Refractory castable for roller casting end cover and preparation method thereof

By using a combination of mineral raw materials and functional nanomaterials in the roll casting end cap, cementless refractory castables were prepared, which solved the problems of traditional refractory materials falling off and heat shrinking at high temperatures, and achieved high temperature mechanical properties and morphological stability The lifting ensures the normal operation of the roll.

CN118637934BActive Publication Date: 2024-11-12SHANDONG REFRACTORIES GROUP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411112232.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-12
Estimated Expiration
2044-08-14

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention belongs to the technical field of refractory castables, and specifically relates to a refractory castable for roller casting end covers and a preparation method thereof. The refractory castable is composed of the following raw materials: mineral raw materials, α-Al2O3 micropowder, silicon dioxide micropowder, titanium carbide modified carbon nanotubes, nano zirconium dioxide, polyvinyl alcohol fiber, aluminum lactate, a binder and water; wherein the mineral raw material is a mixture of plate-like corundum, magnesium aluminum spinel and pyrochloreite, and the binder is a mixture of magnesium hydrogen phosphate and hydrated alumina. The refractory castable for roller casting end covers described in the present invention has good mechanical properties at room temperature and high temperature and high morphological stability. The high high temperature strength ensures that no cracking occurs under high-speed rotation and vibration during centrifugal casting of rollers, and the good morphological stability prevents the end covers from peeling off, falling off, etc. during high-temperature use, thereby avoiding the refractory material from entering the liquid medium and affecting the quality of the rollers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of refractory castables, and specifically relates to a refractory castable for a roller casting end cover and a preparation method thereof. Background Art

[0002] Rollers are tools that cause the metal of the rolled material to undergo plastic deformation, and are important consumable parts that determine the efficiency of the rolling mill and the quality of the rolled material. Casting rolls refer to the type of rolls manufactured by the production method of directly casting molten steel or molten iron. At present, with the rapid development of my country's steel roll industry, centrifugal casting rolls are developing rapidly. However, during the use of the end caps installed at both ends of the centrifugal casting molten steel mold sleeve, the refractory materials used are prone to falling off, falling off, and thermal shrinkage. This is because the existing end caps generally use traditional cement-bonded castables. Due to the high amount of cement added, the amount of water added to the castable increases, and the later drying and dehydration of the prefabricated parts takes a long time. The cement hydration causes the temperature of the castable to be high and the strength to be low. In addition, excessive cement use introduces a large amount of CaO, which reduces the high-temperature performance of the castable, ultimately affecting the normal use of the end caps.

[0003] The end caps are fixed at both ends of the centrifugal casting steel mold sleeve. Driven by the centrifuge, the centrifugal casting steel mold sleeve rotates at high speed, generating huge vibrations. At the same time, the temperature of the injected molten steel or molten iron is as high as 1350-1550℃, and the end caps are directly in contact with the high-temperature molten steel or molten iron at room temperature. Therefore, the refractory castables used for the end caps are required to have the following characteristics: (1) have a certain strength to ensure that there is no cracking under high-speed rotation and vibration; (2) have a low linear change rate and no thermal shrinkage; (3) have a high thermal shock stability, and no peeling or falling off during use, so as to avoid the refractory material entering the liquid medium and affecting the quality of the roll.

[0004] In summary, it is an inevitable trend for refractory castables for end covers to develop towards high-strength, low-cement bonding or even cement-free castings. Therefore, it is imperative to study a new type of refractory castable for roll casting end covers and improve the mechanical properties of the castable without using cement as a binder. Summary of the invention

[0005] The purpose of the present invention is to provide a refractory castable for roller casting end cover, wherein the refractory castable has good anti-burst performance and mechanical strength; the present invention also provides a preparation method thereof.

[0006] The refractory castable for roller casting end cover described in the present invention is composed of the following raw materials, measured in parts by weight: 71-73 parts of mineral raw materials, 12-14 parts of α-Al2O3 micropowder, 6-8 parts of silicon dioxide micropowder, 5-6 parts of titanium carbide modified carbon nanotubes, 1.4-1.6 parts of nano zirconium dioxide, 0.05-0.07 parts of polyvinyl alcohol fibers, 0.03-0.05 parts of aluminum lactate, 6-7 parts of binders and 4-5 parts of water; wherein the mineral raw materials are a mixture of plate-like corundum, magnesia-aluminum spinel and pyrope, and the binder is a mixture of magnesium hydrogen phosphate and hydrated alumina.

