High-strength ceramic product and manufacturing process thereof
By adding toughening agents and composite additives to the alumina and zirconia matrix, and combining ultraviolet light and microwave sintering technology, the problem that the combination of zirconia and alumina cannot improve the strength of ceramic products has been solved, and high-strength and high-toughness ceramic products have been achieved.
Patent Information
- Application Number
- CN202411024264.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-29
AI Technical Summary
In the existing technology, the combination of zirconium oxide and alumina cannot effectively improve the fracture toughness and strength of ceramic products, thus limiting their application in more fields.
High-strength ceramic products are prepared by using alumina and zirconium oxide as the matrix, adding toughening agents, magnesium oxide and chromium oxide, and using a mixture of hyperbranched allyl polysilazane, cysteine, dimercaptopolyethylene glycol with nano boron nitride and nano yttrium oxide as composite additives, combined with ultraviolet light and microwave sintering technology.
It significantly improves the thermal shock resistance, high temperature resistance, corrosion resistance and mechanical properties of ceramic products, and enhances the density and fracture toughness of ceramics.
Smart Images

Figure BDA0004968101940000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic products, in particular to a high-strength ceramic product and a manufacturing process thereof. Background Art
[0002] Traditional ceramics are made from silicate as raw material, which is mixed with water to form a slurry, and then molded and sintered to obtain finished products. With the development of new technologies, traditional ceramics can no longer meet the needs of social development, which has promoted the development of advanced ceramics. Advanced ceramic materials have many excellent properties and play an important role in many fields such as aerospace, automotive industry, electronic equipment, medical equipment, energy technology, etc., promoting the progress of science and technology and industry.
[0003] Advanced ceramics refer to ceramic materials with excellent properties, which are usually used in high-tech fields and special engineering applications; common advanced ceramics include: oxide ceramics, silicon carbide ceramics, boron nitride ceramics, silicon boride ceramics, rare earth oxide ceramics, and composite ceramics; these ceramics have better performance and wider application fields than traditional ceramics; among them, the most representative oxide ceramics are alumina (Al2O3) and zirconia (ZrO2), which have excellent wear resistance, corrosion resistance, high temperature stability and electrical insulation properties, and are widely used in high temperature and high performance fields such as molds, industrial seals, and gas turbines; zirconia can combine well with alumina to play a strengthening role. Although zirconia can improve the fracture toughness and strength of alumina, its effect is limited, thus restricting its development in more fields.
[0004] In summary, it is of great significance to prepare a high-strength ceramic product. Summary of the invention
[0005] The object of the present invention is to provide a high-strength ceramic product and a manufacturing process thereof to solve the problems raised in the above background technology.
[0006] A manufacturing process of a high-strength ceramic product comprises the following steps:
[0007] S1: mixing alumina, zirconia, toughening agent, sintering aid and composite additive for 40 to 65 minutes to obtain a premix;
[0008] S2: placing the premix in a mold for extrusion molding, and irradiating with ultraviolet light for 1.5 to 2.2 hours to obtain a green body;
[0009] S3: Pre-sintering and microwave sintering the green body in sequence to obtain a ceramic product.
[0010] More optimally, the raw materials of the premix include the following components: by weight, 65 to 78 parts of zirconium oxide, 15 to 20 parts of aluminum oxide, 10 to 15 parts of toughening agent, 7 to 10 parts of sintering aid and 15 to 18 parts of composite additives; the sintering aid includes 4 to 5 parts of magnesium oxide and 3 to 4 parts of chromium oxide.
[0011] A more optimized preparation method of the composite additive is: adding hyperbranched allyl polysilazane, cysteine, dithiol polyethylene glycol and azobisisobutyronitrile to tetrahydrofuran and uniformly mixing to obtain a mixed solution; ball-milling the mixed solution with nano boron nitride and nano yttrium oxide in a nitrogen atmosphere for 2 to 2.5 hours, and drying at 70 to 75° C. to obtain the composite additive.
[0012] More optimally, the raw materials of the mixed liquid include the following components: by weight, 6 to 7 parts of hyperbranched allyl polysilazane, 0.002 to 0.004 parts of azobisisobutyronitrile, 1 to 1.5 parts of cysteine, 2 to 2.5 parts of dithiol polyethylene glycol and 15 to 20 parts of tetrahydrofuran; the raw materials of the composite additive include the following components: by weight, 25 to 30 parts of the mixed liquid, 4 to 5 parts of nano boron nitride and 2 to 3 parts of nano yttrium oxide.
