Radar absorbing material with honeycomb structure and processing method thereof
By combining porous absorbing materials with composite printing liquid, 3D printing technology was used to manufacture radar absorbing materials with honeycomb structures, which solved the problems of insufficient absorption and mechanical properties of existing materials, and achieved efficient electromagnetic wave absorption and improved material stability.
Patent Information
- Application Number
- CN202411111466.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-14
AI Technical Summary
Existing radar absorbing materials have poor absorption performance, durability, and mechanical properties.
A combination of porous absorbing material and composite printing liquid was used to prepare a radar absorbing material with a honeycomb structure through 3D printing technology. The porous absorbing material was prepared from boric acid, melamine, γ-aminopropyltriethoxysilane, 2,4-pyridinedicarboxylic acid and N-ethyl-p-toluidine. The composite printing liquid was prepared from 4,4'-diaminodiphenyl ether, 3,4,9,10-perylenetetracarboxylic dianhydride, graphene and ferric chloride, forming a salt solution with a π-conjugated system and a mixed nanomaterial.
This study achieves excellent absorption performance, mechanical properties, and stability of radar absorbing materials, increases the propagation path and attenuation opportunities of electromagnetic waves within the material, and improves the mechanical strength and durability of the material.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of radar absorbing material processing, and in particular relates to a radar absorbing material with a honeycomb structure and a processing method thereof. Background Art
[0002] With the continuous advancement of modern military technology, military equipment such as fighters, missiles, and warships have increasingly stringent requirements for low radar cross-sectional areas. In order to reduce the possibility of being detected by enemy radar systems and improve combat effectiveness and concealment, the development of efficient radar absorbing materials has become the key. Honeycomb structure absorbing materials, with their unique structure and material composition, can effectively absorb electromagnetic waves in a wider frequency band, reduce reflections, and thus significantly reduce the echo intensity of radar signals, becoming a hot topic in military research. In wireless communication systems, problems such as multipath propagation and signal interference often lead to signal attenuation and distortion, affecting communication quality. Honeycomb structure absorbing materials can be used to make absorbing walls, absorbing baffles and other equipment to effectively absorb electromagnetic waves in the surrounding environment, reduce signal reflection and interference, and improve the transmission quality and reliability of communication systems. In addition, in antenna design, honeycomb structure absorbing materials can also be used to make antenna covers to suppress stray radiation from antennas and improve antenna performance and directivity.
[0003] Patent CN 111925684 B discloses a radar absorbing material and a preparation method thereof. The radar absorbing material includes an electromagnetic wave absorber, a resin and a curing agent. The resin includes an epoxy resin and a modified epoxy resin. The modified epoxy resin includes one or more of a rubber-modified epoxy resin, a polyurethane-modified epoxy resin and a polyacrylate-modified epoxy resin. The glass transition temperature (Tg) of the modified epoxy resin is less than -50°C. The radar absorbing material prepared by the invention uses a composite system consisting of a modified epoxy resin with a lower Tg and a traditional epoxy resin as a matrix material of the absorbing coating material. Since the modified epoxy resin has a lower Tg, a two-phase structure is formed after curing. The micro-region formed by the rubber phase has the dual functions of initiating and terminating silver streaks, thereby improving the flexibility of the coating. However, the radar absorbing material prepared by the invention still has room for improvement in terms of electromagnetic wave absorption performance, material durability and mechanical properties. Summary of the invention
[0004] The object of the present invention is to provide a radar absorbing material with a honeycomb structure and a processing method thereof, so as to solve the technical problems of poor absorbing performance, durability and mechanical properties of the absorbing material in the prior art.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The invention provides a radar absorbing material with a honeycomb structure, which is composed of the following components in parts by weight: 8-14 parts of a porous absorbing material, 30-50 parts of a composite printing liquid, and 2-4 parts of a defoaming agent, wherein the porous absorbing material is prepared from boric acid, melamine, γ-aminopropyltriethoxysilane, 2,4-pyridinedicarboxylic acid and N-ethyl-p-toluidine, and the composite printing liquid is prepared from 4,4'-diaminodiphenyl ether, 3,4,9,10-perylenetetracarboxylic dianhydride, graphene, ferric chloride and sodium nitrate.
[0007] Preferably, the method for preparing the porous absorbing material comprises the following steps:
[0008] Q1: Add boric acid and melamine to a container containing ultrapure water, heat and stir, cool to obtain a white precipitate, wash, dry, place in a nitrogen environment, heat, cool to obtain a crude product, heat the crude product to obtain an intermediate product 1;
[0009] Q2: The intermediate product 1 is ultrasonically dispersed in ultrapure water, irradiated under stirring conditions, and washed and dried after the irradiation to obtain the intermediate product 2;
[0010] Q3: γ-aminopropyltriethoxysilane is added to a container containing toluene, and stirred. Subsequently, the intermediate product 2 is added and heated and stirred. After the stirring is completed, the intermediate product 2 is washed and vacuum dried to obtain the intermediate product 3.
[0011] Q4: Disperse 2,4-pyridinedicarboxylic acid in thionyl chloride, heat to reflux, and then distill under reduced pressure to remove the solvent. Dissolve the remaining solid in dichloromethane, add the intermediate product 3 and triethylamine, heat and stir, then add N-ethyl-p-toluidine and 4-dimethylaminopyridine to continue the reaction. After the reaction is completed, wash and vacuum dry to obtain a porous absorbing material.
