A method for reducing the harm of iron element in 6101 aluminum alloy
By adding an appropriate amount of silicon to the 6101 aluminum alloy melt and performing multiple steps of processing, the problem of iron in aluminum alloy is solved, the mechanical and conductive properties of aluminum alloy are improved, and high-efficiency and low-cost high-quality aluminum alloy preparation is achieved. , promoting its application in the field of new energy and the development of a green circular economy.
Patent Information
- Application Number
- CN202411111251.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-14
AI Technical Summary
The prior art has problems of complex operation and inefficiency in reducing the harm of iron in aluminum alloys, and has failed to effectively solve the impact of iron-rich relative to the matrix liquid aluminum from the source.
Add silicon element to the 6101 aluminum alloy melt so that its mass content is 0.6~7.3 times the mass content of impurity iron element, and control the mass percentage of magnesium element within the range of 0.3~0.8%, by adjusting the melt temperature and carrying out the Multi-step treatments such as homogenization, solid solution, quenching and aging treatment promote the precipitation and precipitation of nanoscale magnesium silicon phases and improve mechanical properties and electrical conductivity.
It has achieved high-efficiency and low-cost preparation of high-quality 6101 aluminum alloy, significantly improving its mechanical properties and conductive properties, promoting the application of aluminum alloys in new energy vehicles and other fields, and helping the development of green, low-carbon circular economy.
Smart Images

Figure CN118639042B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of recycled aluminum alloy melt processing, and specifically relates to a method for reducing the harm of iron elements in 6101 aluminum alloy. Background Art
[0002] 6000 series Al-Mg-Si alloy has the advantages of high specific strength, good electrical conductivity and excellent corrosion resistance, and is widely used in new energy vehicles, 3C electronics, aerospace, rail transit and high-end equipment. In the process of aluminum alloy preparation, electrolytic aluminum is usually used as the raw material for the production of aluminum alloy, and the electrolytic aluminum water inevitably contains the impurity element Fe. In addition, aluminum and aluminum alloys have good recyclability, and their recycling and reuse contribute to the development of green and low-carbon circular economy, showing huge economic and environmental benefits. However, in the process of recycling and reusing waste aluminum secondary resources, Fe is also the relatively high impurity element in recycled aluminum. The introduction of the impurity element Fe can significantly reduce the mechanical properties, corrosion resistance and electrical (thermal) conductivity of aluminum alloys.
[0003] In recent years, there have been a large number of reports on the removal of impurity element Fe in aluminum and aluminum alloy melts. In order to reduce the Fe content in aluminum melt, the patent publication number CN117947275A proposes a medium-frequency magnetic field to assist in removing impurity iron in recycled aluminum, the patent announcement number CN111549237B proposes a method for separating iron impurities in recycled aluminum melt by pulse current, the patent announcement number CN116590536B proposes a flux that can achieve a 40% removal rate of impurity iron in scrap aluminum, the document (SW Kim, UH Im, HC Cha, et al. Removal of primary iron rich phase from aluminum-silicon melt by centrifugal separation. ChinaFoundry, 2013, 10(2): 112-117.) reports a technology for centrifugally separating iron-rich phase from aluminum liquid by using density difference, and the patent announcement number CN107619959B proposes a method for filtering and separating iron phase by using ceramic filtration in combination with metamorphic elements.