[0013] A more optimized preparation method of the toughening agent is: ball-milling carbon nanotubes and urea to obtain a mixture A; adding cerium carbonate to nitric acid and stirring evenly, adding the mixture A, mixing for 10 to 15 minutes, adjusting the pH value to 10 to 12, performing a hydrothermal reaction at 120 to 130° C. for 40 to 48 hours, filtering, and drying; calcining it at 500 to 600° C. for 1 to 1.5 hours to obtain a toughening agent.
[0014] More optimally, the raw materials of the toughening agent include the following components: by weight, 3 to 5 parts of carbon nanotubes, 1 to 3 parts of urea, 4 to 7 parts of cerium carbonate and 10 to 20 parts of nitric acid.
[0015] Preferably, the pre-sintering temperature is 600-750° C., and the pre-sintering time is 40-55 minutes.
[0016] The microwave sintering operation steps are more optimized: heating the green body to 1000-1200°C at a microwave frequency of 200-300 MHz at a heating rate of 12-16°C / min and keeping it warm for 30-45 minutes, and heating it to 1400-1500°C at a heating rate of 40-50°C / min and keeping it warm for 2-3.5 hours to obtain a ceramic product.
[0017] Compared with the prior art, the beneficial effect achieved by the present invention is that: the present invention uses aluminum oxide and zirconium oxide as a matrix, and adds a toughening agent, magnesium oxide, and chromium oxide to prepare a ceramic product.
[0018] Among them, zirconia and alumina have similar lattice structures. The interaction between zirconia and alumina limits the migration of grain boundaries and the growth rate of grains, and can form a solid solution with alumina, thereby improving the density and mechanical properties of ceramics. Zirconia and alumina also have similar thermal expansion coefficients and have a certain toughening effect; the addition of zirconia can reduce the stress accumulation of ceramics when the temperature changes, thereby improving the thermal shock stability and high temperature resistance of ceramics.
[0019] The addition of magnesium oxide can improve the thermal stability and chemical stability of ceramics, reduce the defects of the crystal structure, and thus improve the mechanical properties and thermal shock resistance of ceramics. Chromium oxide itself has good corrosion resistance and hardness, which can improve the corrosion resistance and mechanical properties of ceramics; chromium oxide also has a unique color, which can be used to adjust the color and appearance characteristics of ceramics; and magnesium oxide, chromium oxide and nano-yttrium oxide have the role of sintering aids.
[0020] In order to further improve the fracture toughness of ceramic products, the present invention calcines carbon nanotubes and cerium carbonate to prepare a composite toughening agent containing boron nitride and cerium oxide; the carbon nanotubes have high strength and high modulus, so that they can play a bridging role in the ceramic matrix; when the material is subjected to stress, the carbon nanotubes can bear part of the load, disperse and relieve stress concentration points, and delay the speed of crack propagation; the good interface bonding between the carbon nanotubes and the ceramic matrix can effectively improve the mechanical properties of the composite material, thereby reducing the yield of the material under stress and improving its toughness and wear resistance; the addition of cerium oxide can improve the thermal stability and mechanical properties of ceramic products, and can also slow down the crack propagation of ceramic products, thereby further improving the toughening effect of ceramic products.
[0021] If alumina and zirconia are directly used as the matrix, and toughening agents, magnesium oxide, and chromium oxide are added and evenly mixed before calcining, some of the nanomaterials will agglomerate at high temperatures, thus affecting the performance of the ceramic product.
[0022] In order to improve the dispersion effect of each component in the ceramic product after high-temperature sintering, the present invention uniformly mixes hyperbranched allyl polysilazane, cysteine, dithiol polyethylene glycol and azobisisobutyronitrile to obtain a mixed solution; the mixed solution is ball-milled and mixed with nano boron nitride and nano yttrium oxide in a nitrogen atmosphere for 2 to 2.5 hours to obtain a composite additive.
