Composite membrane and its preparation method and application
By coating a composite film containing phase change material and conductive network on invisible equipment or devices, the problem of icing in a single function of wave absorbing materials and low temperature environment is solved, and efficient deicing and electromagnetic shielding effects are achieved, reducing costs and maintenance requirements.
Patent Information
- Application Number
- CN202411111418.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-14
AI Technical Summary
The existing wave absorbing materials have single functions, inconvenient use and high cost. Invisible equipment or devices are prone to freezing in low temperature environments, affecting normal operation and radar stealth performance.
Using a composite film, which includes fiber material, magnetic material, conductive material, matrix material, phase change material and curing agent, the adhesion of ice is reduced by precipitation of phase change material and forms a conductive network to absorb electromagnetic waves to achieve deicing and electromagnetic shielding effect.
This composite film has good wave absorption performance and deicing effect, which reduces the adhesion of ice and improves the deicing performance. The raw material cost is relatively low. It is suitable for temperature range from -50 ℃ to 200 ℃ and is suitable for invisible Radar stealth and deicing applications for stealth equipment such as aircraft.
Smart Images

Figure CN118638424B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of wave absorbing materials, and in particular, relates to a composite film and a preparation method and application thereof. Background Art
[0002] For some stealth equipment or devices, such as stealth aircraft, radar stealth performance has become an important indicator of stealth aircraft performance. It is not possible to further increase its radar stealth performance through appearance design, that is, to reduce the radar cross-section (RCS). The rapid iteration and upgrade of radar technology at this stage has further enhanced its ability to detect, search and warn monitoring targets, making the detected targets invisible. Although absorbing materials have made certain progress at this stage, they still have problems such as single function, inconvenient use and high cost.
[0003] Some stealth equipment or devices need to operate in low-temperature environments such as ice and snow, which will affect the normal operation or operation of the stealth equipment or devices, and even cause damage to the components of the equipment or devices. If the outside of the equipment or devices is frozen, the de-icing cost will be increased. Take stealth aircraft as an example. Stealth aircraft fly at a high speed and are in a changeable space environment. When the aircraft is affected by ice and snow, the aerodynamic resistance and weight of the fighter will increase, resulting in a decrease in flight performance. In addition, ice and snow may also cause damage to the aircraft's engines, sensors and other equipment, affecting the normal operation of the aircraft. These factors will not only increase maintenance costs, but also reduce the reliability and execution of the aircraft.
[0004] Increasing the radar stealth performance of an aircraft can weaken the radar echo signal and reduce the probability of being detected. Especially in combat, having stealth performance can make it easier for fighters to break through the opponent's air defense network, break through the enemy's defense line, carry out air strikes, and strike key enemy targets without being detected. Summary of the invention
[0005] The purpose of the present application is to provide a composite film and a preparation method and application thereof, aiming to solve the problem of single function existing in some absorbing materials.
[0006] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:
[0007] In a first aspect, the present application provides a composite film, which comprises the following components in percentage by weight, based on the total weight of the composite film being 100%:
[0008] Fiber materials, 0%-10%;
[0009] Magnetic materials, 20%-40%;
[0010] Conductive materials, 5%-15%;
[0011] Base material, 30%-60%;
[0012] Curing agent, 1%-15%;
[0013] Phase change materials, 3%-20%;
[0014] The phase change material complies with the requirement that it is precipitated from a matrix material under a condition higher than its own melting temperature.
[0015] The composite membrane provided by the present application has good wave absorption performance, and at the same time has the function of reducing ice formation and improving deicing effect, and the raw material cost is relatively low. The composite membrane provided by the present application has a wide working temperature range: -50 ℃-200 ℃. The composite membrane provided by the present application reduces the adhesion of ice by the precipitation of internal phase change materials, thereby achieving the effect of reducing the possibility of ice formation and improving deicing performance. The electromagnetic waves are attenuated by the conductive network composed of magnetic materials, conductive materials and fiber materials.
[0016] In a second aspect, the present application provides a method for preparing a composite membrane, comprising:
[0017] Provide the component raw materials of the above composite membrane:
[0018] The fiber material, the magnetic material, the conductive material, the matrix material, the phase change material and the curing agent are mixed and then cured to obtain the composite film.
[0019] The present application provides a method for preparing a composite film, obtaining a composite material with a conductive network structure and a phase change material uniformly dispersed in a matrix material, ensuring the uniformity and stability of the composite film, and the prepared composite film has good electromagnetic shielding performance and deicing performance. In addition, the preparation method is relatively simple and the raw material cost is low.
[0020] In a third aspect, the composite film and / or the composite film prepared by the preparation method is used as an electromagnetic shielding material and / or as an anti-icing and de-icing material.
[0021] The composite film provided in the present application can be directly coated on sensitive parts of stealth aircraft through a brush coating process, achieving the dual effects of active deicing and reducing radar scattering interface, and the construction process is simple. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0023] Figure 1 It is Fe provided in the embodiment of the present application 3 O 4 Flow chart of the nanoparticle preparation process.
[0024] Figure 2 It is Fe provided in the embodiment of the present application 3 O 4 SEM images of nanoparticles; Figure 2 a in the middle represents the SEM image with a scale of 1 μm; Figure 2 (b) shows the SEM image with a scale bar of 50 nm.
[0025] Figure 3 It is Fe provided in the embodiment of the present application 3 O 4 @rGO / CF / PDMS / 10%Paraffin composite film and paraffin precipitation in graphite; Figure 3 a in the middle represents the composite membrane diagram; Figure 3 Figure b shows the paraffin precipitation diagram in the composite film.