[0012] In the above process, the synthesis reaction formula of the porous absorbing material is as follows:
[0013]
[0014] Preferably, in Q1, the molar ratio of boric acid to melamine is (0.8-1.2): (0.9-1.2), the heating and stirring temperature is 80-90°C, the stirring time is 10-12h, washed with ultrapure water 3-5 times, the drying temperature is 80-90°C, the time is 10-12h, and the heating treatment process is: first preheated at 300°C for 1h, then heated to 1100°C at a heating rate of 2°C / min, maintained for 2h, then heated to 1460°C at a heating rate of 5°C / min, maintained for 4h, the heating treatment temperature of the crude product is 550-600°C, and the treatment time is 10-12h.
[0015] Preferably, in Q2, the ratio of the intermediate product 1 to ultrapure water is (1.5-3) g: (150-300) mL, and the radiation source is 60 Co γ-ray, irradiation dose rate 60Gy·min -1 , the absorbed dose is 250kGy, nitrous oxide is blown in during the irradiation process, washed with ultrapure water 3-5 times, the drying temperature is 60-70°C, and the time is 10-12h; in Q3, the amount ratio of γ-aminopropyltriethoxysilane, toluene and intermediate product 2 is (240-300)μL: (240-300)mL: (1.2-1.5)g, the stirring time is 10-12min, the heating and stirring temperature is 100-110°C, washed with toluene and ethanol 3-5 times respectively, the vacuum drying temperature is 60-70°C, and the time is 8-10h.
[0016] Preferably, in Q4, the dosage ratio of 2,4-pyridinedicarboxylic acid and thionyl chloride is (0.85-1.7) g: (15-30) mL, the heating reflux temperature is 85-95°C, and the time is 3-5 h. The dosage ratio of the remaining solid, dichloromethane, intermediate product 3, triethylamine, N-ethyl-p-toluidine and 4-dimethylaminopyridine is (0.5-0.7) g: (70-80) mL: (500-700) mg: (5.4-6.2) mL: (1.5-2.3) mL: (35-45) mg. The heating reflux temperature is 80-90°C and the time is 3-5 h. The heating and stirring temperature is 60-70°C and the time is 2-4 h. The reaction is continued for 2-4 h. The product is washed with dichloromethane 3-5 times. The vacuum drying temperature is 60-70°C and the time is 10-12 h.
[0017] Preferably, the method for preparing the composite printing liquid comprises the following steps:
[0018] S1: adding 4,4'-diaminodiphenyl ether, triethylamine and ultrapure water into a container, heating and stirring to react, then adding 3,4,9,10-perylenetetracarboxylic dianhydride and ultrapure water, and continuously stirring to obtain a salt solution;
[0019] S2: adding graphene, ferric chloride and sodium nitrate to ultrapure water, ultrasonically treating to obtain a suspension, transferring the suspension to a reactor, hydrothermally treating, cooling, centrifuging, washing, vacuum drying after the treatment, and then heating the dried substance in a tube furnace to obtain a mixed nanomaterial;
[0020] S3: Add the salt solution to the dispersion bottle, then add the mixed nanomaterials, seal and mix in the dispersion bottle, then punch a hole in the cap of the dispersion bottle, insert a stirring paddle through the cap into the bottle, heat and stir to obtain a composite printing liquid.
[0021] In the above process, 4,4'-diaminodiphenyl ether and 3,4,9,10-perylenetetracarboxylic dianhydride undergo condensation reaction to prepare a salt solution, and then graphene and ferric chloride are used as raw materials to prepare a mixed nanomaterial by a hydrothermal method. After the salt solution and the mixed nanomaterial are mixed, a composite printing liquid is obtained.
[0022] Preferably, in S1, the molar ratio of 4,4'-diaminodiphenyl ether, triethylamine and 3,4,9,10-perylenetetracarboxylic dianhydride is (1-2): (2-4): (1-2), the temperature of the heating and stirring reaction is 80-85°C, the time is 45-60 min, and the stirring time is 1-2 h. In S2, the amount ratio of graphene, ferric chloride, sodium nitrate and ultrapure water is (20-35) mg: (1-2) g: (2-4) g: (75-150) mL, the ultrasonic treatment time is 30-50 min, the hydrothermal treatment temperature is 60-65°C, the time is 10-12 h, the ultrapure water and ethanol are used for washing, the vacuum drying temperature is 60-70°C, the tubular furnace heating temperature is 350-400°C, the heating atmosphere is 40% hydrogen and 60% nitrogen, and the heating time is 2-3 h.
[0023] Preferably, in S3, the amount ratio of the salt solution to the mixed nanomaterial is (40-50) mL: (4-6) g, the mixing conditions are: stirring at 500 rpm for 10 min, stirring at 1000 rpm for 10 min, stirring at 1500 rpm for 10 min, the heating stirring temperature is 80-85°C, and the stirring time is 1-2 h.
[0024] Preferably, the method for processing the radar absorbing material having a honeycomb structure comprises the following steps:
[0025] Step (1): the porous absorbing material and the composite printing liquid are mixed and stirred, and then a defoaming agent is added. After the mixture is evenly mixed, the mixture is placed in a syringe of a printer, and then the syringe is placed on an extrusion frame of a 3D printer to print to obtain a precursor;
[0026] Step (2): placing the precursor in a drying oven, heating it, and cooling it to obtain a radar absorbing material having a honeycomb structure.
[0027] Preferably, in step (1), the nozzle diameter of the syringe is 0.26-0.41 mm, the printing temperature is 40-60°C, and the printing speed is 25-40 mm / s; in step (2), the heating process is: 100°C for 1 hour, 150°C for 1 hour, 200°C for 1 hour, 240°C for 1 hour, 300°C for 1 hour, and 400°C for 1 hour.