[0023] Among them, the branched structure and silicon-nitrogen bond of hyperbranched allyl polysilazane enable hyperbranched allyl polysilazane to form effective chemical bonds on the ceramic surface, thereby improving its adhesion and compatibility with the particles; cysteine and dithiol polyethylene glycol cysteine can form stable chemical bonds on the surface of ceramic powders due to their sulfur and other groups, and synergistically improve the dispersibility and stability of the powders with hyperbranched allyl polysilazane.
[0024] Ball-milling and mixing hyperbranched allyl polysilazane, cysteine, and dithiocarbyl polyethylene glycol with nano-boron nitride and nano-yttrium oxide can not only improve the uniform distribution of nano-boron nitride and nano-yttrium chloride in the premix, but also form an organic-inorganic interface with the surface of hard components such as alumina and zirconia, enhance the adhesion and compatibility between the interface layers, prevent particle agglomeration, and thus improve the density and mechanical properties of the ceramic.
[0025] Among them, the addition of nano-boron nitride can help absorb and disperse stress, and can also increase the toughness of ceramic materials, so that its ceramic products can resist external impact and stress, thereby improving thermal shock resistance; nano-boron nitride has a smaller grain size, which can reduce the porosity and density fluctuations of the material, thereby improving the density of the ceramic.
[0026] Adding an appropriate amount of yttrium oxide can stabilize the crystal phase structure of zirconia and transform it into a more stable cubic phase, making it have better thermal shock resistance and beneficial to improving the mechanical properties and wear resistance of zirconia.
[0027] The composite additive, aluminum oxide, zirconium oxide, a toughening agent, magnesium oxide and chromium oxide are ball-milled and mixed to obtain a premix, which is then extruded and molded. Under ultraviolet light irradiation and the action of a photoinitiator, a click chemical reaction occurs between the vinyl groups on the hyperbranched allyl polysilazane in the composite additive and the thiol groups on cysteine and dithiol polyethylene glycol to form covalent bonds, so that organic substances and nanoparticles can effectively fill gaps and defects, increase the density and strength of the material, and improve its overall performance, thereby obtaining a green body.
[0028] The green body is pre-sintered to pyrolyze and remove these organic substances, thereby reducing the residues in the sintering process and ensuring the purity and chemical stability of the final product. Pre-sintering can also bond the ceramic powder in an incompletely sintered state, thereby improving the strength and hardness of the material.
[0029] Finally, the green body is subjected to microwave sintering to obtain ceramic products. The microwaves can heat the material deeply, promote the combination and growth of particles, and help form a more uniform and denser ceramic microstructure. In addition, during the microwave sintering process, the hyperbranched allyl polysilazane in the composite additive generates SiCNO, which is beneficial to enhance the high temperature stability and chemical stability of the ceramic products. DETAILED DESCRIPTION
[0030] The following is a preferred implementation of the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. For ordinary technicians in this technical field, all other embodiments obtained by ordinary technicians in this field without creative work without departing from the principle of the embodiment of the present invention are within the scope of protection of the present invention.
[0031] In the following specific embodiments, parts are by weight. In the present embodiment, it should be noted that the purchase manufacturers of all raw materials involved in the present invention are exemplary without any special restrictions: the CAS number of diallylamine is 124-02-7; the CAS number of trimethylchlorosilane is 75-77-4; the CAS number of Karstedt catalyst is 81032-58-8, the CAS number of azobisisobutyronitrile is 78-67-1; the CAS number of cysteine is 52-90-4; the item number of dithiol polyethylene glycol is 80020104; the item number of nano yttrium oxide is AM-Y203-201-1, and the particle size is 50nm; the model of nano boron nitride is CW-BN-001; the particle size is 50nm; the CAS number of cerium carbonate is 54451-25-1; the item number of aluminum oxide is JS3646; the item number of zirconium oxide is DS140; the item number of carbon nanotubes is WD3713.
[0032] The preparation method of hyperbranched allyl polysilazane comprises the following steps: (1) adding 23 parts of a n-hexane solution of trimethylchlorosilane to 200 parts of n-hexane, 50 parts of diallylamine and 40.5 parts of triethylamine under nitrogen protection and ice-water bath conditions, stirring for 15 minutes under ice-water bath conditions after the addition is complete, continuing the reaction at room temperature for 2 hours, standing until complete precipitation, filtering to remove the precipitation, rotary evaporation to remove excess solvent, and distilling under reduced pressure at 0.003 Mpa and 45° C. to obtain an intermediate; and (2) reacting 12 parts of the intermediate with 0.5 parts of a Karstedt catalyst at 85° C. for 10 to 15 hours, cooling to room temperature, dissolving with ether, precipitating with acetonitrile three times, filtering, collecting the liquid, and distilling to remove the solvent to obtain a hyperbranched allyl polysilazane.
