, K2O: 0~1%, Na2O+K2O+Cs2O: 0~3%.

[0064] In the embodiment of the present invention, tetravalent oxides such as CeO2 and GeO2 are additionally introduced to improve the chemical stability and hardness of the glass, regulate the crystallization process of the glass, and increase the refractive index of the glass body, so that the refractive index of the precipitated crystals is more matched with the residual glass, thereby achieving the beneficial effect of improving the transmittance of the glass.

[0065] In the present invention, Example 13 is a preferred component when the ratio of the above components is controlled within a reasonable range. The characterization spectrum of the microcrystalline glass of Example 13 is as follows: Figure 1-Figure 3 shown. Figure 1 The XRD spectrum obtained by using an X-ray powder diffractometer to test the glass-ceramics of Example 13. From the figure, it can be seen that the main crystalline phases of the glass-ceramics are petalite and lithium disilicate, and also contain a small amount of β-quartz. Figure 2 This is a morphology image taken under a scanning electron microscope (SEM) of the glass-ceramics of Example 13. As can be seen from the image, dense small grains are precipitated inside the glass-ceramics, and the grain size is basically within 50 nm. Figure 3 : This is the visible band transmittance spectrum of the microcrystalline glass of Example 13. At 550nm, the transmittance of the microcrystalline glass of Example 13 can reach 91%.

[0066] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A transparent microcrystalline glass, characterized in that: The following components are included by weight percentage: SiO2: 65~80% Al2O3: 5~10% Li2O: 5~15% ZrO2: 1~8% P2O5: 1~6% Also includes CeO2 and / or GeO2; Cs2O and / or Na2O and / or K2O; CeO2: 0~0.5%, GeO2: 0~1% and GeO2+CeO2: 0~1%; Cs2O: 0~1%, Na2O: 0~3%, K2O: 0~1% and Na2O+K2O+Cs2O: 0~3%; Among them, the ratio of ZrO2 / P2O5: 1.5~3; The ratio of the total amount of glass network formers to the total amount of nucleating agents (SiO2+Al2O3) / (ZrO2+P2O5) is 7.5~17; Ratio of (Li2O+Cs2O+Na2O+K2O) / (ZrO2+P2O5): 1~3; The method for preparing the transparent microcrystalline glass comprises the following steps: (1) Weigh the raw materials according to the proportion, grind and mix them thoroughly, and then put them into a platinum crucible; (2) placing the platinum crucible containing the mixed raw materials into a furnace at 1550-1650°C for pre-sintering, and then grinding the pre-sintered glass clinker to obtain uniform glass powder; (3) The glass powder is melted, stirred and clarified in a platinum crucible; (4) After clarification, the glass is cast into a preheated mold; (5) The formed glass is quickly transferred to an annealing furnace for annealing at the glass transition temperature, and the temperature is naturally lowered after annealing. (6) The glass is subjected to segmented precision heat treatment to ultimately obtain glass-ceramics.

2. The transparent microcrystalline glass according to claim 1, characterized in that: Expressed in weight percentage, it selectively contains MgO: 0~5%, ZnO: 0~5%, Y2O3: 0~2%, La2O3: 0~2%, and Gd2O3: 0~2%.

3. The transparent microcrystalline glass according to claim 1, characterized in that: It also contains a clarifier, which includes, by weight percentage, Sb2O3: 0.1-1.0%, and / or NaNO3: 0.1-1.0%, and / or NaSbO3: 0.1-1.0%, and / or Na2SO4: 0.1-1.0%, and / or SnO2: 0.1-1.0%.

4. The transparent microcrystalline glass according to claim 1, characterized in that: In step (3), the glass powder is melted at 1550-1650°C for 2-5 hours, during which time it is stirred 2-3 times using a platinum stirring rod, each stirring for 30 minutes. The clarification process is carried out at 1550-1600°C for 0.5-2 hours.

5. The transparent micro-ceramic glass according to claim 1, characterized in that: The stepwise precision heat treatment process in step (6) is as follows: the nucleation temperature of the base glass heat treatment is controlled between 50°C and 100°C higher than the glass transition temperature, the nucleation time is 1 to 6 hours, the crystallization temperature is controlled at the crystallization starting temperature, and the crystallization time is 0.5 to 1 hour.