[0026] Figure 4 It is Fe provided in the embodiment of the present application 3 O 4 @Electromagnetic parameters of rGO / CF / PDMS / 10%Paraffin composite membrane; Figure 4 In Chinese: “Frequency” means frequency, and its unit is GHz; Figure 4 a represents the curve of the relationship between the real part of the complex dielectric constant ε' and the frequency; Figure 4 b in the figure represents the curve of the relationship between the imaginary part of the complex dielectric constant ε'' and the frequency; Figure 4 c represents the relationship between the real part of complex magnetic permeability µ' and the frequency; Figure 4 In the figure d, it represents the curve of the relationship between the imaginary part of complex magnetic permeability µ'' and the frequency.
[0027] Figure 5 It is Fe provided in the embodiment of the present application 3 O 4 @The effective absorption bandwidth of rGO / CF / PDMS / 10%Paraffin composite film in the 2 GHz-18 GHz frequency band (RL≤-10 dB means 90% of electromagnetic waves are absorbed); Figure 5 In: "Frequency" means frequency, the unit is GHz; "Reflection Loss" means reflection loss, the unit is dB.
[0028] Figure 6 It is Fe provided in the embodiment of the present application 3 O 4@rGO / CF / PDMS / 0-20%Paraffin composite membrane deicing effect diagram; Figure 6 Chinese: "Ice adhesion strength" refers to the adhesion strength of ice.
[0029] Figure 7 The different Fe 3 O 4 @Comparison of electromagnetic parameters of composite membranes with different GO contents; Figure 7 In: "Frequency" indicates frequency, the unit is GHz; ε' indicates the real part of complex permittivity; ε'' indicates the imaginary part of complex permittivity; µ' indicates the real part of complex magnetic permeability; µ'' indicates the imaginary part of complex magnetic permeability; Figure 7 a represents the curve of the relationship between the real part of the complex dielectric constant ε' and the frequency; Figure 7 b in the figure represents the curve of the relationship between the imaginary part of the complex dielectric constant ε'' and the frequency; Figure 7 c represents the relationship between the real part of complex magnetic permeability µ' and the frequency; Figure 7 In the figure d, it represents the curve of the relationship between the imaginary part of complex magnetic permeability µ'' and the frequency.
[0030] Figure 8 is the electromagnetic parameter of the composite film provided in Comparative Example 1 of the present application; Figure 8 a in the figure represents the relationship between the complex dielectric constant and the frequency; Figure 8 b in the figure shows the relationship between complex magnetic permeability and frequency.
[0031] Fig. 9 is the electromagnetic parameter of the composite membrane provided in Comparative Example 2 of the present application; Fig. 9 a in the figure represents the relationship between the complex dielectric constant and the frequency; Fig. 9 b in the figure shows the relationship between complex magnetic permeability and frequency.
[0032] Fig.10 is the electromagnetic parameter of the composite membrane provided in Comparative Example 3 of the present application; Fig.10 a in the figure represents the relationship between the complex dielectric constant and the frequency; Fig.10 b in the figure shows the relationship between complex magnetic permeability and frequency. DETAILED DESCRIPTION
[0033] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0034] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.
[0035] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.
[0036] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0037] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0038] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also indicate the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as µg, mg, g, kg, etc.
[0039] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.
[0040] The term "TEA" is the abbreviation of "Triethanolamine", which means triethanolamine, and its chemical formula is: 6 H 15 NO 3 ; The term "EG" is an abbreviation for "ethylene glycol", which has the chemical formula: (CH 2 OH) 2 ; The term "PDMS" is the abbreviation of "Polydimethylsiloxane", which means polydimethylsiloxane, and its chemical formula is (C 2 H 6 OSi) n ; The term “GO” is the abbreviation of “graphene oxide”, which means graphene oxide.
[0041] In a first aspect, an embodiment of the present application provides a composite film, which comprises the following components in percentage by weight, based on the total weight of the composite film being 100%:
[0042] Fiber materials, 0%-10%;
[0043] Magnetic materials, 20%-40%;
[0044] Conductive materials, 5%-15%;
[0045] Base material, 30%-60%;
[0046] Curing agent, 1%-15%;
[0047] Phase change materials, 3%-20%;
[0048] The phase change material complies with the requirement that it is precipitated from a matrix material under a condition higher than its own melting temperature.
[0049] The composite membrane provided by the present application has good wave absorption performance, and at the same time has the function of reducing ice formation and improving deicing effect, and the raw material cost is relatively low. The composite membrane provided by the present application has a wide working temperature range: -50 ℃ to 200 ℃. The composite membrane provided by the present application reduces the adhesion of ice by the precipitation of internal phase change materials, thereby achieving the effect of reducing the possibility of ice formation and improving deicing performance. The electromagnetic waves are attenuated by the conductive network composed of magnetic materials, conductive materials and fiber materials.
[0050] The matrix material can provide the basic structure and mechanical support of the composite film, while the phase change characteristics of the phase change can provide deicing function. The softness of the matrix material helps the uniform distribution and solidification of the phase change material. The mutual solubility of the matrix material and the phase change material may affect the structural stability of the composite film. Too much phase change material may cause the mechanical properties of the composite film to decrease. Therefore, it is necessary to reasonably design the amount of phase change material and matrix material.
[0051] The matrix material can provide a carrier for magnetic materials, conductive materials, etc., and at the same time, magnetic materials, conductive materials, etc. can enhance the electromagnetic wave absorption performance of the composite film. For example, the uniform distribution of magnetic materials and conductive materials in the matrix material can improve the magnetic and conductive properties. However, the softness of the matrix material can limit the filling amount of magnetic and conductive materials, thereby affecting the electromagnetic properties. In addition, the addition of magnetic materials and conductive materials may change the mechanical properties of the matrix material, such as strength and durability. Therefore, it is necessary to reasonably design the amount of each component.