[0033] Embodiment 1: A process for manufacturing a high-strength ceramic product, comprising the following steps:
[0034] S1: The preparation method of the composite additive is as follows: (1) adding 6 parts of hyperbranched allyl polysilazane, 0.0025 parts of azobisisobutyronitrile, 1 part of cysteine, and 2 parts of dithiol polyethylene glycol to 15 parts of tetrahydrofuran to obtain a mixed solution; (2) ball-milling 30 parts of the mixed solution, 4 parts of nano-boron nitride, and 2 parts of nano-yttrium oxide under a nitrogen atmosphere for 2 hours, and drying at 75° C. to obtain a composite additive;
[0035] The toughening agent is prepared by: (1) ball-milling 3 parts of carbon nanotubes and 2 parts of urea to obtain a mixture A; (2) adding 4 parts of cerium carbonate to 10 parts of nitric acid to dissolve, adding the mixture A, mixing for 15 minutes, adjusting the pH value to 10, performing a hydrothermal reaction at 120° C. for 40 hours, filtering, drying, and calcining at 500° C. for 1.2 hours to obtain a toughening agent;
[0036] S2: 15 parts of aluminum oxide, 65 parts of zirconium oxide, 10 parts of toughening agent, 8 parts of sintering aid, and 18 parts of composite additive are mixed for 50 minutes to obtain a premix; wherein the sintering aid is 5 parts of magnesium oxide and 3 parts of chromium oxide;
[0037] S3: placing the premix in a mold for extrusion molding, and irradiating it under 365nm, 100W ultraviolet light for 2 hours to obtain a green body;
[0038] S4: The green body is pre-sintered at 600°C for 40 minutes, then heated to 1000°C at a heating rate of 12°C / min at a microwave frequency of 280 MHz and kept warm for 40 minutes, and then heated to 1400°C at a heating rate of 40°C / min and kept warm for 3.5 hours to obtain a ceramic product.
[0039] Embodiment 2: A process for manufacturing a high-strength ceramic product, comprising the following steps:
[0040] S1: The preparation method of the composite additive is as follows: (1) adding 6 parts of hyperbranched allyl polysilazane, 0.0025 parts of azobisisobutyronitrile, 1 part of cysteine, and 2 parts of dithiol polyethylene glycol to 15 parts of tetrahydrofuran to obtain a mixed solution; (2) ball-milling 30 parts of the mixed solution, 4 parts of nano-boron nitride, and 2 parts of nano-yttrium oxide under a nitrogen atmosphere for 2 hours, and drying at 75° C. to obtain a composite additive;
[0041] The toughening agent is prepared by: (1) ball-milling 3 parts of carbon nanotubes and 2 parts of urea to obtain a mixture A; (2) adding 4 parts of cerium carbonate to 10 parts of nitric acid to dissolve, adding the mixture A, mixing for 15 minutes, adjusting the pH value to 10, performing a hydrothermal reaction at 120° C. for 40 hours, filtering, drying, and calcining at 500° C. for 1.2 hours to obtain a toughening agent;
[0042] S2: 15 parts of aluminum oxide, 78 parts of zirconium oxide, 12 parts of toughening agent, 8 parts of sintering aid, and 16 parts of composite additive are mixed for 50 minutes to obtain a premix; wherein the sintering aid is 5 parts of magnesium oxide and 3 parts of chromium oxide;
[0043] S3: placing the premix in a mold for extrusion molding, and irradiating it under 365nm, 100W ultraviolet light for 2 hours to obtain a green body;
[0044] S4: The green body is pre-sintered at 600°C for 40 minutes, then heated to 1000°C at a heating rate of 12°C / min at a microwave frequency of 280 MHz and kept warm for 40 minutes, and then heated to 1400°C at a heating rate of 40°C / min and kept warm for 3.5 hours to obtain a ceramic product.