[0004] In addition to the above-mentioned iron removal technology, a modification technology for iron-rich phases in aluminum and aluminum alloys has also been developed. The addition of elements transforms the iron-rich phase from needle-shaped to nearly spherical or granular, thereby reducing the harm of the iron-rich phase. The patent with announcement number CN111254303B proposes a method for adding Mn and B elements to recycled aluminum to improve the morphology of the iron-rich phase. The literature (J. Santos, AEW Jarfors, AK Dahle. Formation of iron-rich intermetallic phases inAl-Si-Mg: Influence of cooling rate and strontium modification. Metallurgicaland Materials Transactions A, 2019, 50(9): 4148-4165) reported the effect of the addition of the element Sr on the formation of iron-rich phases in Al-Si-Mg alloys, indicating that the addition of Sr can change the nucleation and growth conditions of the iron-rich phase and promote the formation of fine flake π-Al 8 FeMg 3 Si 6 phase formation, while inhibiting the formation of needle-like β-Al 5 The literature (HX Jiang, SX Li, QJZheng, LL Zhang, J. He, Y. Song, CK Deng, JZ Zhao. Effect of minorlanthanum on the microstructures, tensile and electrical properties of Al-Fealloys, Materials and Design, 2020, 195, 108991) and the literature (Zhang Zhenkai, Guo Yongchun, Xia Feng, et al. Effect of Ce-enriched rare earth and ultrasonic field on iron-rich phase in Al-Si alloy. Rare Metals, 2019, 43(2): 219-224) reported the enrichment characteristics of rare earth elements La and Ce in aluminum alloys and their effects on Al 5The inhibitory effect of FeSi on the growth of the preferred direction of the iron-rich phase, and the effect of ultrasonic cavitation on the refinement of the iron-rich phase. In addition, in terms of heat treatment process, the literature (X. Wu, H. Zhang, Z. Ma, et al. Interactions between Fe-rich intermetallics and Mg-Siphase in Al-Si-Mg alloys. Journal of Alloys and Compounds, 2019, 786: 205-214) reported the effects of Mg content and heat treatment process on the transformation of Fe-rich phase in aluminum alloys, indicating that when the Mg content is low (0.3~0.45%, mass fraction), the Mg element diffuses from the iron-rich phase to the Al matrix, promoting the formation of more Mg 2 Si strengthening phase is beneficial to improving mechanical properties.
[0005] The above iron removal and iron-rich phase modification technologies have their own advantages and disadvantages. They are generally complex to operate, have a long time period, and have low efficiency. The appropriate addition of alloying elements is relatively simple, clean and efficient in reducing the harm of iron-rich phases, but previous technologies mainly focus on regulating the type and morphology of Fe-rich phases, while the understanding of the source of the influence of impurity element Fe on the structure and properties of Al-Mg-Si alloys is still imperfect, ignoring the influence of the formation of iron-rich phases (Al, Fe, Si) on the matrix aluminum liquid itself and its improvement methods. With the continuous development of the aluminum industry and the improvement of requirements for aluminum alloy performance and cost, it is becoming more and more urgent to efficiently reduce the harm of impurity iron elements in recycled aluminum, and it is urgent to develop new methods and technologies from the source. Summary of the invention
[0006] The purpose of the present invention is to provide a method for reducing the harm of iron elements in 6101 aluminum alloy, reduce the harm of iron elements in 6101 aluminum alloy melt by utilizing the interaction between elements, prepare high-quality 6101 aluminum alloy with high efficiency and low cost, promote the recycling of secondary metal resources, and contribute to the development of green, low-carbon and circular economy.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] A method for reducing the harm of iron in 6101 aluminum alloy, comprising adding silicon to a 6101 aluminum alloy melt containing impurity iron, so that the mass content of silicon in the 6101 aluminum alloy melt is 0.6-7.3 times the mass content of impurity iron, and controlling the mass percentage of magnesium in the 6101 aluminum alloy melt within the range of 0.3-0.8%.
[0009] The method for reducing the harm of iron in 6101 aluminum alloy is to add silicon to the 6101 aluminum alloy melt containing impurity iron, so that the mass content of silicon in the 6101 aluminum alloy melt is 4.1 times the mass content of impurity iron, and the mass percentage of magnesium in the 6101 aluminum alloy melt is 0.6%, and the yield strength, tensile strength, elongation and conductivity of the 6101 aluminum alloy reach 195.33MPa, 216MPa, 13% and 58.13%IACS respectively.
[0010] The method for reducing the harm of iron in 6101 aluminum alloy comprises the following steps: first, clarifying the mass percentage of magnesium, silicon and impurity element iron in the aluminum alloy; second, placing the 6101 aluminum alloy in a smelting furnace for melting, and adjusting the melt temperature to 750°C; then adding Al-Si master alloy to the melt, and stirring to obtain a uniform 6101 aluminum alloy melt; then, adding a refining agent to the melt and introducing argon gas for purification, then adjusting the melt temperature to 690°C-710°C, standing for 10 minutes, and casting the melt into an aluminum alloy ingot; finally, the aluminum alloy ingot is subjected to a homogenization treatment at 470°C for 10 hours, a solution treatment and quenching treatment at 530°C for 2 hours, a rolling deformation treatment, and an aging treatment at 195°C for 12 hours, in order to obtain a high-quality 6101 aluminum alloy.