[0052] The addition of magnetic materials and conductive materials can improve the thermal conductivity of phase change materials and help accelerate the phase change process. At the same time, the presence of phase change materials can provide a filling matrix for magnetic materials and conductive materials, enhancing their conductivity. However, too much magnetic material and conductive material may affect the phase change characteristics of phase change materials, such as hindering the fluidity and phase change rate of phase change materials. Therefore, it is necessary to reasonably design the amount of each component.
[0053] Magnetic materials, conductive materials, and fiber materials can form a composite structure to improve the electromagnetic properties of the composite film. However, they may compete with each other during the filling process, resulting in uneven structure of the composite film or waste of materials. Therefore, it is necessary to reasonably design the amount of each component.
[0054] In some embodiments, based on the total weight of the composite film being 100%, the composite film includes the following components in weight percentage: fiber material, 1%-10%; magnetic material, 20%-40%; conductive material, 5%-15%; matrix material, 30%-60%; curing agent, 1%-15%; and phase change material, 7%-20%.
[0055] In some embodiments, the phase change material meets the requirement that: it precipitates from the matrix material at a temperature above -20°C. More preferably, the phase change material meets the requirement that: it precipitates from the matrix material at a temperature between -20°C and room temperature (eg, 25°C).
[0056] In some embodiments, the matrix material includes a polymer resin, the polymer resin includes at least one of polydimethylsiloxane and polyurethane; and / or the phase change material includes at least one of liquid paraffin and polyvinyl alcohol; and / or the magnetic material includes at least one of ferrosoferric oxide nanoparticles, iron oxide, and nickel oxide; and / or the conductive material includes at least one of graphene oxide, carbon nanotubes, and graphene.
[0057] The matrix material is mainly used to provide the flexibility and weather resistance of the composite film, and its surface has a certain hydrophobicity. For example, polydimethylsiloxane (PDMS), polydimethylsiloxane is a hydrophobic material, which means that its surface does not tend to interact with water molecules, but repels water molecules and shows low hydrophilicity. Therefore, when ice comes into contact with the PDMS surface, due to the hydrophobic nature of PDMS, it does not promote the adsorption of water molecules on its surface, thereby reducing the adhesion between ice and PDMS. In this case, the arrangement of water molecules on the PDMS surface is not as orderly and tight as on the ice surface, resulting in weakened interfacial interaction between ice and PDMS and reduced adhesion. In applications where it is necessary to reduce the adhesion of materials to ice, other materials with similar hydrophobic properties can be considered, such as other polymer resins with special treatments, such as polyurethane. The selection of these materials should be determined based on specific application requirements and environmental conditions to ensure that the expected performance and effects are achieved.
[0058] Phase change materials are mainly used for deicing, reducing the adhesion of ice by separating out from the main body of the base material. Phase change materials include but are not limited to liquid paraffin and polyethylene wax.
[0059] The magnetic material includes at least one of ferroferric oxide nanoparticles, iron oxide, and nickel oxide;
[0060] The conductive material includes at least one of graphene oxide, carbon nanotubes and graphene.
[0061] The magnetic material is mainly used to absorb electromagnetic waves and improve the electromagnetic wave shielding performance of the composite film. The magnetic material includes but is not limited to ferroferric oxide nanoparticles, iron oxide, and nickel oxide.
[0062] More preferably, the average particle size of the ferrosoferric oxide nanoparticles is 50 nm-200 nm.
[0063] The conductive material is mainly used as a part of the conductive network to improve the conductive properties of the composite film and enhance the mechanical properties. The conductive material includes but is not limited to graphene oxide, carbon nanotubes, and graphene.
[0064] Further preferably, the average radial size of the graphene oxide is 5 μm-8 μm.
[0065] In addition, the fiber material is mainly used to enhance the mechanical properties and conductive properties of the composite film. The fiber material includes carbon fiber, carbon nanotube, carbon black, etc. Preferably, the carbon fiber includes chopped carbon fiber.
[0066] Curing agents are mainly used to promote the curing and molding of materials during the preparation process, so that the composite film has certain mechanical properties and durability. Curing agents include but are not limited to:
[0067] Epoxy resin curing agent: for example, amine curing agent (such as ethylenediamine, tetraethylenediamine), acid anhydride curing agent (such as acid anhydride curing agent, epoxy imidazole curing agent), etc.;
[0068] Polyimide curing agent: such as thermosetting polyimide resin curing agent, amino resin curing agent, etc.;
[0069] Polyether curing agent: such as polyether polyol, polyether amine, etc.
[0070] More preferably, the curing agent is bisphenol A diglycidyl ether.
[0071] The amount of fiber material used is 1% to 10%. Increasing the content of fiber material is beneficial to improving the mechanical strength and electrical conductivity of the composite film, but too high a content may cause the processing performance of the composite film to decrease.
[0072] The amount of magnetic material used is 20% to 40%. Increasing the content of magnetic material is beneficial to improving the electromagnetic wave shielding performance of the composite film, but too high a content may cause the mechanical properties of the composite film to decrease.
[0073] The amount of conductive material used is 5% to 15%. Increasing the content of conductive material is beneficial to improving the conductivity and mechanical properties of the composite material, but too high a content may increase the cost of the composite material and reduce the processing performance.
[0074] The amount of matrix material used is 30% to 60%. Increasing the content of matrix material is beneficial to improving the flexibility and weather resistance of the composite film, and is also beneficial to molding and processing, but too high a content may cause the strength and rigidity of the composite film to decrease.
[0075] The dosage of phase change material is 5% to 20%. Increasing the content of liquid paraffin can improve the active deicing function of the composite film and reduce the adhesion of ice, but too high a content may affect the mechanical properties and stability of the composite material.
[0076] The dosage of curing agent is 1% to 10%. The dosage of curing agent needs to be sufficient to ensure that the composite film material can be cured and formed, but too high a content may cause the composite film material to cure too fast or the reaction to be incomplete, affecting the performance of the composite film.