[0045] Embodiment 3: A process for manufacturing a high-strength ceramic product, comprising the following steps:
[0046] S1: The preparation method of the composite additive is as follows: (1) adding 6 parts of hyperbranched allyl polysilazane, 0.0025 parts of azobisisobutyronitrile, 1 part of cysteine, and 2 parts of dithiol polyethylene glycol to 15 parts of tetrahydrofuran to obtain a mixed solution; (2) ball-milling 30 parts of the mixed solution, 4 parts of nano-boron nitride, and 2 parts of nano-yttrium oxide under a nitrogen atmosphere for 2 hours, and drying at 75° C. to obtain a composite additive;
[0047] The toughening agent is prepared by: (1) ball-milling 3 parts of carbon nanotubes and 2 parts of urea to obtain a mixture A; (2) adding 4 parts of cerium carbonate to 10 parts of nitric acid to dissolve, adding the mixture A, mixing for 15 minutes, adjusting the pH value to 10, performing a hydrothermal reaction at 120° C. for 40 hours, filtering, drying, and calcining at 500° C. for 1.2 hours to obtain a toughening agent;
[0048] S2: 78 parts of aluminum oxide, 20 parts of zirconium oxide, 15 parts of toughening agent, 8 parts of sintering aid, and 18 parts of composite additive are mixed for 50 minutes to obtain a premix; wherein the sintering aid is 5 parts of magnesium oxide and 3 parts of chromium oxide;
[0049] S3: placing the premix in a mold for extrusion molding, and irradiating it under 365nm, 100W ultraviolet light for 2 hours to obtain a green body;
[0050] S4: The green body is pre-sintered at 600°C for 40 minutes, then heated to 1000°C at a heating rate of 12°C / min at a microwave frequency of 280 MHz and kept warm for 40 minutes, and then heated to 1400°C at a heating rate of 40°C / min and kept warm for 3.5 hours to obtain a ceramic product.
[0051] Comparative Example 1 is based on Example 2, except that cysteine and dithiopolyethylene glycol are not added to the mixed solution;
[0052] S1: The preparation method of the composite additive is as follows: (1) adding 6 parts of hyperbranched allyl polysilazane, 4 parts of nano boron nitride, and 2 parts of nano yttrium oxide to 15 parts of tetrahydrofuran to obtain a mixed solution; (2) ball milling the mixed solution under a nitrogen atmosphere for 2 hours, and drying at 75° C. to obtain a composite additive;
[0053] The toughening agent is prepared by: (1) ball-milling 3 parts of carbon nanotubes and 2 parts of urea to obtain a mixture A; (2) adding 4 parts of cerium carbonate to 10 parts of nitric acid to dissolve, adding the mixture A, mixing for 15 minutes, adjusting the pH value to 10, performing a hydrothermal reaction at 120° C. for 40 hours, filtering, drying, and calcining at 500° C. for 1.2 hours to obtain a toughening agent;
[0054] S2: 15 parts of aluminum oxide, 78 parts of zirconium oxide, 12 parts of toughening agent, 8 parts of sintering aid, and 16 parts of composite additive are mixed for 50 minutes to obtain a premix; wherein the sintering aid is 5 parts of magnesium oxide and 3 parts of chromium oxide;
[0055] S3: placing the premix in a mold and extruding it to obtain a green body;
[0056] S4: The green body is pre-sintered at 600°C for 40 minutes, then heated to 1000°C at a heating rate of 12°C / min at a microwave frequency of 280 MHz and kept warm for 40 minutes, and then heated to 1400°C at a heating rate of 40°C / min and kept warm for 3.5 hours to obtain a ceramic product.