[0011] The principle of the present invention is as follows:
[0012] In the preparation process of 6101 aluminum alloy, electrolytic aluminum is usually used as the raw material for the production of aluminum alloy, which will inevitably introduce impurity iron elements; in addition, in the process of recycling and reusing waste aluminum secondary resources, the recycled aluminum contains a relatively high content of impurity iron elements. The presence of impurity iron elements will lead to insufficient mechanical properties and electrical conductivity of aluminum alloys. Based on the in-depth study of the source of the influence of impurity element Fe on the structure and performance of 6101 aluminum alloy, the present invention clarifies the influence of the formation of iron-rich phase on the matrix aluminum liquid itself: during the solidification process of 6101 aluminum alloy melt containing impurity element iron, the formation of iron-rich phase leads to a decrease in the concentration of silicon dissolved in the matrix liquid phase, resulting in an imbalance in the ratio of silicon to magnesium in the alloy matrix liquid phase, and then the number density of nano-scale magnesium-silicon (Mg, Si) strengthening phase precipitated in the α-Al matrix is reduced, and the concentration of magnesium dissolved in the α-Al matrix is increased. The present invention adopts the method of adding an appropriate amount of Si element to the 6101 aluminum alloy melt to promote the precipitation of nano-scale magnesium-silicon (Mg, Si) phase, on the one hand, reducing the harm of lattice distortion caused by excessive solid solution of Mg element in α-Al matrix, so as to improve the conductivity of 6101 aluminum alloy; on the other hand, increasing the number density of precipitation of nano-scale magnesium-silicon (Mg, Si) phase is conducive to precipitation strengthening, so as to improve the mechanical properties of 6101 aluminum alloy.
[0013] The advantages and beneficial effects of the present invention are as follows:
[0014] After adding an appropriate amount of Si to the commercially available 6101 aluminum alloy and the recycled 6101 aluminum alloy containing the impurity element iron, the present invention utilizes the interaction between elements to reduce the harm of the iron element in the melt of the commercially available 6101 aluminum alloy and the recycled 6101 aluminum alloy, and prepares high-quality 6101 aluminum alloy materials with excellent mechanical properties and electrical conductivity with high efficiency and low cost, promoting its application in the fields of new energy vehicles, electricity, transportation, etc. According to relevant patents (such as: Announcement No. CN105950893B), the conductivity of aluminum wires for electrical use nationwide can be increased by 0.1% IACS, which can reduce 10 billion kWh of electricity loss each year. This is conducive to the development of a green, low-carbon, circular economy, and has significant economic resource and social environmental benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a high-resolution image of the β″ phase of the transmission electron microscope (TEM) characterization analysis of the sample in Example 1.
[0016] Figure 2 This is a high-resolution image of the β′ phase of the transmission electron microscope (TEM) characterization analysis of the sample in Example 1.
[0017] Figure 3 This is a transmission electron microscope TEM image of the sample in Example 1. The black particles in the figure are (Mg, Si) phases, and the white ones are α-Al matrix.
[0018] Figure 4 This is a transmission electron microscope TEM image of the sample in Example 2. The black particles in the figure are (Mg, Si) phases, and the white ones are α-Al matrix.
[0019] Figure 5 This is a transmission electron microscope TEM image of the sample in Example 3. The black particles in the figure are (Mg, Si) phases, and the white ones are α-Al matrix.
[0020] Figure 6 This is a transmission electron microscope TEM image of the sample of Example 4. The black particles in the figure are (Mg, Si) phases, and the white ones are α-Al matrix.
[0021] Figure 7 This is a transmission electron microscope TEM image of the sample in Example 5. The black particles in the figure are (Mg, Si) phases, and the white ones are α-Al matrix.
[0022] Figure 8 This is a transmission electron microscope TEM image of the sample in Example 6. The black particles in the figure are (Mg, Si) phases, and the white ones are α-Al matrix.
[0023] Fig. 9The X-ray diffraction analysis results of the 6101 aluminum alloy of Example 1, Example 2 and Example 3, the diffraction angle 2θ is between 20 and 80 o X-ray diffraction spectrum. In the figure, the horizontal axis 2θ is the diffraction angle (degree), and the vertical axis Intensity is the relative intensity (au).