[0007] in:

[0008] The mass ratio of plate-shaped corundum, magnesium-aluminum spinel and pyroxene in the mineral raw materials is 4-6: 2-5: 5-7.

[0009] The mineral raw materials, calculated by mass percentage, are composed of 15-18% of granular materials with a particle size of 5mm<≤8mm, 15-18% of granular materials with a particle size of 3mm<≤5mm, 20-24% of granular materials with a particle size of 1mm<≤3mm, 21-24% of granular materials with a particle size of 0.074mm<≤1mm, and 20-24% of powder materials with a particle size of ≤0.074mm.

[0010] The mass ratio of magnesium hydrogen phosphate to hydrated alumina in the binder is 1:0.45-0.55.

[0011] The particle size of α-Al2O3 powder is 2 μm, and the particle size of silica powder is 0.3 μm.

[0012] The preparation method of titanium carbide modified carbon nanotubes comprises the following steps: mixing carbon nanotubes, titanium powder and mixed salt, reacting at 1100°C for 3.5 hours under argon atmosphere, cooling to room temperature with the furnace, and then washing, filtering and drying to prepare titanium carbide modified carbon nanotubes.

[0013] in:

[0014] The molar ratio of carbon nanotubes to titanium powder is 1:0.5, and the added amount of the mixed salt is 8% of the total mass of the carbon nanotubes and titanium powder.

[0015] The mixed salt is a mixture of potassium chloride and lithium chloride, and the molar ratio of potassium chloride to lithium chloride is 59:41.

[0016] The product was washed with boiling water at 100°C, filtered and dried at 115°C for 12.5h.

[0017] The refractory castable for the roll casting end cover described in the present invention uses a mixture of plate-shaped corundum, magnesium-aluminum spinel and pyroxene as the main raw materials. Magnesium-aluminum spinel has the characteristics of small thermal expansion coefficient, strong corrosion resistance and good thermal shock resistance. It is used in combination with plate-shaped corundum, so that the prepared refractory castable has good slag corrosion resistance and good flexural strength. In order to reduce production costs, part of pyroxene is also added. The pyroxene interacts with other raw materials at high temperature to generate mullite reinforcement phase in situ, which fundamentally ensures the mechanical properties of the refractory castable. In addition, α-Al2O3 micropowder and silicon dioxide micropowder are added to the refractory castable. The addition of micropowder can improve the fluidity of the castable and increase the density of the castable. At high temperature, the two react with each other to generate mullite reinforcement phase, so that the prepared refractory castable has good high-temperature strength.

[0018] The refractory castable for roller casting end cover described in the present invention creatively adds carbon nanotubes modified with titanium carbide, nano zirconium dioxide, polyvinyl alcohol fibers and aluminum lactate. The four are used in combination to synergistically improve the mechanical properties, anti-burst performance and corrosion resistance of the prepared refractory castable. Among them: first, a titanium carbide coating is generated on the surface of the carbon nanotubes through a high-temperature in-situ reaction, thereby obtaining titanium carbide modified carbon nanotubes. The role of the titanium carbide modified carbon nanotubes is to reduce the thermal expansion of the refractory castable and improve the slag resistance of the refractory castable. The addition of nano zirconium dioxide is beneficial to increase the grain boundary activity, thereby densifying the refractory castable, and improving the high-temperature mechanical properties and corrosion resistance of the refractory castable. In order to improve the early strength of the refractory castable, hydrated alumina is used in the binder. The use of hydrated alumina will hinder the removal of water vapor in the refractory castable, making the anti-burst performance of the refractory castable worse. Therefore, polyvinyl alcohol fiber and aluminum lactate are compounded to improve the anti-burst performance of the refractory castable. Among them, polyvinyl alcohol fiber can produce exhaust channels earlier, thereby reducing the damage of the pressure generated by water vapor to the refractory castable. Compounding with aluminum lactate ensures that the mechanical strength of the refractory castable is not reduced.