[0028] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0029] 1. The present invention first uses boric acid, melamine, γ-aminopropyltriethoxysilane, 2,4-pyridinedicarboxylic acid and N-ethyl-p-toluidine as raw materials to prepare a porous absorbing material, then uses 4,4'-diaminodiphenyl ether, 3,4,9,10-perylenetetracarboxylic dianhydride, graphene and ferric chloride as raw materials to prepare a composite printing liquid, mixes the porous absorbing material with the composite printing liquid, obtains a precursor by a 3D printer, and then obtains a radar absorbing material by heating. The obtained material has excellent absorbing performance, mechanical properties and stability.
[0030] 2. The present invention uses boric acid, melamine, γ-aminopropyltriethoxysilane, 2,4-pyridinedicarboxylic acid and N-ethyl-p-toluidine as raw materials to prepare a porous absorbing material, and adds the porous absorbing material to the radar absorbing material to make it have excellent absorbing performance. The pore structure contained in the porous absorbing material can serve as the multiple reflection and scattering center of electromagnetic waves. When the radar wave is incident on the surface of the material, part of the electromagnetic wave will enter the pore and repeatedly reflect and scatter between the pore walls, thereby increasing the propagation path and attenuation chance of the electromagnetic wave inside the material. In addition, inside the pore, the electromagnetic wave interacts with the material medium, and the electromagnetic energy is converted into heat energy or other forms of energy for dissipation through mechanisms such as dielectric loss and magnetic loss, thereby achieving effective absorption of electromagnetic waves.
[0031] 3. The present invention uses 4,4'-diaminodiphenyl ether, 3,4,9,10-perylenetetracarboxylic dianhydride, graphene and ferric chloride as raw materials to prepare a composite printing liquid, and then uses the composite printing liquid for printing in a 3D printer, so that the obtained radar absorbing material has excellent absorbing performance, durability and mechanical properties. The 4,4'-diaminodiphenyl ether and 3,4,9,10-perylenetetracarboxylic dianhydride in the composite printing liquid react to form a salt solution with a π conjugated system. The π conjugated system can effectively absorb electromagnetic waves and convert electromagnetic wave energy into heat energy through intramolecular electron transfer, thereby achieving absorption and attenuation of electromagnetic waves. The added mixed nanomaterials can form a composite material with both dielectric loss and magnetic loss. The high electrical conductivity and specific surface area of graphene are conducive to the absorption of electromagnetic waves. Iron tetroxide has excellent ferromagnetism and can enhance magnetic loss capacity. At the same time, the high conductivity of the mixed nanomaterials promotes the interaction between electromagnetic waves and the material matrix, thereby enhancing the wave absorption effect. The obtained honeycomb structure not only increases the specific surface area, but also provides more electromagnetic wave scattering and absorption interfaces, thereby increasing the propagation path and attenuation opportunities of electromagnetic waves inside the material. The added graphene can improve the mechanical strength and durability of the material, and prevent the material from being damaged or deformed during use. DETAILED DESCRIPTION
[0032] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Embodiment 1: This embodiment discloses a method for preparing a porous absorbing material, comprising the following steps:
[0034] Q1: 1.25 g of boric acid and 2.68 g of melamine were added to a container containing 250 mL of ultrapure water, heated and stirred at 80°C for 12 h, cooled to obtain a white precipitate, washed with ultrapure water three times, dried at 85°C for 12 h, placed in a nitrogen environment, first preheated at 300°C for 1 h, then heated to 1100°C at a heating rate of 2°C / min, maintained for 2 h, then heated to 1460°C at a heating rate of 5°C / min, maintained for 4 h, and after the heating treatment, cooled to obtain a crude product, and the crude product was heated at 550°C for 12 h to obtain intermediate product 1;
[0035] Q2: 2.25 g of intermediate product 1 was ultrasonically dispersed in 225 mL of ultrapure water and irradiated under stirring. The radiation source was 60 Co γ-ray, irradiation dose rate 60Gy·min -1 The absorbed dose was 250 kGy, nitrous oxide was blown into the irradiation process, and after the irradiation, it was washed with ultrapure water for 5 times and dried at 70 °C for 12 h to obtain the intermediate product 2;
[0036] Q3: Add 270 μL of γ-aminopropyltriethoxysilane to a container containing 270 mL of toluene and stir. Then, add 1.35 g of intermediate product 2 and heat and stir at 110°C for 12 min. After stirring, wash with toluene and ethanol for 5 times, respectively, and dry under vacuum at 70°C for 10 h to obtain intermediate product 3.
[0037] Q4: 1.24 g of 2,4-pyridinedicarboxylic acid was dispersed in 22.5 mL of thionyl chloride, heated to reflux at 85 °C for 3 h, and then the solvent was distilled off under reduced pressure. 0.6 g of the remaining solid was dissolved in 75 mL of dichloromethane, and then 600 mg of intermediate product 3 and 5.8 mL of triethylamine were added. The mixture was heated and stirred at 70 °C for 4 h, and then 1.9 mL of N-ethyl-p-toluidine and 40 mg of 4-dimethylaminopyridine were added to continue the reaction for 3 h. After the reaction was completed, the mixture was washed with dichloromethane three times and dried in vacuo at 65 °C for 12 h to obtain a porous absorbing material.