[0024] Fig.10 The X-ray diffraction analysis results of the 6101 aluminum alloy of Example 1, Example 2 and Example 3, the diffraction angle 2θ is between 43.2 and 45.6 o The local X-ray diffraction spectrum of . In the figure, the horizontal axis 2θ is the diffraction angle (degree), and the vertical axis Intensity is the relative intensity (au). DETAILED DESCRIPTION
[0025] In the preparation process of 6101 aluminum alloy, impurity Fe element is very easy to react with Si element and Al element to generate coarse AlFeSi iron-rich phase, thereby reducing the mechanical properties and electrical conductivity of the alloy. In addition, aluminum and aluminum alloys have good recyclability. However, in the recycling process of waste aluminum secondary resources, 6101 recycled aluminum is mixed with high content of impurity element iron, and the introduction of impurity element Fe significantly reduces the performance of recycled 6101 aluminum alloy. The present invention studies the influence of appropriate amount of Si element on the organization and performance of commercial 6101 aluminum alloy and recycled 6101 aluminum alloy containing impurity element iron, and finds that adding appropriate amount of Si can react with Mg element dissolved in α-Al matrix to promote the precipitation of (Mg, Si) phase precipitation, thereby reducing the solid solubility of Mg element in matrix, increasing the number of nanoscale (Mg, Si) phases, and then synergistically improving the mechanical properties and electrical conductivity of commercial 6101 aluminum alloy and recycled 6101 aluminum alloy, and obtaining high-quality 6101 aluminum alloy.
[0026] During the specific implementation process, an appropriate amount of Si was additionally added to the commercially available 6101 aluminum alloy melt so that the mass content of silicon element was 3.7~4.1 times the mass content of impurity iron element. The silicon content in the obtained 6101 aluminum alloy melt was increased by 0.2~0.6 times compared with the corresponding 6101 aluminum alloy, which can synergistically improve the mechanical properties and electrical conductivity. The performance indicators of 6101 aluminum alloy materials are as follows: tensile strength is 210~220 MPa, and the increase is 10~20 MPa; the electrical conductivity is 57.7~58.3% IACS, and the increase is 0.4~1.0%IACS.
[0027] During the specific implementation process, an appropriate amount of Si is additionally added to the recycled 6101 aluminum alloy melt so that the mass content of silicon is 1.8~2.2 times the mass content of impurity iron. The silicon content in the obtained 6101 aluminum alloy melt is 0.6~1.0 times higher than that of the corresponding 6101 aluminum alloy, which can synergistically improve the mechanical properties and electrical conductivity. The performance indicators of the recycled 6101 aluminum alloy material are as follows: tensile strength is 220~240 MPa, and the increase is 10~30 MPa; the electrical conductivity is 55.9~56.5% IACS, and the increase is 0.3~0.9% IACS.
[0028] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments, but the protection scope and application scope of the present invention are not limited to the following embodiments. Example 1
[0029] In this embodiment, on the basis of 6101 aluminum alloy (calculated by mass percentage, the contents of main elements in the aluminum alloy are: magnesium 0.6%, silicon 0.35%, iron 0.1%, and the balance is Al), no additional Si element is added.
[0030] In this embodiment, the specific implementation steps are as follows:
[0031] (1) Place a commercially available 6101 aluminum alloy ingot into a melting furnace for melting, and adjust the melt temperature to 750°C;
[0032] (2) A refining agent (based on mass percentage, its composition is 40% sodium cryolite and 46% fluoride salt) is introduced into the melt to react and prepare Al 5 Ti 1 B master alloy salt slag, 10% aluminum fluoride, 2% calcium fluoride, 2% potassium feldspar) and argon gas was introduced for purification, and then the melt temperature was adjusted to 700°C and allowed to stand for 10 minutes to obtain a 6101 aluminum alloy melt;
[0033] (3) pouring the 6101 aluminum alloy melt into a mold and cooling and solidifying it to obtain an aluminum alloy ingot;
[0034] (4) heating the aluminum alloy ingot to 470°C, keeping the temperature for 10 hours for homogenization treatment, and cooling the ingot to room temperature along with the furnace;
[0035] (5) heating the aluminum alloy ingot after homogenization treatment to 530° C. and keeping the temperature for 2 hours to perform solid solution treatment and quenching treatment;
[0036] (6) performing rolling deformation treatment on the ingot after solution treatment and quenching treatment at room temperature to obtain an aluminum alloy profile;
[0037] (7) The deformed aluminum alloy profile is heated to 195°C and kept at this temperature for 12 hours for aging treatment.