[0019] The refractory castable for the roller casting end cover described in the present invention uses a mixture of magnesium hydrogen phosphate and hydrated alumina as a binder. Among them: magnesium hydrogen phosphate has the advantages of small strength loss at medium and low temperatures, little influence by ambient temperature, good adhesion, etc., but if only magnesium hydrogen phosphate is used as a binder, it is easy to cause a significant decrease in the elastic modulus of the refractory castable, so hydrated alumina is used in combination. In order to make the refractory castable for the roller casting end cover have good early strength, hydrated alumina, i.e., ρ-Al2O3, is added to the binder. The addition of hydrated alumina can significantly improve the high-temperature mechanical properties of the refractory castable and the refractoriness of the refractory castable. Therefore, the binder is mainly magnesium hydrogen phosphate, supplemented by hydrated alumina, and the two are used in combination, so that the binder and other raw materials work synergistically to ensure that the prepared refractory castable has good comprehensive performance.

[0020] The method for preparing the refractory castable for roller casting end cover of the present invention comprises the following steps:

[0021] (1) Adding mineral raw materials, α-Al2O3 powder, silicon dioxide powder, titanium carbide modified carbon nanotubes, nano zirconium dioxide, polyvinyl alcohol fiber, aluminum lactate and binder into a mixer in proportion and dry mixing;

[0022] (2) Adding water to the dry mixture obtained in step (1) and mixing again, casting the mixed slurry in a mold, curing, demoulding, and drying to obtain a refractory castable for a roll casting end cover.

[0023] in:

[0024] The curing time in step (2) is 50-52 hours, and the curing temperature is room temperature.

[0025] In step (2), the drying temperature is 112-115° C. and the drying time is 13-13.5 h.

[0026] Compared with the prior art, the present invention has the following effects:

[0027] (1) The refractory castable for the end cap of the roll casting of the present invention has good mechanical properties at room temperature and high temperature and high morphological stability. The high high temperature strength ensures that the centrifugal casting roll does not crack under high-speed rotation and vibration, and the good morphological stability prevents the end cap from peeling off or falling off during high-temperature use, thereby preventing the refractory material from entering the liquid medium and affecting the quality of the roll.

[0028] (2) The refractory castable for the roller casting end cover described in the present invention does not add calcium aluminate cement in the binder, thereby overcoming the defect that the calcium oxide component in the cement reacts with Al2O3 and SiO2 in the castable at high temperature to form low melting point phases such as calcium feldspar and calcium aluminum feldspar, thereby reducing the refractoriness and high temperature strength of the refractory material.

[0029] (3) The method for preparing the refractory castable for the roller casting end cover of the present invention has a simple process and easy-to-control parameters. The prepared refractory castable for the end cover has stable comprehensive performance. DETAILED DESCRIPTION

[0030] The present invention is further described below with reference to the embodiments.

[0031] The manufacturer of nano zirconium dioxide is Shanghai Chaowei Nano Technology Co., Ltd., and the product model is CW-ZrO2-002.

[0032] Example 1

[0033] The refractory castable for the roller casting end cover described in this Example 1 is composed of the following raw materials, measured in parts by weight: 72 parts of mineral raw materials, 13 parts of α-Al2O3 micropowder, 7 parts of silica micropowder, 5.5 parts of titanium carbide modified carbon nanotubes, 1.5 parts of nano zirconium dioxide, 0.06 parts of polyvinyl alcohol fiber, 0.04 parts of aluminum lactate, 6.5 parts of binder and 4.5 parts of water; wherein the mineral raw material is a mixture of plate-like corundum, magnesia-aluminum spinel and pyroxene, and the binder is a mixture of magnesium hydrogen phosphate and hydrated alumina.

[0034] in:

[0035] The mass ratio of plate-shaped corundum, magnesia-alumina spinel and pyroxene in the mineral raw materials is 5:3.5:6.