[0077] In some embodiments, the conductive material is coated on the outside of the magnetic material; and / or, the mass ratio of the magnetic material to the conductive material is 3:1-5:1.
[0078] The mass ratio of magnetic material to conductive material will affect the uniformity and quality of the composite material in which the conductive material covers the magnetic material.
[0079] The mass ratio of magnetic material to conductive material is preferably designed to be 3:1-5:1. Increasing the proportion of magnetic particles can further increase the imaginary part of magnetic permeability, thereby improving the magnetic loss capacity of the composite film; however, the density of the composite film will also increase, which is not conducive to the use of the composite film in lightweight scenarios. Therefore, the present invention preferably designs the mass ratio of magnetic material to conductive material to be 3:1-5:1, which is conducive to improving the magnetic loss capacity of the composite film while meeting the lightweight application requirements.
[0080] In addition, the mixing time will also have a certain influence on the uniformity of the composite material, etc. Preferably, the mixing time is 20 min-40 min.
[0081] In some embodiments, the magnetic material is ferroferric oxide nanoparticles, and the conductive material is graphene oxide.
[0082] First, ferroferric oxide nanoparticles have high specific capacitance and good magnetic permeability, which enables them to play a role in magnetic loss in electromagnetic wave absorption. Magnetic loss mainly comes from hysteresis loss and eddy current loss inside the material. These loss mechanisms can effectively consume the energy of the incident electromagnetic wave, thereby reducing the reflection and transmission of the electromagnetic wave.
[0083] Secondly, the high specific surface area and excellent conductivity of graphene oxide provide another way for the absorption of electromagnetic waves. The presence of graphene oxide layer not only enhances the conductivity loss of the material, but also promotes multiple reflections and scattering of electromagnetic waves inside the material due to its layered structure, increasing the interaction opportunities between electromagnetic waves and materials, thereby improving the absorption efficiency.
[0084] In addition, the combination of ferroferric oxide nanoparticles and graphene oxide can also improve the impedance matching of the composite material. Impedance matching refers to the matching of the surface impedance of the material with the impedance of free space, which is crucial for the effective absorption of electromagnetic waves. Good impedance matching can reduce the reflection of electromagnetic waves on the surface of the material, allowing more electromagnetic waves to enter the material and be absorbed.
[0085] In summary, the combination of ferroferric oxide nanoparticles and graphene oxide provides an efficient and multifunctional solution for electromagnetic wave absorption. The development of this composite material is of great significance for improving electromagnetic compatibility and protecting against electromagnetic pollution.
[0086] In some embodiments, the fiber material is chopped carbon fiber; the matrix material is polydimethylsiloxane; and the phase change material is liquid paraffin.
[0087] The present application prepares a flexible composite film by mixing ferroferric oxide nanoparticles with graphene oxide, chopped carbon fibers, polydimethylsiloxane, liquid paraffin and a curing agent. The composite film can reduce the adhesion of ice by the precipitation of internal paraffin, thereby reducing the possibility of icing and improving the deicing performance; and the electromagnetic waves are attenuated by the conductive network composed of ferroferric oxide nanoparticles, graphene oxide and chopped carbon fibers.
[0088] The composite membrane provided by the present application contains electromagnetic dual loss materials, and achieves good microwave absorption effect at a thin thickness. Nano-scale ferroferric oxide, graphene oxide and short-cut carbon fiber are used as absorbents with low density to achieve lightweight design.
[0089] A second aspect of the embodiment of the present application provides a method for preparing a composite film, comprising:
[0090] Providing the above-mentioned composite membrane component raw materials:
[0091] The fiber material, the magnetic material, the conductive material, the matrix material, the phase change material and the curing agent are mixed and then cured to obtain a composite film.
[0092] The present application provides a method for preparing a composite film, obtaining a composite material with a conductive network structure and a phase change material uniformly dispersed in a matrix material, ensuring the uniformity and stability of the composite film, and the prepared composite film has good electromagnetic shielding performance and deicing performance. In addition, the preparation method is relatively simple and the raw material cost is low.
[0093] In some embodiments, the step of mixing the fiber material, the magnetic material, the conductive material, the matrix material, the phase change material and the curing agent comprises:
[0094] Adding magnetic material and conductive material into water, mixing and drying, to obtain a composite material of conductive material coated magnetic material;
[0095] Phase change material, composite material and fiber material are added into the matrix material, and then curing agent is added and mixed.
[0096] In the present application, the magnetic material and the conductive material are mixed, and external forces such as stirring are used to promote the uniform mixing of the magnetic material and the conductive material, and a composite material of the conductive material coated with the magnetic material is prepared based on physical mixing and adsorption. Preferably, in the preparation of Fe 3 O 4 @GO composite material, Fe 3 O 4 Electrostatic interaction and π-π stacking may occur between nanoparticles and GO, making Fe 3 O 4 The nanoparticles are evenly dispersed on the surface of GO.
[0097] In the present application, phase change material, composite material and fiber material are added to the matrix material for mixing, and then a curing agent is added for mixing. By mixing the components, the components are evenly dispersed in the matrix material for subsequent curing.
[0098] In the present application, the composite membrane precursor solution is solidified by conventional solidification means (such as drying) so that the curing agent and the base material undergo a cross-linking reaction to form a network structure of the composite membrane, and finally a solidified composite membrane is prepared.
[0099] A third aspect of an embodiment of the present application provides an application of a composite film, wherein the composite film and / or the composite film prepared by the above-mentioned preparation method is used as an electromagnetic shielding material, and / or as an anti-icing and de-icing material.
[0100] The composite film provided in this application can be applied in the following fields:
[0101] 1) Aerospace:
[0102] Used to prepare coatings on the surfaces of aircraft, helicopters and drones to improve their performance in adverse weather conditions, such as anti-icing, de-icing and lightning strike reduction capabilities.