[0038] In this embodiment, the analysis results show that the performance indicators of the 6101 aluminum alloy profile obtained without the additional addition of Si element are as follows: tensile strength is 200 MPa, and electrical conductivity is 57.3% IACS. The mass content of silicon element is 3.5 times the mass content of impurity iron element. The commercially available 6101 aluminum alloy has good electrical conductivity, but the formation process of the iron-rich phase in the alloy consumes Si in the Al matrix, which reduces the concentration of Si element in the Al matrix, and then reduces the number density of nano-scale magnesium silicon (Mg, Si) strengthening phase precipitated in the α-Al matrix. Figure 1-Figure 2 As shown in Figure 2, it can be seen from the TEM high-resolution image that β″ and β′ (Mg, Si) phases are formed during the aging process, but the number density of the (Mg, Si) phase precipitated during the aging treatment is small, as shown in Figure 2. Figure 3 . As a result, the concentration of magnesium dissolved in the α-Al matrix increases, causing lattice distortion, thereby reducing the electrical conductivity. To this end, the design is optimized and an appropriate amount of Si element is added on this basis to promote the precipitation of nanoscale magnesium-silicon (Mg, Si) phases. On the one hand, the harm of lattice distortion caused by excessive Mg dissolved in the α-Al matrix is reduced to improve the electrical conductivity of the 6101 aluminum alloy; on the other hand, increasing the number density of precipitation of nanoscale magnesium-silicon (Mg, Si) phases is conducive to precipitation strengthening, so as to improve the mechanical properties of the 6101 aluminum alloy. Example 2
[0039] In this embodiment, on the basis of 6101 aluminum alloy (calculated by mass percentage, the content of main elements in the aluminum alloy is: 0.6% magnesium, 0.35% silicon, 0.1% iron, and the balance is Al), 0.02wt% Si element is added.
[0040] In this embodiment, the specific implementation steps are as follows:
[0041] (1) Place a commercially available 6101 aluminum alloy ingot into a melting furnace for melting, and adjust the melt temperature to 750°C;
[0042] (2) adding 0.02 wt % Si element to the melt in the form of Al-12% Si master alloy (Si 12%, balance Al, by mass percentage) and stirring for 10 minutes to obtain a uniform melt;
[0043] (3) A refining agent (based on mass percentage, its composition is 40% sodium cryolite and 46% fluoride salt) is introduced into the melt to react and prepare Al 5 Ti 1 B master alloy salt slag, 10% aluminum fluoride, 2% calcium fluoride, 2% potassium feldspar) and argon gas was introduced for purification, and then the melt temperature was adjusted to 690°C and allowed to stand for 10 minutes to obtain a 6101 aluminum alloy melt;
[0044] (4) pouring the 6101 aluminum alloy melt into a mold and cooling and solidifying it to obtain an aluminum alloy ingot;
[0045] (5) heating the aluminum alloy ingot to 470°C, keeping the temperature for 10 hours for homogenization, and cooling the ingot to room temperature along with the furnace;
[0046] (6) heating the aluminum alloy ingot after homogenization treatment to 530° C. and keeping the temperature for 2 hours to perform solid solution treatment and quenching treatment;
[0047] (7) performing rolling deformation treatment on the ingot after solution treatment and quenching treatment at room temperature to obtain an aluminum alloy profile;
[0048] (8) The deformed aluminum alloy profile is heated to 195°C and kept at this temperature for 12 hours for aging treatment.
[0049] In this embodiment, the analysis results show that in the 6101 aluminum alloy profile obtained after adding 0.02wt% Si, the mass content of silicon is 3.7 times the mass content of impurity iron, and the performance indicators are as follows: tensile strength is 210 MPa, and electrical conductivity is 57.76% IACS. Figure 4 As shown, compared with Example 1 without additional addition of Si element, the number density of (Mg, Si) phase precipitated in the sample of this example during the aging treatment increases, and the tensile strength and electrical conductivity are increased by 10 MPa and 0.43% IACS respectively, especially the electrical conductivity improvement effect is obvious. Example 3
[0050] In this embodiment, on the basis of 6101 aluminum alloy (calculated by mass percentage, the content of main elements in the aluminum alloy is: 0.6% magnesium, 0.35% silicon, 0.1% iron, and the balance is Al), 0.06wt% Si element is added.