[0036] The mineral raw materials, calculated by mass percentage, have the following raw material composition: 17% of granules with a particle size of 5mm<≤8mm, 15% of granules with a particle size of 3mm<≤5mm, 20% of granules with a particle size of 1mm<≤3mm, 24% of granules with a particle size of 0.074mm<≤1mm, and 24% of powder with a particle size of ≤0.074mm.

[0037] The mass ratio of magnesium hydrogen phosphate to hydrated alumina in the binder is 1:0.50.

[0038] The particle size of α-Al2O3 powder is 2 μm, and the particle size of silica powder is 0.3 μm.

[0039] The preparation method of titanium carbide modified carbon nanotubes comprises the following steps: mixing carbon nanotubes, titanium powder and mixed salt, reacting at 1100°C for 3.5 hours under argon atmosphere, cooling to room temperature with the furnace, and then washing, filtering and drying to prepare titanium carbide modified carbon nanotubes.

[0040] in:

[0041] The molar ratio of carbon nanotubes to titanium powder is 1:0.5, and the added amount of the mixed salt is 8% of the total mass of the carbon nanotubes and titanium powder.

[0042] The mixed salt is a mixture of potassium chloride and lithium chloride, and the molar ratio of potassium chloride to lithium chloride is 59:41.

[0043] The product was washed with boiling water at 100°C, filtered and dried at 115°C for 12.5h.

[0044] The method for preparing the refractory castable for the roll casting end cover described in this embodiment 1 comprises the following steps:

[0045] (1) Adding mineral raw materials, α-Al2O3 powder, silicon dioxide powder, titanium carbide modified carbon nanotubes, nano zirconium dioxide, polyvinyl alcohol fiber, aluminum lactate and binder into a mixer in proportion and dry mixing;

[0046] (2) Adding water to the dry mixture obtained in step (1) and mixing again, casting the mixed slurry in a mold, curing, demoulding, and drying to obtain a refractory castable for a roll casting end cover.

[0047] in:

[0048] The curing time in step (2) is 51 hours, and the curing temperature is room temperature.

[0049] In step (2), the drying temperature is 114° C. and the drying time is 13.2 h.

[0050] Example 2

[0051] The refractory castable for the roller casting end cover described in this Example 2 is composed of the following raw materials, measured in parts by weight: 71 parts of mineral raw materials, 14 parts of α-Al2O3 micropowder, 6 parts of silica micropowder, 6 parts of titanium carbide modified carbon nanotubes, 1.4 parts of nano zirconium dioxide, 0.07 parts of polyvinyl alcohol fibers, 0.03 parts of aluminum lactate, 6 parts of binder and 4 parts of water; wherein the mineral raw materials are a mixture of plate-like corundum, magnesia-aluminum spinel and pyroxene, and the binder is a mixture of magnesium hydrogen phosphate and hydrated alumina.

[0052] in:

[0053] The mass ratio of plate-shaped corundum, magnesia-alumina spinel and pyroxene in the mineral raw materials is 6:5:5.

[0054] The mineral raw materials are composed of the following raw materials in percentage by mass: 15% of granules with a particle size of 5mm<≤8mm, 18% of granules with a particle size of 3mm<≤5mm, 22% of granules with a particle size of 1mm<≤3mm, 22% of granules with a particle size of 0.074mm<≤1mm, and 23% of powder with a particle size of ≤0.074mm.

[0055] The mass ratio of magnesium hydrogen phosphate to hydrated alumina in the binder is 1:0.45.

[0056] The particle size of α-Al2O3 powder is 2 μm, and the particle size of silica powder is 0.3 μm.

[0057] The preparation method of titanium carbide modified carbon nanotubes comprises the following steps: mixing carbon nanotubes, titanium powder and mixed salt, reacting at 1100°C for 3.5 hours under argon atmosphere, cooling to room temperature with the furnace, and then washing, filtering and drying to prepare titanium carbide modified carbon nanotubes.

[0058] in:

[0059] The molar ratio of carbon nanotubes to titanium powder is 1:0.5, and the added amount of the mixed salt is 8% of the total mass of the carbon nanotubes and titanium powder.