[0038] This embodiment discloses a method for preparing a composite printing liquid, comprising the following steps:
[0039] S1: 1.5 g of 4,4'-diaminodiphenyl ether, 1.52 g of triethylamine and 50 mL of ultrapure water were added to a container, the temperature was raised to 85°C and stirred for 60 min, then 2.94 g of 3,4,9,10-perylenetetracarboxylic dianhydride and 8.5 mL of ultrapure water were added, and stirring was continued for 2 h to obtain a salt solution;
[0040] S2: 27.5 mg of graphene, 1.5 g of ferric chloride and 3 g of sodium nitrate were added to 112.5 mL of ultrapure water, and ultrasonic treatment was performed for 50 min to obtain a suspension, which was transferred to a reactor and hydrothermally treated at 65 ° C for 12 h. After the treatment, the suspension was cooled, centrifuged, washed with ultrapure water and ethanol, and vacuum dried at 65 ° C. The dried substance was then placed in a tubular furnace at 400 ° C and heated for 3 h in a heating atmosphere of 40% hydrogen and 60% nitrogen to obtain a mixed nanomaterial;
[0041] S3: Add 45 mL of salt solution to the dispersion bottle, then add 5 g of mixed nanomaterials, seal it and place it in the dispersant bottle for mixing, stir at 500 rpm for 10 min, stir at 1000 rpm for 10 min, stir at 1500 rpm for 10 min, then punch a hole in the cap of the dispersion bottle, put a stirring paddle through the cap and into the bottle, stir at 85 ° C for 2 h to obtain a composite printing liquid.
[0042] The present embodiment discloses a radar absorbing material with a honeycomb structure, which is composed of the following components in parts by weight: 11 parts of porous absorbing material, 40 parts of composite printing liquid, and 3 parts of defoaming agent.
[0043] This embodiment discloses a method for processing a radar absorbing material having a honeycomb structure, comprising the following steps:
[0044] Step (1): the porous absorbing material and the composite printing liquid are mixed and stirred, and then a defoaming agent is added. After the mixture is evenly mixed, it is placed in a syringe of a printer. The nozzle diameter of the syringe is 0.26 mm, the printing temperature is 40° C., and the printing speed is 25 mm / s. Then, the syringe is placed in an extrusion rack of a 3D printer to print to obtain a precursor;
[0045] Step (2): placing the precursor in a drying oven, heating it at 100°C for 1 hour, 150°C for 1 hour, 200°C for 1 hour, 240°C for 1 hour, 300°C for 1 hour, and 400°C for 1 hour, and cooling it to obtain a radar absorbing material with a honeycomb structure.
[0046] Embodiment 2: This embodiment discloses a method for preparing a porous absorbing material, comprising the following steps:
[0047] Q1: Add 1g of boric acid and 2.29g of melamine to a container containing 250mL of ultrapure water, heat and stir at 80°C for 12h, cool to obtain a white precipitate, wash with ultrapure water three times, dry at 85°C for 12h, place in a nitrogen environment, first preheat at 300°C for 1h, then heat to 1100°C at a heating rate of 2°C / min, hold for 2h, then heat to 1460°C at a heating rate of 5°C / min, hold for 4h, after heating treatment, cool to obtain a crude product, heat the crude product at 550°C for 12h to obtain intermediate product 1;
[0048] Q2: 1.5 g of intermediate product 1 was ultrasonically dispersed in 150 mL of ultrapure water and irradiated under stirring. The radiation source was 60 Co γ-ray, irradiation dose rate 60Gy·min -1 The absorbed dose was 250 kGy, nitrous oxide was blown into the irradiation process, and after the irradiation, it was washed with ultrapure water for 5 times and dried at 70 °C for 12 h to obtain the intermediate product 2;
[0049] Q3: Add 240 μL of γ-aminopropyltriethoxysilane to a container containing 300 mL of toluene and stir. Then, add 1.2 g of intermediate product 2 and heat and stir at 110°C for 12 min. After stirring, wash with toluene and ethanol for 5 times respectively, and dry under vacuum at 70°C for 10 h to obtain intermediate product 3.
[0050] Q4: Disperse 0.85 g of 2,4-pyridinedicarboxylic acid in 15 mL of thionyl chloride, heat under reflux at 85 °C for 3 h, remove the solvent by distillation under reduced pressure, dissolve 0.5 g of the remaining solid in 70 mL of dichloromethane, add 500 mg of intermediate 3 and 5.4 mL of triethylamine, heat and stir at 70 °C for 4 h, then add 1.5 mL of N-ethyl-p-toluidine and 35 mg of 4-dimethylaminopyridine and continue the reaction for 3 h. After the reaction is completed, wash with dichloromethane three times and dry under vacuum at 65 °C for 12 h to obtain a porous absorbing material.
[0051] This embodiment discloses a method for preparing a composite printing liquid, comprising the following steps:
[0052] S1: 1 g of 4,4'-diaminodiphenyl ether, 1.01 g of triethylamine and 50 mL of ultrapure water were added to a container, the temperature was raised to 85°C and stirred for 60 min, then 1.96 g of 3,4,9,10-perylenetetracarboxylic dianhydride and 8.5 mL of ultrapure water were added, and the mixture was stirred for 2 h to obtain a salt solution;
[0053] S2: 20 mg of graphene, 1 g of ferric chloride and 2 g of sodium nitrate were added to 75 mL of ultrapure water, and ultrasonic treatment was performed for 50 min to obtain a suspension, and the suspension was transferred to a reactor and hydrothermally treated at 65 ° C for 12 h. After the treatment, it was cooled, centrifuged, washed with ultrapure water and ethanol, and vacuum dried at 65 ° C. The dried material was then placed in a tubular furnace at 400 ° C and heated for 3 h. The heating atmosphere was 40% hydrogen and 60% nitrogen to obtain a mixed nanomaterial;
[0054] S3: Add 40 mL of salt solution to the dispersion bottle, then add 4 g of mixed nanomaterials, seal and mix in the dispersion bottle, stir at 500 rpm for 10 min, stir at 1000 rpm for 10 min, stir at 1500 rpm for 10 min, then punch a hole in the cap of the dispersion bottle, put a stirring paddle through the cap and into the bottle, stir at 85 ° C for 2 h to obtain a composite printing liquid.