[0051] In this embodiment, the specific implementation steps are as follows:
[0052] (1) Place a commercially available 6101 aluminum alloy ingot into a melting furnace for melting, and adjust the melt temperature to 750°C;
[0053] (2) adding 0.06 wt % Si element to the melt in the form of Al-12% Si master alloy and stirring for 10 minutes to obtain a uniform melt;
[0054] (3) A refining agent (based on mass percentage, its composition is 40% sodium cryolite and 46% fluoride salt) is introduced into the melt to react and prepare Al 5 Ti 1B master alloy salt slag, 10% aluminum fluoride, 2% calcium fluoride, 2% potassium feldspar) and argon gas was introduced for purification, and then the melt temperature was adjusted to 710°C and allowed to stand for 10 minutes to obtain a 6101 aluminum alloy melt;
[0055] (4) pouring the 6101 aluminum alloy melt into a mold and cooling and solidifying it to obtain an aluminum alloy ingot;
[0056] (5) heating the aluminum alloy ingot to 470°C, keeping the temperature for 10 hours for homogenization, and cooling the ingot to room temperature along with the furnace;
[0057] (6) heating the aluminum alloy ingot after homogenization treatment to 530° C. and keeping the temperature for 2 hours to perform solid solution treatment and quenching treatment;
[0058] (7) performing rolling deformation treatment on the ingot after solution treatment and quenching treatment at room temperature to obtain an aluminum alloy profile;
[0059] (8) The deformed aluminum alloy profile is heated to 195°C and kept at this temperature for 12 hours for aging treatment.
[0060] In this embodiment, the analysis results show that in the 6101 aluminum alloy profile obtained after adding 0.06wt% Si, the mass content of silicon element is 4.1 times the mass content of impurity iron element, and the performance indicators are as follows: yield strength is 195.33MPa, tensile strength is 216MPa, elongation is 13%, and conductivity is 58.13%IACS. Figure 5 As shown, compared with Example 1 without additional addition of Si element, the number density of (Mg, Si) phase precipitated in the sample of this example during the aging treatment is further increased, and the tensile strength and electrical conductivity are increased by 16 MPa and 0.83% IACS respectively. In comparison, the conductivity improvement effect is more significant. Example 4
[0061] In this embodiment, on the basis of recycled 6101 aluminum alloy (calculated by mass percentage, the contents of main elements in the aluminum alloy are: magnesium 0.6%, silicon 0.35%, iron 0.3%, and the balance is Al), no additional Si element is added.
[0062] In this embodiment, the specific implementation steps are as follows:
[0063] (1) Place the recycled 6101 aluminum alloy ingot into a melting furnace for melting, and adjust the melt temperature to 750°C;
[0064] (2) A refining agent (based on mass percentage, its composition is 40% sodium cryolite and 46% fluoride salt) is introduced into the melt to react and prepare Al 5 Ti 1B master alloy salt slag, 10% aluminum fluoride, 2% calcium fluoride, 2% potassium feldspar) and argon gas was introduced for purification, and then the melt temperature was adjusted to 700°C and allowed to stand for 10 minutes to obtain a 6101 aluminum alloy melt;
[0065] (3) pouring the 6101 aluminum alloy melt into a mold and cooling and solidifying it to obtain an aluminum alloy ingot;
[0066] (4) heating the aluminum alloy ingot to 470°C, keeping the temperature for 10 hours for homogenization treatment, and cooling the ingot to room temperature along with the furnace;
[0067] (5) heating the aluminum alloy ingot after homogenization treatment to 530° C. and keeping the temperature for 2 hours to perform solid solution treatment and quenching treatment;
[0068] (6) performing rolling deformation treatment on the ingot after solution treatment and quenching treatment at room temperature to obtain an aluminum alloy profile;
[0069] (7) The deformed aluminum alloy profile is heated to 195°C and kept at this temperature for 12 hours for aging treatment.
[0070] In this embodiment, the analysis results show that the performance indicators of the recycled 6101 aluminum alloy profile obtained without the additional addition of Si element are as follows: tensile strength is 210 MPa, and electrical conductivity is 55.6% IACS. Compared with the iron content in the commercially available 6101 aluminum alloy in this embodiment, the iron content in the recycled aluminum alloy is higher and the electrical conductivity is lower. The mass content of silicon element is 1.17 times the mass content of impurity iron element. The formation process of the iron-rich phase precipitated in the alloy consumes Si in the Al matrix. Compared with the commercially available 6101 aluminum alloy, the content of Si element in the Al matrix in the recycled 6101 aluminum alloy becomes lower due to the precipitation of a large amount of iron-rich phase, so that the number density of nanoscale magnesium silicon (Mg, Si) strengthening phase precipitated in the α-Al matrix during the aging treatment is smaller, such as Figure 6 As shown. Therefore, compared with the commercially available 6101 aluminum alloy of Example 1, the concentration of magnesium element dissolved in the α-Al matrix is greater, so that the lattice distortion is more serious, and the conductivity decreases more significantly. In order to prepare high-quality recycled 6101 aluminum alloy at low cost, the design is optimized and an appropriate amount of Si element is added on this basis to promote the precipitation of nanoscale magnesium silicon (Mg, Si) phase. On the one hand, the harm of lattice distortion caused by excessive Mg element dissolved in the α-Al matrix is reduced to improve the conductivity of the recycled 6101 aluminum alloy; on the other hand, increasing the number density of precipitation of nanoscale magnesium silicon (Mg, Si) phase is conducive to precipitation strengthening, so as to improve the mechanical properties of the recycled 6101 aluminum alloy. Example 5
[0071] In this embodiment, on the basis of recycled 6101 aluminum alloy (calculated by mass percentage, the content of main elements in the aluminum alloy is: 0.6% magnesium, 0.35% silicon, 0.3% iron, and the balance is Al), 0.2wt% Si element is added.