[0060] The mixed salt is a mixture of potassium chloride and lithium chloride, and the molar ratio of potassium chloride to lithium chloride is 59:41.

[0061] The product was washed with boiling water at 100°C, filtered and dried at 115°C for 12.5h.

[0062] The method for preparing the refractory castable for the roll casting end cover described in this embodiment 2 comprises the following steps:

[0063] (1) Adding mineral raw materials, α-Al2O3 powder, silicon dioxide powder, titanium carbide modified carbon nanotubes, nano zirconium dioxide, polyvinyl alcohol fiber, aluminum lactate and binder into a mixer in proportion and dry mixing;

[0064] (2) Adding water to the dry mixture obtained in step (1) and mixing again, casting the mixed slurry in a mold, curing, demoulding, and drying to obtain a refractory castable for a roll casting end cover.

[0065] in:

[0066] The curing time in step (2) is 50 hours and the curing temperature is room temperature.

[0067] In step (2), the drying temperature is 112° C. and the drying time is 13.5 h.

[0068] Example 3

[0069] The refractory castable for the roller casting end cover described in this Example 3 is composed of the following raw materials, measured in parts by weight: 73 parts of mineral raw materials, 12 parts of α-Al2O3 micropowder, 8 parts of silica micropowder, 5 parts of titanium carbide modified carbon nanotubes, 1.6 parts of nano zirconium dioxide, 0.05 parts of polyvinyl alcohol fibers, 0.05 parts of aluminum lactate, 7 parts of binder and 5 parts of water; wherein the mineral raw materials are a mixture of plate-like corundum, magnesium aluminum spinel and pyroxene, and the binder is a mixture of magnesium hydrogen phosphate and hydrated alumina.

[0070] in:

[0071] The mass ratio of plate-shaped corundum, magnesia-alumina spinel and pyroxene in the mineral raw materials is 4:2:7.

[0072] The mineral raw materials are composed of the following raw materials in percentage by mass: 18% of granules with a particle size of 5mm<≤8mm, 17% of granules with a particle size of 3mm<≤5mm, 24% of granules with a particle size of 1mm<≤3mm, 21% of granules with a particle size of 0.074mm<≤1mm, and 20% of powder with a particle size of ≤0.074mm.

[0073] The mass ratio of magnesium hydrogen phosphate to hydrated alumina in the binder is 1:0.55.

[0074] The particle size of α-Al2O3 powder is 2 μm, and the particle size of silica powder is 0.3 μm.

[0075] The preparation method of titanium carbide modified carbon nanotubes comprises the following steps: mixing carbon nanotubes, titanium powder and mixed salt, reacting at 1100°C for 3.5 hours under argon atmosphere, cooling to room temperature with the furnace, and then washing, filtering and drying to prepare titanium carbide modified carbon nanotubes.

[0076] in:

[0077] The molar ratio of carbon nanotubes to titanium powder is 1:0.5, and the added amount of the mixed salt is 8% of the total mass of the carbon nanotubes and titanium powder.

[0078] The mixed salt is a mixture of potassium chloride and lithium chloride, and the molar ratio of potassium chloride to lithium chloride is 59:41.

[0079] The product was washed with boiling water at 100°C, filtered and dried at 115°C for 12.5h.

[0080] The method for preparing the refractory castable for the roll casting end cover described in this embodiment 3 comprises the following steps:

[0081] (1) Adding mineral raw materials, α-Al2O3 powder, silicon dioxide powder, titanium carbide modified carbon nanotubes, nano zirconium dioxide, polyvinyl alcohol fiber, aluminum lactate and binder into a mixer in proportion and dry mixing;

[0082] (2) Adding water to the dry mixture obtained in step (1) and mixing again, casting the mixed slurry in a mold, curing, demoulding, and drying to obtain a refractory castable for a roll casting end cover.

[0083] in:

[0084] The curing time in step (2) is 52 hours, and the curing temperature is room temperature.

[0085] In step (2), the drying temperature is 115° C. and the drying time is 13 h.