[0055] The present embodiment discloses a radar absorbing material with a honeycomb structure, which is composed of the following components in parts by weight: 8 parts of porous absorbing material, 30 parts of composite printing liquid, and 2 parts of defoaming agent.
[0056] This embodiment discloses a method for processing a radar absorbing material having a honeycomb structure, comprising the following steps:
[0057] Step (1): the porous absorbing material and the composite printing liquid are mixed and stirred, and then a defoaming agent is added. After the mixture is evenly mixed, it is placed in a syringe of a printer. The nozzle diameter of the syringe is 0.26 mm, the printing temperature is 40° C., and the printing speed is 25 mm / s. Then, the syringe is placed in an extrusion rack of a 3D printer to print to obtain a precursor;
[0058] Step (2): placing the precursor in a drying oven, heating it at 100°C for 1 hour, 150°C for 1 hour, 200°C for 1 hour, 240°C for 1 hour, 300°C for 1 hour, and 400°C for 1 hour, and cooling it to obtain a radar absorbing material with a honeycomb structure.
[0059] Embodiment 3: This embodiment discloses a method for preparing a porous absorbing material, comprising the following steps:
[0060] Q1: 1.5 g of boric acid and 3.06 g of melamine were added to a container containing 250 mL of ultrapure water, heated and stirred at 80°C for 12 h, cooled to obtain a white precipitate, washed with ultrapure water three times, dried at 85°C for 12 h, placed in a nitrogen environment, first preheated at 300°C for 1 h, then heated to 1100°C at a heating rate of 2°C / min, maintained for 2 h, then heated to 1460°C at a heating rate of 5°C / min, maintained for 4 h, and after the heating treatment, cooled to obtain a crude product, and the crude product was heated at 550°C for 12 h to obtain intermediate product 1;
[0061] Q2: 3 g of intermediate product 1 was ultrasonically dispersed in 300 mL of ultrapure water and irradiated under stirring. The radiation source was 60 Co γ-ray, irradiation dose rate 60Gy·min -1 The absorbed dose was 250 kGy, nitrous oxide was blown into the irradiation process, and after the irradiation, it was washed with ultrapure water for 5 times and dried at 70 °C for 12 h to obtain the intermediate product 2;
[0062] Q3: Add 300 μL of γ-aminopropyltriethoxysilane to a container containing 240 mL of toluene and stir. Then, add 1.5 g of intermediate product 2 and heat and stir at 110°C for 12 min. After stirring, wash with toluene and ethanol for 5 times, respectively, and dry under vacuum at 70°C for 10 h to obtain intermediate product 3.
[0063] Q4: Disperse 1.7 g of 2,4-pyridinedicarboxylic acid in 30 mL of thionyl chloride, heat under reflux at 85 °C for 3 h, remove the solvent by distillation under reduced pressure, dissolve 0.7 g of the remaining solid in 80 mL of dichloromethane, add 700 mg of intermediate 3 and 6.2 mL of triethylamine, heat and stir at 70 °C for 4 h, then add 2.3 mL of N-ethyl-p-toluidine and 45 mg of 4-dimethylaminopyridine and continue the reaction for 3 h. After the reaction is completed, wash with dichloromethane three times and dry under vacuum at 65 °C for 12 h to obtain a porous absorbing material.
[0064] This embodiment discloses a method for preparing a composite printing liquid, comprising the following steps:
[0065] S1: 2 g of 4,4'-diaminodiphenyl ether, 2.02 g of triethylamine and 50 mL of ultrapure water were added to a container, the temperature was raised to 85°C and stirred for 60 min, then 3.92 g of 3,4,9,10-perylenetetracarboxylic dianhydride and 8.5 mL of ultrapure water were added, and the mixture was stirred for 2 h to obtain a salt solution;
[0066] S2: 35 mg of graphene, 2 g of ferric chloride and 4 g of sodium nitrate were added to 150 mL of ultrapure water, and ultrasonic treatment was performed for 50 min to obtain a suspension, and the suspension was transferred to a reactor and hydrothermally treated at 65 ° C for 12 h. After the treatment, it was cooled, centrifuged, washed with ultrapure water and ethanol, and vacuum dried at 65 ° C. The dried material was then placed in a 400 ° C tubular furnace and heated for 3 h. The heating atmosphere was 40% hydrogen and 60% nitrogen to obtain a mixed nanomaterial;
[0067] S3: Add 50 mL of salt solution to the dispersion bottle, then add 6 g of mixed nanomaterials, seal and mix in the dispersion bottle, stir at 500 rpm for 10 min, stir at 1000 rpm for 10 min, stir at 1500 rpm for 10 min, then punch a hole in the cap of the dispersion bottle, put a stirring paddle through the cap and into the bottle, stir at 85 ° C for 2 h to obtain a composite printing liquid.
[0068] The present embodiment discloses a radar absorbing material with a honeycomb structure, which is composed of the following components in parts by weight: 14 parts of porous absorbing material, 50 parts of composite printing liquid, and 4 parts of defoaming agent.
[0069] This embodiment discloses a method for processing a radar absorbing material having a honeycomb structure, comprising the following steps:
[0070] Step (1): the porous absorbing material and the composite printing liquid are mixed and stirred, and then a defoaming agent is added. After the mixture is evenly mixed, it is placed in a syringe of a printer. The nozzle diameter of the syringe is 0.26 mm, the printing temperature is 40° C., and the printing speed is 25 mm / s. Then, the syringe is placed in an extrusion rack of a 3D printer to print to obtain a precursor;
[0071] Step (2): placing the precursor in a drying oven, heating it at 100°C for 1 hour, 150°C for 1 hour, 200°C for 1 hour, 240°C for 1 hour, 300°C for 1 hour, and 400°C for 1 hour, and cooling it to obtain a radar absorbing material with a honeycomb structure.