[0072] In this embodiment, the specific implementation steps are as follows:
[0073] (1) Place the recycled 6101 aluminum alloy ingot into a melting furnace for melting, and adjust the melt temperature to 750°C;
[0074] (2) adding 0.2 wt% Si element to the melt in the form of Al-12% Si master alloy and stirring for 10 minutes to obtain a uniform melt;
[0075] (3) A refining agent (based on mass percentage, its composition is 40% sodium cryolite and 46% fluoride salt) is introduced into the melt to react and prepare Al 5 Ti 1 B master alloy salt slag, 10% aluminum fluoride, 2% calcium fluoride, 2% potassium feldspar) and argon gas was introduced for purification, and then the melt temperature was adjusted to 690°C and allowed to stand for 10 minutes to obtain a 6101 aluminum alloy melt;
[0076] (4) pouring the 6101 aluminum alloy melt into a mold and cooling and solidifying it to obtain an aluminum alloy ingot;
[0077] (5) heating the aluminum alloy ingot to 470°C, keeping the temperature for 10 hours for homogenization treatment, and cooling the ingot to room temperature along with the furnace;
[0078] (6) heating the aluminum alloy ingot after homogenization treatment to 530° C. and keeping the temperature for 2 hours to perform solid solution treatment and quenching treatment;
[0079] (7) performing rolling deformation treatment on the ingot after solution treatment and quenching treatment at room temperature to obtain an aluminum alloy profile;
[0080] (8) The deformed aluminum alloy profile is heated to 195°C and kept at this temperature for 12 hours for aging treatment.
[0081] In this embodiment, the analysis results show that the mass content of silicon in the recycled 6101 aluminum alloy profile obtained after adding 0.2wt% Si is 1.83 times the mass content of impurity iron, and the performance indicators are as follows: tensile strength is 222 MPa, and electrical conductivity is 55.9% IACS. Figure 7 As shown, compared with Example 4 without additional addition of Si element, the number density of (Mg, Si) phase precipitated in the sample of this example during the aging treatment increases, and the tensile strength and electrical conductivity are increased by 12 MPa and 0.3% IACS respectively, with obvious effects. Example 6
[0082] In this embodiment, on the basis of recycled 6101 aluminum alloy (calculated by mass percentage, the content of main elements in the aluminum alloy is: 0.6% magnesium, 0.35% silicon, 0.3% iron, and the balance is Al), 0.3wt% Si element is added.
[0083] In this embodiment, the specific implementation steps are as follows:
[0084] (1) Place the recycled 6101 aluminum alloy ingot into a melting furnace for melting, and adjust the melt temperature to 750°C;
[0085] (2) adding 0.3 wt% Si element to the melt in the form of Al-12% Si master alloy and stirring for 10 minutes to obtain a uniform melt;
[0086] (3) A refining agent (based on mass percentage, its composition is 40% sodium cryolite and 46% fluoride salt) is introduced into the melt to react and prepare Al 5 Ti 1 B master alloy salt slag, 10% aluminum fluoride, 2% calcium fluoride, 2% potassium feldspar) and argon gas was introduced for purification, and then the melt temperature was adjusted to 710°C and allowed to stand for 10 minutes to obtain a 6101 aluminum alloy melt;
[0087] (4) pouring the 6101 aluminum alloy melt into a mold and cooling and solidifying it to obtain an aluminum alloy ingot;
[0088] (5) heating the aluminum alloy ingot to 470°C, keeping the temperature for 10 hours for homogenization, and cooling the ingot to room temperature along with the furnace;
[0089] (6) heating the aluminum alloy ingot after homogenization treatment to 530° C. and keeping the temperature for 2 hours to perform solid solution treatment and quenching treatment;
[0090] (7) performing rolling deformation treatment on the ingot after solution treatment and quenching treatment at room temperature to obtain an aluminum alloy profile;
[0091] (8) The deformed aluminum alloy profile is heated to 195°C and kept at this temperature for 12 hours for aging treatment.