[0086] Comparative Example 1

[0087] The preparation method of the refractory castable for the roller casting end cover described in this comparative example 1 is the same as that of Example 1, and the only difference is that the raw material composition of the refractory castable is different. The refractory castable for the roller casting end cover described in this comparative example 1 is composed of the following raw materials in parts by weight: 72 parts of mineral raw materials, 13 parts of α-Al2O3 powder, 7 parts of silica powder, 1.5 parts of nano zirconium dioxide, 0.06 parts of polyvinyl alcohol fiber, 0.04 parts of aluminum lactate, 6.5 parts of binder and 4.5 parts of water; wherein the mineral raw materials are a mixture of plate-like corundum, magnesium aluminum spinel and pyrope, and the binder is a mixture of magnesium hydrogen phosphate and hydrated alumina.

[0088] Comparative Example 2

[0089] The preparation method of the refractory castable for the roller casting end cover described in this comparative example 2 is the same as that of Example 1, and the only difference is that the raw material composition of the refractory castable is different. The refractory castable for the roller casting end cover described in this comparative example 2 is composed of the following raw materials in parts by weight: 72 parts of mineral raw materials, 13 parts of α-Al2O3 micropowder, 7 parts of silica micropowder, 5.5 parts of titanium carbide modified carbon nanotubes, 0.06 parts of polyvinyl alcohol fiber, 0.04 parts of aluminum lactate, 6.5 parts of binder and 4.5 parts of water; wherein the mineral raw material is a mixture of plate-like corundum, magnesium aluminum spinel and pyrope, and the binder is a mixture of magnesium hydrogen phosphate and hydrated alumina.

[0090] Comparative Example 3

[0091] The preparation method of the refractory castable for the roller casting end cover described in this comparative example 3 is the same as that of Example 1, and the only difference is that the raw material composition of the refractory castable is different. The refractory castable for the roller casting end cover described in this comparative example 3 is composed of the following raw materials in parts by weight: 72 parts of mineral raw materials, 13 parts of α-Al2O3 micropowder, 7 parts of silicon dioxide micropowder, 5.5 parts of titanium carbide modified carbon nanotubes, 1.5 parts of nano zirconium dioxide, 6.5 parts of binder and 4.5 parts of water; wherein the mineral raw material is a mixture of plate-like corundum, magnesium aluminum spinel and pyrope, and the binder is a mixture of magnesium hydrogen phosphate and hydrated alumina.

[0092] Comparative Example 4

[0093] The raw material composition and preparation method of the refractory castable for the roll casting end cover described in this comparative example 4 are the same as those in Example 1, and the only difference is that the binder in the raw material is different from that in Example 1. The binder used in the refractory castable described in this comparative example 4 is calcium aluminate cement CA-50.

[0094] The performance tests were conducted on the refractory castables for roller casting end caps prepared in Examples 1-3 and Comparative Examples 1-4. The results are shown in Table 1 below:

[0095] Table 1 Performance test results of refractory castables of Examples 1-3 and Comparative Examples 1-4

[0096]

[0097] It can be seen from Table 1 that the mechanical properties of the refractory castables prepared in Examples 1-3 are significantly better than those in Comparative Examples 1-4. Compared with Example 1, in Comparative Example 1, no carbon nanotubes modified with titanium carbide are added to the raw materials. Compared with Example 1, in Comparative Example 2, no nano zirconium dioxide is added to the raw materials. Compared with Example 1, in Comparative Example 3, no polyvinyl alcohol fiber and aluminum lactate are added to the raw materials, all of which cause the performance of the prepared refractory castables to decrease. It can be seen that the titanium carbide modified carbon nanotubes, nano zirconium dioxide, polyvinyl alcohol fiber and aluminum lactate in the raw materials are used in combination and synergistically to improve the mechanical properties, anti-burst performance and anti-corrosion performance of the prepared refractory castables. In addition, the binder in Comparative Example 4 is calcium aluminate cement. Since the calcium oxide component in the cement reacts with Al2O3 and SiO2 in the castable at high temperature to form low-melting-point phases such as calcium feldspar and calcium aluminum feldspar, the strength of the refractory castable decreases.