[0103] Used to prepare exterior coatings for satellites and spacecraft to protect them from the extreme temperatures and electromagnetic radiation they encounter in space.
[0104] 2) Automobile Industry:
[0105] Used to prepare coatings on the surfaces of automotive glass, body and sensors to improve the driving safety of vehicles in adverse weather conditions, such as deicing and enhancing electromagnetic wave shielding capabilities.
[0106] Used to prepare coatings for electric vehicle battery pack casings to improve battery performance and life in low temperature environments.
[0107] 3) Electronic products:
[0108] Used to prepare coatings on the surface of electronic equipment to absorb electromagnetic waves and reduce electromagnetic interference, thereby improving the performance and stability of the equipment.
[0109] Used to prepare antenna surface coatings for wireless communication equipment, radar and microwave equipment to enhance their efficiency in receiving and transmitting electromagnetic waves.
[0110] 4) Construction:
[0111] Used to prepare coatings for building exterior walls or roofs to improve the building's thermal insulation and wind and rain resistance, and reduce electromagnetic interference to indoor electronic equipment.
[0112] Used to prepare coatings for bridges and elevated roads to prevent ice and snow accumulation and improve road traffic safety.
[0113] 5) Energy sector:
[0114] Used to prepare coatings on the surfaces of wind turbines and solar panels to improve the performance and reliability of energy equipment in extreme climate conditions.
[0115] Used to prepare coatings on the surfaces of energy transmission lines and transformers to reduce ice and snow accumulation and improve the electromagnetic compatibility of equipment.
[0116] 6) Military and security fields:
[0117] Used to prepare coatings on the surfaces of military aircraft, ships and armored vehicles to improve their stealth and survivability in harsh environments and electromagnetic interference.
[0118] Used to prepare coatings for military communications and radar equipment to improve the concealment and anti-interference capabilities of communications and surveillance systems.
[0119] In some embodiments, the composite film provided in the present application can be used as a surface material of a stealth device or apparatus and can be coated on the surface of the stealth device or apparatus.
[0120] In some embodiments, the composite film provided in the present application can also be used as a raw material to prepare other composite film materials for use as stealth equipment or devices.
[0121] Preferably, the coating thickness is 1 mm-2 mm.
[0122] The thickness of the coating should be sufficient to ensure that the composite film forms a uniform and dense covering layer on the surface of the equipment or device to ensure the stability and reliability of its performance. A coating that is too thin may not completely cover the surface, affecting the function, while a coating that is too thick may result in uneven coating and incomplete curing.
[0123] The thickness of the coating affects its weight and wind resistance. A coating that is too thick will increase the weight of the equipment or device, such as increasing the weight of a stealth aircraft, which may affect its flight performance and fuel consumption; at the same time, a coating that is too thick will also increase the roughness of the surface, increase wind resistance, and affect its operating speed and fuel efficiency.
[0124] A coating that is too thick may impose additional load on the fuselage structure, affecting its durability and life; at the same time, for some materials, a coating that is too thick may cause uneven thermal expansion or stress concentration, causing cracking or failure.
[0125] In summary, although there may be certain limitations on the thickness of the composite film as a coating, the specific thickness range will be affected by many factors. Generally, the thickness of the composite film as a coating is preferably set at 1 mm-2 mm to ensure uniform coverage and good performance. However, the actual thickness range may vary depending on factors such as specific application requirements, material properties, and aircraft design.
[0126] In some embodiments, the composite film provided in the present application can be directly coated on sensitive parts of a stealth aircraft through a brush coating process, achieving the dual effects of active deicing and reducing the radar scattering interface, and the construction process is simple.
[0127] The following describes the invention in conjunction with specific embodiments.
[0128] Ingredients
[0129]
[0130] Example 1
[0131] This embodiment provides a composite film, and the specific preparation method is as follows:
[0132] S1. FeCl 3 6H 2 O (0.14 g) and FeCl 2 ·4H 2 O (0.1032 g) was dissolved in distilled water (50 g) and ultrasonically dispersed for 2 h to obtain a mixed solution;
[0133] S2. Add 1 mol / L NaOH solution to the mixed solution obtained in step S1, and adjust the pH value of the mixed solution to 10;
[0134] S3. Then the solution prepared in step S2 is continuously stirred at 80 °C for 5 h to form a colloidal solution;
[0135] S4. Finally, the prepared product was dried in a vacuum oven at 65 °C for 24 h, and washed alternately with deionized water and anhydrous ethanol for 3 times to obtain Fe 3 O 4 Nanoparticles; preparation process such as Figure 1 As shown;
[0136] S5. 4.5 g Fe 3 O 4 Nanoparticles and 2.25 g GO were added to 100 mL distilled water and stirred evenly to precipitate. The mixture was dried in an oven at 70 °C to obtain the material Fe 3 O 4 @GO;
[0137] S6. Add different weight fractions (0%, 3%, 5%, 7%, 10%, 15%, 20%) of liquid paraffin, 6.75 g Fe 3 O 4 @GO and 0.32g chopped carbon fiber were added to 8.2g PDMS in sequence, stirred evenly, and then 0.82g curing agent was added and stirred again for 5min. The uniform composite material was spread on a glass plate to prepare a composite film. These composite film samples are collectively referred to as Fe 3 O 4 @rGO / CF / PDMS / 0-20%Paraffin.