[0072] Embodiment 4: This embodiment discloses a method for preparing a porous absorbing material, comprising the following steps:
[0073] Q1: 1.15 g of boric acid and 2.47 g of melamine were added to a container containing 250 mL of ultrapure water, heated and stirred at 80°C for 12 h, cooled to obtain a white precipitate, washed with ultrapure water three times, dried at 85°C for 12 h, placed in a nitrogen environment, first preheated at 300°C for 1 h, then heated to 1100°C at a heating rate of 2°C / min, maintained for 2 h, then heated to 1460°C at a heating rate of 5°C / min, maintained for 4 h, and after the heating treatment, cooled to obtain a crude product, and the crude product was heated at 550°C for 12 h to obtain an intermediate product 1;
[0074] Q2: 2.5 g of intermediate product 1 was ultrasonically dispersed in 200 mL of ultrapure water and irradiated under stirring. The radiation source was 60 Co γ-ray, irradiation dose rate 60Gy·min -1 The absorbed dose was 250 kGy, nitrous oxide was blown into the irradiation process, and after the irradiation, it was washed with ultrapure water for 5 times and dried at 70 °C for 12 h to obtain the intermediate product 2;
[0075] Q3: Add 290 μL of γ-aminopropyltriethoxysilane to a container containing 250 mL of toluene and stir. Then, add 1.3 g of intermediate product 2 and heat and stir at 110°C for 12 min. After stirring, wash with toluene and ethanol for 5 times, respectively, and dry under vacuum at 70°C for 10 h to obtain intermediate product 3.
[0076] Q4: 1.05 g of 2,4-pyridinedicarboxylic acid was dispersed in 25 mL of thionyl chloride, heated under reflux at 85 °C for 3 h, and then the solvent was removed by distillation under reduced pressure. 0.55 g of the remaining solid was dissolved in 72 mL of dichloromethane, and then 560 mg of intermediate 3 and 5.6 mL of triethylamine were added. The mixture was heated and stirred at 70 °C for 4 h, and then 1.7 mL of N-ethyl-p-toluidine and 38 mg of 4-dimethylaminopyridine were added and the reaction continued for 3 h. After the reaction was completed, the mixture was washed with dichloromethane three times and dried under vacuum at 65 °C for 12 h to obtain a porous absorbing material.
[0077] This embodiment discloses a method for preparing a composite printing liquid, comprising the following steps:
[0078] S1: 1.2 g of 4,4'-diaminodiphenyl ether, 1.28 g of triethylamine and 50 mL of ultrapure water were added to a container, the temperature was raised to 85°C and stirred for 60 min, then 2.45 g of 3,4,9,10-perylenetetracarboxylic dianhydride and 8.5 mL of ultrapure water were added, and the mixture was stirred for 2 h to obtain a salt solution;
[0079] S2: 25 mg of graphene, 1.2 g of ferric chloride and 3.5 g of sodium nitrate were added to 89.3 mL of ultrapure water, and ultrasonic treatment was performed for 50 min to obtain a suspension, which was transferred to a reactor and hydrothermally treated at 65 ° C for 12 h. After the treatment, the suspension was cooled, centrifuged, washed with ultrapure water and ethanol, and vacuum dried at 65 ° C. The dried substance was then placed in a tubular furnace at 400 ° C and heated for 3 h in a heating atmosphere of 40% hydrogen and 60% nitrogen to obtain a mixed nanomaterial;
[0080] S3: Add 42 mL of salt solution to the dispersion bottle, then add 4.5 g of mixed nanomaterials, seal and place in a dispersant bottle for mixing, stir at 500 rpm for 10 min, stir at 1000 rpm for 10 min, stir at 1500 rpm for 10 min, then punch a hole in the cap of the dispersion bottle, put a stirring paddle through the cap and into the bottle, stir at 85 ° C for 2 h to obtain a composite printing liquid.
[0081] The present embodiment discloses a radar absorbing material with a honeycomb structure, which is composed of the following components in parts by weight: 10 parts of porous absorbing material, 35 parts of composite printing liquid, and 2.5 parts of defoaming agent.
[0082] This embodiment discloses a method for processing a radar absorbing material having a honeycomb structure, comprising the following steps:
[0083] Step (1): the porous absorbing material and the composite printing liquid are mixed and stirred, and then a defoaming agent is added. After the mixture is evenly mixed, it is placed in a syringe of a printer. The nozzle diameter of the syringe is 0.26 mm, the printing temperature is 40° C., and the printing speed is 25 mm / s. Then, the syringe is placed in an extrusion rack of a 3D printer to print to obtain a precursor;
[0084] Step (2): placing the precursor in a drying oven, heating it at 100°C for 1 hour, 150°C for 1 hour, 200°C for 1 hour, 240°C for 1 hour, 300°C for 1 hour, and 400°C for 1 hour, and cooling it to obtain a radar absorbing material with a honeycomb structure.
[0085] Comparative Example 1: Compared with Example 1, in the process of preparing the porous absorbing material in Comparative Example 1, melamine is not added, and other conditions remain unchanged.
[0086] Comparative Example 2: Compared with Example 1, in the process of preparing the porous absorbing material in Comparative Example 2, no γ-aminopropyltriethoxysilane is added, and other conditions remain unchanged.