[0092] In this embodiment, the analysis results show that in the recycled 6101 aluminum alloy profile obtained after adding 0.3wt% Si, the mass content of silicon is 2.17 times the mass content of impurity iron, and the performance indicators are as follows: tensile strength is 235 MPa, and electrical conductivity is 56.3% IACS. Figure 8As shown, compared with Example 4 without additional addition of Si element, the number density of (Mg, Si) phase precipitated in the sample of this example during the aging treatment is further increased, and the tensile strength and electrical conductivity are increased by 25 MPa and 0.7% IACS respectively. In comparison, the conductivity improvement effect is more significant.
[0093] It can be seen that after adding an appropriate amount of silicon to the 6101 aluminum alloy melt containing the impurity element iron, the number density of (Mg, Si) particles precipitated during the aging process increases. Figure 9-10 As shown in the figure, X-ray diffraction spectrum analysis shows that by adding 0.02wt%Si and 0.06wt%Si to the commercially available 6101 aluminum alloy containing the impurity element iron, the solute Mg in the α-Al matrix combines with the introduced Si and precipitates out as (Mg,Si) phase. On the one hand, the lattice distortion caused by excessive solid solution of Mg in the α-Al matrix is reduced, the lattice constant of the α-Al matrix is reduced, and the diffraction peak shifts to a large angle, thereby improving the electrical conductivity of the 6101 aluminum alloy; on the other hand, increasing the number density of the nanoscale (Mg,Si) precipitate phase is conducive to precipitation strengthening, thereby improving the mechanical properties of the 6101 aluminum alloy, which has significant economic and social benefits for reducing the power loss of aluminum wires used for electrical work throughout the country.
Claims
1. A method for reducing the harm of iron in 6101 aluminum alloy, characterized in that: The commercially available 6101 aluminum alloy melt is additionally added with an appropriate amount of Si so that the mass content of silicon is 3.7 to 4.1 times the mass content of impurity iron. The silicon content in the obtained 6101 aluminum alloy melt is 0.2 to 0.6 times higher than that of the corresponding commercially available 6101 aluminum alloy. Alternatively, an appropriate amount of Si is additionally added to the recycled 6101 aluminum alloy melt so that the mass content of silicon is 1.8 to 2.2 times the mass content of impurity iron, and the silicon content in the obtained 6101 aluminum alloy melt is increased by 0.6 to 1.0 times compared with the corresponding recycled 6101 aluminum alloy; The method for reducing the harm of iron in 6101 aluminum alloy comprises the following steps: first, clarifying the mass percentage of magnesium, silicon and impurity element iron in the aluminum alloy; second, placing the 6101 aluminum alloy in a smelting furnace for melting, and adjusting the melt temperature to 750°C; then adding Al-Si master alloy to the melt, and stirring to obtain a uniform 6101 aluminum alloy melt; then, adding a refining agent to the melt and introducing argon gas for purification, then adjusting the melt temperature to 690°C-710°C, standing for 10 minutes, and casting the melt into an aluminum alloy ingot; finally, the aluminum alloy ingot is subjected to a homogenization treatment at 470°C for 10 hours, a solution treatment and quenching treatment at 530°C for 2 hours, a rolling deformation treatment, and an aging treatment at 195°C for 12 hours, in order to obtain a high-quality 6101 aluminum alloy.
2. The method for reducing the harm of iron in 6101 aluminum alloy according to claim 1, characterized in that: Silicon is added to the commercially available 6101 aluminum alloy melt containing the impurity element iron, so that the mass content of silicon in the 6101 aluminum alloy melt is 4.1 times the mass content of the impurity iron. At the same time, the mass percentage of magnesium in the 6101 aluminum alloy melt is 0.6%. The yield strength, tensile strength, elongation and electrical conductivity of the 6101 aluminum alloy reach 195.33MPa, 216MPa, 13% and 58.13%IACS, respectively.
Citation Information
Cited By
Method for regulating and controlling structure and performance of high-Fe-content 6016 secondary aluminum alloy
CN120442971A