[0057] Comparative Example 2 is based on Example 2, but no carbon nanotubes are added to the toughening agent;
[0058] S1: The preparation method of the composite additive is as follows: (1) adding 6 parts of hyperbranched allyl polysilazane, 0.0025 parts of azobisisobutyronitrile, 1 part of cysteine, and 2 parts of dithiol polyethylene glycol to 15 parts of tetrahydrofuran to obtain a mixed solution; (2) ball-milling 30 parts of the mixed solution, 4 parts of nano-boron nitride, and 2 parts of nano-yttrium oxide under a nitrogen atmosphere for 2 hours, and drying at 75° C. to obtain a composite additive;
[0059] The toughening agent is prepared by adding 4 parts of cerium carbonate to 10 parts of nitric acid to dissolve, adding urea, mixing for 15 minutes, adjusting the pH value to 10, performing a hydrothermal reaction at 120° C. for 40 hours, filtering, drying, and calcining at 500° C. for 1.2 hours to obtain the toughening agent;
[0060] S2: 15 parts of aluminum oxide, 78 parts of zirconium oxide, 12 parts of toughening agent, 8 parts of sintering aid, and 16 parts of composite additive are mixed for 250 minutes to obtain a premix; wherein the sintering aid is 5 parts of magnesium oxide and 3 parts of chromium oxide;
[0061] S3: placing the premix in a mold for extrusion molding, and irradiating it under 365nm, 100W ultraviolet light for 2 hours to obtain a green body;
[0062] S4: The green body is pre-sintered at 600°C for 40 minutes, then heated to 1000°C at a heating rate of 12°C / min at a microwave frequency of 280 MHz and kept warm for 40 minutes, and then heated to 1400°C at a heating rate of 40°C / min and kept warm for 3.5 hours to obtain a ceramic product.
[0063] Comparative Example 3 Based on Example 2, the green body is directly sintered at high temperature;
[0064] S1: The preparation method of the composite additive is as follows: (1) adding 6 parts of hyperbranched allyl polysilazane, 0.0025 parts of azobisisobutyronitrile, 1 part of cysteine, and 2 parts of dithiol polyethylene glycol to 15 parts of tetrahydrofuran to obtain a mixed solution; (2) ball-milling 30 parts of the mixed solution, 4 parts of nano-boron nitride, and 2 parts of nano-yttrium oxide under a nitrogen atmosphere for 3 hours, and drying at 75° C. to obtain a composite additive;
[0065] The toughening agent is prepared by: (1) ball-milling 3 parts of carbon nanotubes and 2 parts of urea to obtain a mixture A; (2) adding 4 parts of cerium carbonate to 10 parts of nitric acid to dissolve, adding the mixture A, mixing for 15 minutes, adjusting the pH value to 10, performing a hydrothermal reaction at 120° C. for 40 hours, filtering, drying, and calcining at 500° C. for 1.2 hours to obtain a toughening agent;
[0066] S2: 15 parts of aluminum oxide, 78 parts of zirconium oxide, 12 parts of toughening agent, 8 parts of sintering aid, and 16 parts of composite additive are mixed for 50 minutes to obtain a premix; wherein the sintering aid is 5 parts of magnesium oxide and 3 parts of chromium oxide;
[0067] S3: placing the premix in a mold for extrusion molding, and irradiating it under 365nm, 100W ultraviolet light for 2 hours to obtain a green body;
[0068] S4: heating the green body to 1000° C. at a heating rate of 12° C. / min and keeping the temperature for 40 minutes, and then heating the green body to 1400° C. at a heating rate of 40° C. / min and keeping the temperature for 3.5 hours to obtain a ceramic product.
[0069] Comparative Example 4 is based on Example 2, firstly, a modified allyl polysilazane is obtained by ultraviolet irradiation, and then a composite additive is prepared;
[0070] S1: The preparation method of the composite additive is as follows: (1) adding 6 parts of hyperbranched allyl polysilazane, 0.0025 parts of azobisisobutyronitrile, 1 part of cysteine, and 2 parts of dithiol polyethylene glycol to 15 parts of tetrahydrofuran, irradiating the mixture under ultraviolet light of 365 nm and 100 W for 2 hours, and drying the mixture at 75° C. to obtain modified allyl polysilazane; (2) ball-milling and mixing 10 parts of modified allyl polysilazane, 4 parts of nano boron nitride, and 2 parts of nano yttrium oxide under a nitrogen atmosphere for 2 hours to obtain a composite additive;
[0071] The toughening agent is prepared by: (1) ball-milling 3 parts of carbon nanotubes and 2 parts of urea to obtain a mixture A; (2) adding 4 parts of cerium carbonate to 10 parts of nitric acid to dissolve, adding the mixture A, mixing for 15 minutes, adjusting the pH value to 10, performing a hydrothermal reaction at 120° C. for 40 hours, filtering, drying, and calcining at 500° C. for 1.2 hours to obtain a toughening agent;
[0072] S2: 15 parts of aluminum oxide, 78 parts of zirconium oxide, 12 parts of toughening agent, 8 parts of sintering aid, and 16 parts of composite additive are mixed for 50 minutes to obtain a premix; wherein the sintering aid is 5 parts of magnesium oxide and 3 parts of chromium oxide;
[0073] S3: placing the premix in a mold and extruding it to obtain a green body;
[0074] S4: The green body is pre-sintered at 600°C for 40 minutes, then heated to 1000°C at a heating rate of 12°C / min at a microwave frequency of 280 MHz and kept warm for 40 minutes, and then heated to 1400°C at a heating rate of 40°C / min and kept warm for 3.5 hours to obtain a ceramic product.