[0087] Comparative Example 3: Compared with Example 1, in the process of preparing the composite printing liquid in Comparative Example 3, 4,4'-diaminodiphenyl ether is not added, and other conditions remain unchanged.
[0088] Comparative Example 4: Compared with Example 1, in Comparative Example 4, during the preparation of the composite printing liquid, no ferric chloride was added, and other conditions remained unchanged.
[0089] Comparative Example 5: Compared with Example 1, in the process of preparing the radar absorbing material in Comparative Example 5, no porous absorbing material is added, and other conditions remain unchanged.
[0090] Comparative Example 6: Compared with Example 1, in the process of preparing the radar absorbing material in Comparative Example 6, the composite printing liquid is replaced by a saline solution, and other conditions remain unchanged.
[0091] The radar absorbing materials prepared in Examples 1-4 and Comparative Examples 1-6 were subjected to performance tests. The out-of-plane compression performance of the samples was measured using a universal testing machine. In the displacement control mode, the samples were compressed at a speed of 2 mm / min until they were destroyed. The durability of the samples was tested according to FZ / T 50047-2019. The samples were soaked in acid solution and the absorbing performance of the samples was tested according to GB / T 30142-2013. The test results are shown in Table 1:
[0092] Table 1
[0093] project Compression strength / MPa Fracture strength reduction rate / % Shielding effectiveness / dB Example 1 39.7 4.6 24 Example 2 39.4 4.8 23 Example 3 39.2 5.1 23 Example 4 39.1 5.0 22 Comparative Example 1 39.0 5.2. 18 Comparative Example 2 38.9 5.1 17 Comparative Example 3 34.6 7.9. 18 Comparative Example 4 34.8 7.7 16 Comparative Example 5 38.6 5.3 14 Comparative Example 6 34.0 8.2 14
[0094] It can be seen from the test results in Table 1 that the radar absorbing materials prepared in Examples 1-4 of the present invention have excellent mechanical properties, durability and absorbing properties. Shielding effectiveness refers to the ratio of the electric field intensity, magnetic field intensity or power measured with and without shielding material at a certain point under the same excitation. The larger the shielding effectiveness value, the stronger the attenuation ability of the material or structure to electromagnetic waves, that is, the better the shielding effect. From the comparison between comparative example 1 and embodiments 1-4, it can be seen that the addition of melamine can make the radar absorbing material have excellent absorbing performance; from the comparison between comparative example 2 and embodiments 1-4, it can be seen that the addition of γ-aminopropyltriethoxysilane can make the radar absorbing material have excellent absorbing performance; from the comparison between comparative example 3 and embodiments 1-4, it can be seen that the addition of 4,4'-diaminodiphenyl ether can make the radar absorbing material have excellent mechanical properties, durability and absorbing performance; from the comparison between comparative example 4 and embodiments 1-4, it can be seen that the addition of ferric chloride can make the radar absorbing material have excellent mechanical properties, durability and absorbing performance; from the comparison between comparative example 5 and embodiments 1-4, it can be seen that the addition of porous absorbing material can make the radar absorbing material have excellent absorbing performance; from the comparison between comparative example 6 and embodiments 1-4, it can be seen that the use of composite printing liquid can make the radar absorbing material have excellent mechanical properties, durability and absorbing performance.
[0095] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
[0096] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. Radar absorbing material with honeycomb structure, It is characterized in that The invention is composed of the following components in parts by weight: 8-14 parts of porous absorbing material, 30-50 parts of composite printing liquid, and 2-4 parts of defoaming agent, wherein the porous absorbing material is prepared from boric acid, melamine, γ-aminopropyltriethoxysilane, 2,4-pyridinedicarboxylic acid and N-ethyl-p-toluidine, and the composite printing liquid is prepared from 4,4'-diaminodiphenyl ether, 3,4,9,10-perylenetetracarboxylic dianhydride, graphene, ferric chloride and sodium nitrate. The preparation method of the porous absorbing material comprises the following steps: Q1: Add boric acid and melamine to a container containing ultrapure water, heat and stir, cool to obtain a white precipitate, wash, dry, place in a nitrogen environment, heat, cool to obtain a crude product, heat the crude product to obtain an intermediate product 1; Q2: The intermediate product 1 is ultrasonically dispersed in ultrapure water, irradiated under stirring conditions, and washed and dried after the irradiation to obtain the intermediate product 2; Q3: γ-aminopropyltriethoxysilane is added to a container containing toluene, and stirred. Subsequently, the intermediate product 2 is added and heated and stirred. After the stirring is completed, the intermediate product 2 is washed and vacuum dried to obtain the intermediate product 3. Q4: 2,4-pyridinedicarboxylic acid is dispersed in thionyl chloride, heated to reflux, and the solvent is removed by vacuum distillation. The remaining solid is dissolved in dichloromethane, and then the intermediate product 3 and triethylamine are added, heated and stirred, and then N-ethyl-p-toluidine and 4-dimethylaminopyridine are added to continue the reaction. After the reaction is completed, the porous absorbing material is washed and vacuum dried to obtain a porous absorbing material; The method for preparing the composite printing liquid comprises the following steps: S1: adding 4,4'-diaminodiphenyl ether, triethylamine and ultrapure water into a container, heating and stirring to react, then adding 3,4,9,10-perylenetetracarboxylic dianhydride and ultrapure water, and continuously stirring to obtain a salt solution; S2: adding graphene, ferric chloride and sodium nitrate to ultrapure water, ultrasonically treating to obtain a suspension, transferring the suspension to a reactor, hydrothermally treating, cooling, centrifuging, washing, vacuum drying after the treatment, and then heating the dried substance in a tube furnace to obtain a mixed nanomaterial; S3: Add the salt solution to the dispersion bottle, then add the mixed nanomaterials, seal and mix in the dispersion bottle, then punch a hole in the cap of the dispersion bottle, insert a stirring paddle through the cap into the bottle, heat and stir to obtain a composite printing liquid.