[0138] The composite membrane samples prepared with different mass fractions (0%, 3%, 5%, 7%, 10%, 15%, 20%) of liquid paraffin were named as follows: Fe 3 O 4 @rGO / CF / PDMS / 0%Paraffin、Fe 3 O 4 @rGO / CF / PDMS / 3%Paraffin、Fe 3 O 4 @rGO / CF / PDMS / 5%Paraffin、Fe 3 O 4 @rGO / CF / PDMS / 7%Paraffin、Fe 3 O 4 @rGO / CF / PDMS / 10%Paraffin、Fe 3 O 4 @rGO / CF / PDMS / 15%Paraffin、Fe 3 O 4 @rGO / CF / PDMS / 20%Paraffin.
[0139] The prepared composite film was subjected to an adhesion test to determine the optimal liquid paraffin content of the composite film to achieve the best deicing effect. The results are as follows: Figure 6 shown.
[0140] The prepared Fe 3 O 4 The electromagnetic parameters of the rGO / CF / PDMS / 10% Paraffin composite membrane were tested to obtain the electromagnetic parameters of the composite membrane in the 2 GHz-18 GHz frequency band. The results are as follows Figure 4 The electromagnetic parameters are imported into CST Studio software to calculate the reflection loss of the composite film. The results are shown in Figure 5 shown.
[0141] Example 2
[0142] This embodiment provides a composite film, and the specific preparation method is as follows:
[0143] S1. FeCl 3 6H 2 O (0.14 g) and FeCl 2 ·4H 2 O (0.1032 g) was dissolved in distilled water (50 g) and ultrasonically dispersed for 2 h to obtain a mixed solution;
[0144] S2. Add 1 mol / L NaOH solution dropwise to the mixed solution obtained in step S1, and adjust the pH value of the mixed solution to 10;
[0145] S3. Then the solution prepared in step S2 is continuously stirred at 80 °C for 5 h to form a colloidal solution;
[0146] S4. Finally, the prepared product was dried in a vacuum oven at 65 °C for 24 h, and washed alternately with deionized water and anhydrous ethanol for 3 times to obtain Fe 3 O 4 Nanoparticles; preparation process such as Figure 1 As shown;
[0147] S5. Fe 3 O 4 Nanoparticles and GO were added to 100 mL of distilled water and stirred evenly to precipitate. The mixture was dried in an oven at 70 °C to obtain the material Fe 3 O 4 @GO;
[0148] S6. Mix 2.25 g liquid paraffin and Fe 3 O 4 @GO was added to 8.2 g PDMS, stirred evenly, and then 0.82 g curing agent was added, and stirred again for 5 min. The uniform composite material was applied on a glass plate to prepare a composite film. The amount of each raw material used in this example and the names of the corresponding composite film samples prepared are shown in Table 2.
[0149] The electromagnetic parameters of the prepared composite membrane were tested to obtain the electromagnetic parameters of the composite membrane in the frequency band of 2 GHz-18 GHz. The results are as follows: Figure 7 shown.
[0150]
[0151] Comparative Example 1
[0152] This case provides a composite membrane, and the specific preparation method is as follows:
[0153] S1. Use an electronic balance to weigh 17.45 g PDMS and 2.5 g liquid paraffin, put them into a disposable plastic container and stir them for 5 min;
[0154] S2. Add 0.75 g of chopped carbon fiber and 10 g of GO to the mixed solution of PDMS and liquid paraffin and stir for 10 min to form a black solution;
[0155] S3. Add 1.75 g of curing agent to the solution composed of PDMS, liquid paraffin, chopped carbon fiber and GO, and stir for 5 min;
[0156] S4. Pour the mixed solution into the prepared mold and let it stand at room temperature for 30 min to precipitate bubbles in the mixed solution;
[0157] S5. The mixed solution after precipitation was placed in an oven at 80 °C for curing for 1 h to obtain a black flexible composite film prepared from PDMS / liquid paraffin / CF / GO materials;
[0158] The electromagnetic parameters of the prepared composite membrane were tested to obtain the electromagnetic parameters of the composite membrane in the frequency band of 2 GHz-18 GHz. The results are as follows: Figure 8 shown.
[0159] Comparative Example 2
[0160] This case provides a composite membrane, and the specific preparation method is as follows:
[0161] S1. FeCl 3 6H 2 O (0.14 g) and FeCl 2 ·4H 2 O (0.1032 g) was dissolved in distilled water (50 g) and ultrasonically dispersed for 2 h;
[0162] S2. Add 1 mol / L NaOH solution to the mixture in step S1 and adjust the pH value of the mixed solution to 10;
[0163] S3. Then the solution prepared in step S2 is continuously stirred at 80 °C for 5 h to form a colloidal solution;
[0164] S4. Finally, the prepared product was dried in a vacuum oven at 65 °C for 24 h, and washed alternately with deionized water and anhydrous ethanol for 3 times to obtain Fe 3 O 4 Nanoparticles; preparation process such as Figure 1 As shown;
[0165] S5. Add 2.5 g Fe 3 O 4 @GO (2.25 g Fe 3 O 4 , 0.25 g GO) was added to 20.45 g PDMS, stirred evenly, and then 2.05 g curing agent was added and stirred again for 5 min. The uniform composite material was spread on a glass plate to prepare a composite film.
[0166] The electromagnetic parameters of the prepared composite membrane were tested to obtain the electromagnetic parameters of the composite membrane in the frequency band of 2 GHz-18 GHz. The results are as follows: Fig. 9 shown.
[0167] Comparative Example 3
[0168] This case provides a composite membrane, and the specific preparation method is as follows:
[0169] S1. Use an electronic balance to weigh 20.45 g PDMS and 2.5 g liquid paraffin, put them into a disposable plastic container and stir them for 5 min;
[0170] S2. Add 2.05 g of curing agent to the milky white solution composed of PDMS and liquid paraffin, and stir for 5 min;
[0171] S4. Pour the mixed solution into the prepared mold and let it stand at room temperature for 30 min to precipitate bubbles in the mixed solution;
[0172] S5. The mixed solution after precipitation is placed in an oven at 80°C for curing for 1 h to obtain a transparent and flexible composite film made of PDMS / liquid paraffin material.