[0075] Test 1: Thermal shock resistance test: 7 ceramic products of Examples 1 to 3 and Comparative Examples 1 to 4 were taken respectively and placed under 20°C and 200°C for heat exchange treatment twice; and the fracture toughness of Examples 1 to 3 and Comparative Examples 1 to 4 before and after thermal shock resistance was tested, and the average value of the final results was taken, as shown in Table 1;
[0076]
[0077] Table 1
[0078] Conclusion: Comparative Example 1 is based on Example 2, but cysteine and dithiol polyethylene glycol are not added to the mixed solution; the adhesion and compatibility between the organic-inorganic interface formed with the surface of hard components such as alumina and zirconia are reduced, resulting in a decrease in the fracture toughness of the ceramic product. Comparative Example 2 is based on Example 2, but carbon nanotubes are not added to the toughening agent, so that the fracture toughness of the ceramic product is reduced; because carbon nanotubes have high strength and high modulus, they can play a bridging role in the ceramic matrix. When the material is subjected to stress, carbon nanotubes can not only bear part of the load, but also disperse and relieve stress concentration points, thereby slowing down the rate of crack propagation.
[0079] Comparative Example 3 is based on Example 2. The green body is directly hot-pressed and sintered. Within the same sintering time as microwave hot pressing, its production cycle needs to be extended, and the performance of the ceramic product is reduced; because pre-sintering can pyrolyze and remove these organic substances, thereby reducing the residues in the sintering process, and bonding the ceramic powder in an incompletely sintered state, improving the performance of the ceramic; and microwaves can deeply heat the interior of the material, promote the combination and growth of particles, and help to form a more uniform, which is beneficial to improve the performance of ceramic products. Comparative Example 4 is based on Example 2. Modified allyl polysilazane is first obtained by ultraviolet irradiation, and then a composite additive is prepared, so that the organic substance and nanoparticles cannot effectively fill the gaps and defects, thereby reducing the density and strength of the material, resulting in a decrease in the performance of the ceramic product.
[0080] Performance test 2:
[0081] <![CDATA[Apparent density (g·cm -3 )]]> Example 2 5.74 Comparative Example 1 5.32 Comparative Example 2 5.68 Comparative Example 3 5.17 Comparative Example 4 5.52
[0082] Table 2
[0083] Conclusion: Comparative Example 1 is based on Example 2, except that cysteine and dithiol polyethylene glycol are not added to the mixed solution; this results in a decrease in the dispersibility of the composite additive, thereby reducing the density of the ceramic product. Comparative Example 2 is based on Example 2, and it is found that it has little effect on the density of the ceramic product. Comparative Example 3 is based on Example 2, and the green body is directly sintered at high temperature, which results in a decrease in the density of the ceramic product; because microwaves can heat the material deeply, promote the combination and growth of particles, and help form a more uniform and denser ceramic microstructure, the density of Comparative Example 2 is reduced. Comparative Example 4 is based on Example 2. Comparative Example 4 is based on Example 2, and firstly obtains modified allyl polysilazane by ultraviolet irradiation, and then prepares the composite additive, so that the organic matter and nanoparticles cannot effectively fill the gaps and defects, thereby resulting in a decrease in the density of the ceramic product.
[0084] Finally, it should be noted that the above is only a preferred embodiment of the present invention, but the protection scope of this application is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the spirit and principle of the present invention and within the technical scope disclosed in this application should be included in the protection scope of this application; in the absence of conflict, the embodiments of this application and the features in the embodiments can be combined with each other. Therefore, the protection scope of this application shall be based on the protection scope of the claims.