2. The radar absorbing material having a honeycomb structure according to claim 1, It is characterized in that In the Q1, the molar ratio of boric acid to melamine is (0.8-1.2): (0.9-1.2), the heating and stirring temperature is 80-90°C, the stirring time is 10-12h, and it is washed with ultrapure water 3-5 times. The drying temperature is 80-90°C for 10-12h. The heating treatment process is: first preheating at 300°C for 1h, then heating to 1100°C at a heating rate of 2°C / min, maintaining for 2h, and then heating to 1460°C at a heating rate of 5°C / min, maintaining for 4h. The heating treatment temperature of the crude product is 550-600°C, and the treatment time is 10-12h.
3. The radar absorbing material having a honeycomb structure according to claim 1, It is characterized in that In Q2, the ratio of the intermediate product 1 to ultrapure water is (1.5-3) g: (150-300) mL, and the radiation source is 60 Co γ-ray, irradiation dose rate 60Gy·min -1 , the absorbed dose is 250kGy, nitrous oxide is blown in during the irradiation process, washed with ultrapure water 3-5 times, the drying temperature is 60-70°C, and the time is 10-12h; in Q3, the amount ratio of γ-aminopropyltriethoxysilane, toluene and intermediate product 2 is (240-300)μL: (240-300)mL: (1.2-1.5)g, the stirring time is 10-12min, the heating and stirring temperature is 100-110°C, washed with toluene and ethanol 3-5 times respectively, the vacuum drying temperature is 60-70°C, and the time is 8-10h.
4. The radar absorbing material having a honeycomb structure according to claim 1, It is characterized in that In the Q4, the dosage ratio of 2,4-pyridinedicarboxylic acid and thionyl chloride is (0.85-1.7) g: (15-30) mL, the heating reflux temperature is 85-95°C, and the time is 3-5 h. The dosage ratio of the remaining solid, dichloromethane, intermediate 3, triethylamine, N-ethyl-p-toluidine and 4-dimethylaminopyridine is (0.5-0.7) g: (70-80) mL: (500-700) mg: (5.4-6.2) mL: (1.5-2.3) mL: (35-45) mg. The heating reflux temperature is 80-90°C and the time is 3-5 h. The heating and stirring temperature is 60-70°C and the time is 2-4 h. The reaction is continued for 2-4 h. The product is washed with dichloromethane 3-5 times. The vacuum drying temperature is 60-70°C and the time is 10-12 h.
5. The radar absorbing material having a honeycomb structure according to claim 1, It is characterized in that In the S1, the molar ratio of 4,4'-diaminodiphenyl ether, triethylamine and 3,4,9,10-perylenetetracarboxylic dianhydride is (1-2): (2-4): (1-2), the temperature of the heating and stirring reaction is 80-85°C, the time is 45-60 minutes, and the stirring time is 1-2 hours. In the S2, the amount ratio of graphene, ferric chloride, sodium nitrate and ultrapure water is (20-35) mg: (1-2) g: (2-4) g: (75-150) mL, the ultrasonic treatment time is 30-50 minutes, the hydrothermal treatment temperature is 60-65°C, the time is 10-12 hours, the ultrapure water and ethanol are used for washing, the vacuum drying temperature is 60-70°C, the tubular furnace heating temperature is 350-400°C, the heating atmosphere is 40% hydrogen and 60% nitrogen, and the heating time is 2-3 hours.
6. The radar absorbing material having a honeycomb structure according to claim 1, It is characterized in that In the S3, the amount ratio of the salt solution and the mixed nanomaterial is (40-50) mL: (4-6) g, and the mixing conditions are: stirring at 500 rpm for 10 min, stirring at 1000 rpm for 10 min, and stirring at 1500 rpm for 10 min. The heating stirring temperature is 80-85° C. and the stirring time is 1-2 h.
7. A method for processing a radar absorbing material having a honeycomb structure according to any one of claims 1 to 6, It is characterized in that The following steps are involved: Step (1): the porous absorbing material and the composite printing liquid are mixed and stirred, and then a defoaming agent is added. After the mixture is evenly mixed, the mixture is placed in a syringe of a printer, and then the syringe is placed on an extrusion frame of a 3D printer to print to obtain a precursor; Step (2): placing the precursor in a drying oven, heating it, and cooling it to obtain a radar absorbing material having a honeycomb structure.
8. The method for processing the radar absorbing material having a honeycomb structure according to claim 7, It is characterized in that In the step (1), the nozzle diameter of the syringe is 0.26-0.41 mm, the printing temperature is 40-60° C., and the printing speed is 25-40 mm / s; in the step (2), the heating process is: 100° C. for 1 hour, 150° C. for 1 hour, 200° C. for 1 hour, 240° C. for 1 hour, 300° C. for 1 hour, and 400° C. for 1 hour.
Citation Information
Patent Citations
Radar wave-absorbing material and preparation method
CN111925684A
Three-dimensional (3D) printing
CN108883577A
Preparation method of BN / C micro-nano-composite wave-absorbing material based on melamine
CN109320247A
Preparation process of BCN / FexOy@Cf / C composite structure wave-absorbing material
CN113979766A
Heat-conducting wave-absorbing auxiliary agent, low-temperature curing coating, heavy corrosion-resistant coating, and preparation method therefor and use thereof
WO2024149031A1