[0173] The electromagnetic parameters of the prepared composite membrane were tested to obtain the electromagnetic parameters of the composite membrane in the frequency band of 2 GHz-18 GHz. The results are as follows: Fig.10 shown.
[0174] Performance Testing
[0175] 1. Performance testing methods.
[0176] 1. Adhesion test: The composite film was subjected to tensile / peeling test according to ASTM D903 standard.
[0177] 2. Electromagnetic parameter test: The electromagnetic parameters of all composite films were tested in accordance with GB / T 35679-2017. The electromagnetic parameters of the composite film samples in the 2 GHz-18 GHz frequency band were obtained and imported into the CST Studio software to calculate the reflection loss of the composite film.
[0178] 3. Wave-absorbing effect: The evaluation of the wave-absorbing effect of the composite film follows the following criteria, that is, when the reflection loss RL<-10 dB, it is considered that 90% of the electromagnetic waves are absorbed.
[0179] 2. Test results
[0180] like Figure 2 As shown, Fe 3 O 4 The nanoparticles are evenly dispersed and densely arranged, showing aggregation between particles, but the overall surface morphology is relatively regular, without obvious pores or gaps. The particles are spherical, polyhedral or prism-shaped, with sizes ranging from tens to hundreds of nanometers. 3 O 4 All magnetic materials can be used in the embodiments of the present application. Such morphology, distribution and size are beneficial to enhancing the electrical conductivity, electromagnetic wave absorption performance and mechanical strength of the composite film, and affecting the phase change performance of the composite film.
[0181] Fe 3 O 4 As magnetic conductive materials, the uniform dispersion and dense arrangement of nanoparticles help improve the conductivity of the composite film. The aggregation between particles can increase the number and connectivity of conductive channels, thereby reducing resistance and improving conductivity.
[0182] Fe 3 O 4 The size and morphology of nanoparticles have an important influence on the electromagnetic wave absorption performance of the composite film. The size of the particles is between tens and hundreds of nanometers. Nanoparticles within this range have good absorption performance for electromagnetic waves of specific wavelengths. The polyhedral or prismatic morphology of the particles may increase the absorption surface area and further improve the absorption efficiency.
[0183] The close arrangement and aggregation between particles can increase the overall mechanical strength and durability of the composite membrane. This dense structure helps to resist external stress and shear force and improve the stability of the composite membrane.
[0184] The composite film contains phase change materials, Fe 3 O 4 The distribution and arrangement of nanoparticles can affect the phase change properties of phase change materials. The aggregation of particles can lead to partial coverage or blockage of the phase change material, affecting the thermal conductivity and phase change rate of the phase change material.
[0185] like Figure 3As shown in the figure, it can be clearly observed from the optical microscope that the spherical liquid paraffin molecules gradually precipitate from the PDMS channels and form a dense oil film on the surface of the composite film. This process is due to the characteristics of the liquid paraffin in the composite film. At the appropriate temperature, the liquid paraffin molecules have a certain fluidity, are released from the PDMS channels and aggregate on the surface. The dense oil film formed effectively reduces the adhesion of ice and weakens the adhesion between the ice structure and the surface of the composite film. Therefore, the composite film can reduce the adhesion of ice under freezing conditions and achieve the effect of active deicing. This feature is particularly important in the aviation field, which can reduce ice accumulation on the surface of the aircraft and improve flight safety.
[0186] like Figure 4 As shown in the figure, the real part of the complex dielectric constant of the composite film at 2 GHz-18 GHz fluctuates in the range of 9-15, indicating that the composite film has good electricity storage capacity; while the imaginary part of the complex dielectric constant at 3 GHz-11 GHz is larger, indicating that the composite film has good loss performance; the imaginary part of the magnetic permeability of the composite film at 2 GHz-18 GHz is larger, indicating that the composite film has a strong response to the magnetic field, which also means higher energy loss.
[0187] like Figure 5 As shown in the figure, the composite film achieved good microwave absorption effect when the thickness was 1.41 mm, and the effective absorption bandwidth in the 2 GHz-18 GHz frequency band reached 6.19 GHz.
[0188] like Figure 6As shown in the figure, as the content of liquid paraffin in the composite film increases, the adhesion of ice on the composite film tends to decrease. This is because the addition of liquid paraffin changes the properties of the composite film surface, making its surface hydrophobic, reducing the adhesion of ice. Specifically, liquid paraffin is a material with strong hydrophobicity, and its addition to PDMS will make the surface of the overall composite material more hydrophobic. The enhancement of hydrophobicity may be due to the presence of more hydrophobic groups, such as alkyl groups, in the molecular structure of liquid paraffin. Liquid paraffin and PDMS may have a certain compatibility in molecular structure, resulting in the formation of a more uniform composite material after mixing. This compatibility enables liquid paraffin to be evenly dispersed in the PDMS matrix, thereby forming a more uniform hydrophobic layer on the overall surface. The addition of liquid paraffin may fill the microscopic pores or surface unevenness in the PDMS matrix, thereby reducing the contact angle of the surface and enhancing the hydrophobic performance. This filling effect makes the surface smoother, reduces the adhesion of water molecules on the surface, and thus improves the hydrophobicity. However, when the liquid paraffin content reaches 10%, the adhesion of ice on the composite film no longer changes significantly. This may be because the addition of liquid paraffin has reached a certain saturation state, and further increasing the liquid paraffin content does not significantly change the properties of the composite film surface. In addition, too high a liquid paraffin content may cause the composite film surface to be overly hydrophobic, which in turn affects other properties of the composite film. Therefore, a 10% liquid paraffin content may be the optimal content to maintain a balance in the properties of the composite film.