Claims
1. A process for producing high-strength ceramic products, characterized in that: The steps include: S1: mixing alumina, zirconia, toughening agent, sintering aid and composite additive for 40 to 65 minutes to obtain a premix; S2: placing the premix in a mold for extrusion molding, and irradiating with ultraviolet light for 1.5 to 2.2 hours to obtain a green body; S3: Pre-sintering and microwave sintering the green body in sequence to obtain a ceramic product.
2. The manufacturing process of a high-strength ceramic product according to claim 1, characterized in that: The raw materials of the premix include the following components: by weight, 65 to 78 parts of zirconium oxide, 15 to 20 parts of aluminum oxide, 10 to 15 parts of toughening agent, 7 to 10 parts of sintering aid and 15 to 18 parts of composite additive; the sintering aid includes 4 to 5 parts of magnesium oxide and 3 to 4 parts of chromium oxide.
3. The manufacturing process of a high-strength ceramic product according to claim 1, characterized in that: The preparation method of the composite additive comprises the following steps: adding hyperbranched allyl polysilazane, cysteine, dimercapto polyethylene glycol and azobisisobutyronitrile into tetrahydrofuran and uniformly mixing to obtain a mixed solution; ball milling the mixed solution with nano boron nitride and nano yttrium oxide in a nitrogen atmosphere for 2 to 2.5 hours, and drying at 70 to 75° C. to obtain the composite additive.
4. The manufacturing process of a high-strength ceramic product according to claim 3, characterized in that: The raw materials of the mixed liquid include the following components: by weight, 6 to 7 parts of hyperbranched allyl polysilazane, 0.002 to 0.004 parts of azobisisobutyronitrile, 1 to 1.5 parts of cysteine, 2 to 2.5 parts of dithiol polyethylene glycol and 15 to 20 parts of tetrahydrofuran; the raw materials of the composite additive include the following components: by weight, 25 to 30 parts of the mixed liquid, 4 to 5 parts of nano boron nitride and 2 to 3 parts of nano yttrium oxide.
5. The manufacturing process of a high-strength ceramic product according to claim 1, characterized in that: The preparation method of the toughening agent comprises the following steps: mixing carbon nanotubes and urea by ball milling to obtain a mixture A; adding cerium carbonate into nitric acid and stirring evenly, adding the mixture A, mixing for 10 to 15 minutes, adjusting the pH value to 10 to 12, performing a hydrothermal reaction at 120 to 130° C. for 40 to 48 hours, filtering, and drying; and calcining at 500 to 600° C. for 1 to 1.5 hours to obtain the toughening agent.
6. The manufacturing process of a high-strength ceramic product according to claim 5, characterized in that: The raw materials of the toughening agent include the following components: by weight, 3 to 5 parts of carbon nanotubes, 1 to 3 parts of urea, 4 to 7 parts of cerium carbonate and 10 to 20 parts of nitric acid.
7. The manufacturing process of a high-strength ceramic product according to claim 1, characterized in that: The pre-sintering temperature is 600-750° C., and the pre-sintering time is 40-55 minutes.
8. The manufacturing process of a high-strength ceramic product according to claim 1, characterized in that: The microwave sintering operation steps are: heating the green body to 1000-1200°C at a microwave frequency of 200-300 MHz at a heating rate of 12-16°C / min and keeping the temperature for 30-45 minutes, and heating the green body to 1400-1500°C at a heating rate of 40-50°C / min and keeping the temperature for 2-3.5 hours to obtain a ceramic product.
9. A ceramic product prepared according to the manufacturing process of a high-strength ceramic product according to any one of claims 1 to 8.
Citation Information
Patent Citations
Composite ceria-zirconia solid solution and preparation method thereof
CN105642269A
Zirconium oxide-based ceramic material as well as preparation method and application thereof
CN108751984A
Zirconium oxide toughened aluminum oxide cutter and preparation method thereof
CN112939581A
In-situ solidification colloidal forming method of high-performance alumina-based composite ceramic
CN113511914A
Silicon nitride composite ceramic material for sealing ring and preparation method of silicon nitride composite ceramic material
CN116553937A
Cited By
High-strength ceramic and forming process thereof
CN120309315A
Ceramic piece and manufacturing method thereof
CN120664865A
Environment-friendly ceramic and preparation method thereof
CN120965358A
Environment-friendly ceramic and preparation method thereof
CN120965358B