Claims

1. A refractory castable for roller casting end caps, Features: The composition is composed of the following raw materials by weight: 71-73 parts of mineral raw materials, α-Al 2 O 3 12-14 parts of micro powder, 6-8 parts of silicon dioxide micro powder, 5-6 parts of titanium carbide modified carbon nanotubes, 1.4-1.6 parts of nano zirconium dioxide, 0.05-0.07 parts of polyvinyl alcohol fiber, 0.03-0.05 parts of aluminum lactate, 6-7 parts of binder and 4-5 parts of water; wherein the mineral raw material is a mixture of plate-like corundum, magnesium aluminum spinel and pyrope, and the binder is a mixture of magnesium hydrogen phosphate and hydrated alumina; The preparation method of titanium carbide modified carbon nanotubes comprises the following steps: mixing carbon nanotubes, titanium powder and mixed salt, reacting at 1100°C for 3.5 hours under an argon atmosphere, cooling to room temperature with the furnace, and then washing, filtering and drying to prepare titanium carbide modified carbon nanotubes; Wherein: the molar ratio of carbon nanotubes to titanium powder is 1:0.

5.

2. The refractory castable for roller casting end cover according to claim 1, Features: The mass ratio of plate-shaped corundum, magnesium-aluminum spinel and pyroxene in the mineral raw materials is 4-6: 2-5: 5-7.

3. The refractory castable for roller casting end cover according to claim 1, Features: The mineral raw materials, calculated by mass percentage, are composed of 15-18% of granular materials with a particle size of 5mm<≤8mm, 15-18% of granular materials with a particle size of 3mm<≤5mm, 20-24% of granular materials with a particle size of 1mm<≤3mm, 21-24% of granular materials with a particle size of 0.074mm<≤1mm, and 20-24% of powder materials with a particle size of ≤0.074mm.

4. The refractory castable for roller casting end cover according to claim 1, Features: The mass ratio of magnesium hydrogen phosphate to hydrated alumina in the binder is 1:0.45-0.

55.

5. The refractory castable for roller casting end cover according to claim 1, Features: α-Al 2 O 3 The particle size of the micro powder is 2 μm, and the particle size of the silica micro powder is 0.3 μm.

6. The refractory castable for roller casting end cap according to claim 1, Features: In the preparation method of titanium carbide modified carbon nanotubes, the amount of mixed salt added is 8% of the total mass of carbon nanotubes and titanium powder; In the preparation method of titanium carbide modified carbon nanotubes, the mixed salt is a mixture of potassium chloride and lithium chloride, and the molar ratio of potassium chloride to lithium chloride is 59:41; In the preparation method of titanium carbide modified carbon nanotubes, 100° C. boiling water is used for washing, and the carbon nanotubes are filtered and dried at 115° C. for 12.5 hours.

7. A method for preparing a refractory castable for a roll casting end cover according to claim 1, Features: It consists of the following steps: (1) Mineral raw materials, α-Al 2 O 3 Micro powder, silicon dioxide micro powder, titanium carbide modified carbon nanotubes, nano zirconium dioxide, polyvinyl alcohol fiber, aluminum lactate and binder are added into a mixer in proportion and dry mixed; (2) Adding water to the dry mixture obtained in step (1) and mixing again, casting the mixed slurry in a mold, curing, demoulding, and drying to obtain a refractory castable for a roll casting end cover.

8. The method for preparing the refractory castable for roller casting end cover according to claim 7, Features: The curing time in step (2) is 50-52 hours, and the curing temperature is room temperature.

9. The method for preparing a refractory castable for a roll casting end cover according to claim 7, Features: In step (2), the drying temperature is 112-115° C. and the drying time is 13-13.5 h.

Citation Information

Patent Citations

  • Thermal-shock-resistant corundum-spinel refractory castable and preparation method thereof

    CN102718512A

  • Low-aluminum low-heat-conductivity alkali-resistant castable

    CN106830958A

  • Zirconia refractory material and preparation method thereof

    CN112028642A

  • Lightweight spinel-corundum-carbon refractory material and preparation method thereof

    CN112645731A

  • refractory material and its use

    DE102016100810A1