[0189] like Figure 7 As shown, with Fe 3 O 4 With the increase of GO content (30-70%), the real part, imaginary part and imaginary part of the complex dielectric constant of the composite film increased in direct proportion. This may be due to the increase of Fe 3 O 4 The electrical conductivity and dielectric properties of @GO particles increase with the increase of their content, thereby improving the responsiveness of the composite film to electromagnetic waves. On the other hand, in the 1 GHz-6 GHz and 14 GHz-18 GHz frequency bands, the real part of the magnetic permeability of the composite film increases with the increase of Fe 3 O 4 The increase of @GO content may be due to the 3 O 4 The magnetic permeability of @GO particles is enhanced, resulting in an increase in the real part of the magnetic permeability. In the 6 GHz-14 GHz frequency band, the real part of the magnetic permeability of the composite film shows an opposite trend. This may be because in this frequency band, the electromagnetic response of the composite film is affected by other factors, resulting in a different change direction of the real part of the magnetic permeability than in other frequency bands. 3 O 4With the increase of GO content, the electromagnetic properties of the composite film are affected by the internal structure and interaction of the composite material, showing different change trends of the real part of the magnetic permeability in different frequency bands.
[0190] like Figure 8 As shown in the figure, the addition of chopped carbon fiber and GO has improved both the real and imaginary parts of the dielectric constant of the composite film, especially the real part of the dielectric constant. This shows that the addition of chopped carbon fiber and GO can improve the composite film's ability to store and lose electromagnetic waves. Since no magnetic material is added, the complex magnetic permeability of the composite film has not changed.
[0191] like Fig. 9 As shown, after adding GO and Fe 3 O 4 After the addition of nanoparticles, the dielectric constant and magnetic permeability of the composite film were improved to a certain extent, which indicates that GO and Fe 3 O 4 The addition of nanoparticles endows the composite film with the ability to reduce the electrical and magnetic losses of electromagnetic waves. 3 O 4 The addition of nanoparticles has a significant effect on the magnetic permeability of the composite film in the low-frequency range (2 GHz-8 GHz), indicating that magnetic nanoparticles can improve the composite film's ability to resist the loss of low-frequency electromagnetic waves.
[0192] like Fig.10 As shown in the figure, the real part of the dielectric constant of the composite film prepared only with PDMS and liquid paraffin fluctuates in the range of 1.75-2.25, and the value is small, indicating that the composite film has no electrical conductivity; further observation of the imaginary part of the dielectric constant shows that its value is small, indicating that the composite film has no loss of electromagnetic wave ability. Since no magnetic material is added during the preparation of the composite film, the magnetic permeability of the composite film is basically the same as that of air, which can be judged that the composite film has no magnetic loss ability.
[0193] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A composite film, characterized in that Taking the total weight of the composite film as 100%, the components are as follows in weight percentage: Fiber materials, 0%-10%; Magnetic materials, 20%-40%; Conductive materials, 5%-15%; Base material, 30%-60%; Curing agent, 1%-15%; Phase change materials, 3%-20%; The matrix material includes a polymer resin, and the polymer resin includes at least one of polydimethylsiloxane and polyurethane; The phase change material meets the following conditions: it is precipitated from a base material under a temperature condition of -20°C to 25°C; and the phase change material includes at least one of liquid paraffin and polyvinyl alcohol.
2. A composite membrane according to claim 1, characterized in that: Taking the total weight of the composite film as 100%, the composite film comprises the following components in percentage by weight: Fiber materials, 1%-10%; Magnetic materials, 20%-40%; Conductive materials, 5%-15%; Base material, 30%-60%; Curing agent, 1%-15%; Phase change material, 7%-20%.
3. A composite membrane according to claim 1, characterized in that: The magnetic material includes at least one of ferroferric oxide nanoparticles, iron oxide, and nickel oxide; And / or, the conductive material includes at least one of graphene oxide, carbon nanotubes, and graphene.
4. A composite membrane according to claim 1, characterized in that: The conductive material is coated on the surface of the magnetic material; And / or, the mass ratio of the magnetic material to the conductive material is 3:1-5:
1.
5. A composite membrane according to claim 4, characterized in that: The magnetic material is ferroferric oxide nanoparticles, and the conductive material is graphene oxide.
6. A composite membrane according to any one of claims 1 to 5, characterized in that: The fiber material is chopped carbon fiber; The base material is polydimethylsiloxane; The phase change material is liquid paraffin.
7. A method for preparing a composite membrane, characterized in that: include: Providing component raw materials of the composite membrane according to any one of claims 1 to 6: The fiber material, the magnetic material, the conductive material, the matrix material, the phase change material and the curing agent are mixed and then cured to obtain the composite film.
8. The method for preparing a composite membrane according to claim 7, characterized in that: The step of mixing the fiber material, the magnetic material, the conductive material, the matrix material, the phase change material and the curing agent comprises: The magnetic material and the conductive material are added into water, mixed and dried to obtain a composite material in which the conductive material covers the magnetic material; The phase change material, the composite material and the fiber material are added into the matrix material, and then the curing agent is added and mixed.
9. Use of a composite film as an electromagnetic shielding material, an anti-icing material or a deicing material; the composite film is the composite film according to any one of claims 1 to 6 or the composite film prepared by the preparation method according to any one of claims 7 to 8.
Citation Information
Patent Citations
Polyaniline / oxidized graphene / ferriferrous oxide absorbing material and preparation method
CN104163919A
Paraffin composite phase change material with high thermal conductivity and preparation method thereof
CN108285778A
High-enthalpy-value flexible phase-change composite material film and preparation method thereof
CN114539788A
Multifunctional magnetic resin-based composite wave-absorbing coating as well as preparation method and application thereof
CN116285660A
Electroconductive resin composition
JP2011132362A