A high-vanadium content hydrogen-induced cracking resistant container steel plate and preparation method thereof

By increasing the V, Cr and Mo content, reducing the Mn content, and using a specific heat treatment process, a high vanadium content resistant hydrogen-induced cracking container steel plate was prepared, which solved the problem that existing steel plates are prone to hydrogen-induced cracking in harsh environments, and achieved High strength, good low temperature toughness and excellent anti-hydrocracking properties.

CN118639131BActive Publication Date: 2024-11-29ANGANG STEEL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411118569.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-29
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

Existing pressure vessel steel plates are prone to hydrogen-induced cracking problems in harsh corrosive environments, and the strength, low-temperature toughness and hydrogen-induced crack resistance of the steel plates are insufficient.

Method used

By increasing the content of V, Cr and Mo and reducing the content of Mn, a high-vana content anti-hydrogen cracking container steel plate with specific chemical composition was prepared, and a two-stage controlled rolling and cooling technology and normalized heat treatment were used to form bainite + iron. The grain size of the microstructure is 8 to 10.

Benefits of technology

The high strength, good low-temperature toughness and excellent anti-hydrogen cracking performance of the steel plate are achieved, reducing the cost of steel plate preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to a high-vanadium-content hydrogen-induced cracking-resistant container steel plate and a preparation method thereof. The chemical composition and weight percentage content of the steel plate are: C: 0.25%-0.30%, Si: 0.30%-0.40%, Mn: 0.90%-1.00%, P: ≤0.010%, S: ≤0.005%, Cr: 0.30%-0.50%, Mo: 0.15%-0.35%, V: 0.30%-0.40%, Al: 0.006%-0.008%, Cu: 0.20%-0.30%, and the balance is Fe and inevitable impurities. The present invention adopts smelting, continuous casting, heating, rolling and heat treatment processes to prepare the high-vanadium-content hydrogen-induced cracking-resistant container steel plate, and the steel plate has good strength, low-temperature toughness and hydrogen-induced cracking resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pressure vessel steel plates, in particular to a high-vanadium content hydrogen-induced cracking resistant vessel steel plate and a preparation method thereof. Background Art

[0002] Pressure vessels are important equipment for petrochemical enterprises to refine and store crude oil, chemical products and other products. Common problems include hydrogen sulfide stress corrosion cracking. As petrochemical products such as H2S and Cl-, which contain severely corrosive environmental media, are being mined one after another, the service environment of pressure vessel steel plates is becoming increasingly harsh. The physical and chemical reactions of the pressure vessel shell caused by the corrosive medium can easily lead to serious hazards such as hydrogen bulging, hydrogen sulfide stress corrosion cracking, and induced cracking.

[0003] In order to ensure the safe operation of pressure vessels, the steel plates used in pressure vessels are required to have not only good strength, low-temperature toughness and high-temperature service performance, but also excellent resistance to hydrogen-induced cracking.

[0004] The invention patent with publication number CN114318159A provides a 345MPa-grade container steel plate with resistance to hydrogen-induced cracking and a preparation method thereof. Its chemical composition is: C: 0.16-0.22%, Si: 0.01-0.50%, Mn: 1-2%, P: ≤0.010%, S: ≤0.001%, Ti: 0.03-0.13%, and the rest is Fe and unavoidable impurities. However, due to its high manganese content, segregation is prone to occur, which is detrimental to the plasticity and toughness of the steel.

[0005] The invention patent with publication number CN115896616A provides an easy-to-weld normalized pressure vessel steel plate and a manufacturing method. Its chemical composition is: C: 0.16~0.19%, Si: 0.15~0.40%, Mn: 1.45~1.65%, P: ≤0.010%, S: 0.003~0.010%, Ni: 0.40~0.80%, and other elements. The designed pressure vessel steel plate has a relatively complex composition and a high carbon equivalent setting range. The steel plate is prone to welding thermal cracks, which affects the processing and manufacturing of the steel plate.

[0006] The invention patent with publication number CN111748743A provides a corrosion-resistant steel for railway tank cars and a production method thereof. The chemical composition is designed to be: C 0.14-0.18%, Si 0.15-0.40%, Mn 1.25-1.65%, P≤0.020%, S≤0.005%, Cu 0.15-0.30%, Ni 0.20-0.40%, V 0.050-0.080%, Nb 0.010-0.020%, Ti0.008-0.020%, Sb 0.05-0.15%, and the balance is Fe and other elements. However, the disadvantage is that the P content in the steel plate is relatively high, inclusions are easily generated, which affects the resistance to hydrogen-induced cracking, and the tensile strength is relatively low, making it difficult to overcome different service environments.

[0007] Therefore, in view of the above situation, it is urgent to develop a hydrogen-induced cracking-resistant container steel plate with good strength and low-temperature toughness and a preparation method thereof. Summary of the invention

[0008] In order to overcome the defects of the prior art, the technical problem solved by the present invention is to provide a hydrogen-induced cracking resistant container steel plate with a high vanadium content and a preparation method thereof. The present invention increases the contents of elements V, Cr and Mo and reduces the content of Mn to obtain a hydrogen-induced cracking resistant container steel plate with good strength and low-temperature toughness.

[0009] In order to achieve the above object, the present invention adopts the following technical solutions:

[0010] A high-vanadium content hydrogen-induced cracking resistant container steel plate, the chemical composition and weight percentage content of the steel plate are:

[0011] C: 0.25% ~ 0.30%, Si: 0.30% ~ 0.40%, Mn: 0.90% ~ 1.00%, P: ≤ 0.010%, S: ≤ 0.005%, Cr: 0.30% ~ 0.50%, Mo: 0.15% ~ 0.35%, V: 0.30% ~ 0.40%, Al: 0.006% ~ 0.008%, Cu: 0.20% ~ 0.30%, the balance is Fe and unavoidable impurities.

[0012] The microstructure of the steel plate is bainite+ferrite structure, the grain size of the microstructure is 8-10 levels, and the size of carbides in the structure is 1-5 μm.

[0013] The thickness of the steel plate is 28-56 mm.

[0014] The mechanical properties of the steel plate are as follows: yield strength ReL≥540MPa, tensile strength Rm: 700-830MPa, elongation A≥19%, and -40°C impact absorption energy KV2≥100J.

[0015] The reasons for selecting the chemical elements and composition ranges for the steel plate of the present invention are briefly described below:

[0016] C forms various carbides or solid solutions with alloy elements in steel to strengthen the steel. It is an element that directly improves the strength of steel plates. Every 0.1% increase in carbon in steel can increase the tensile strength by about 70 MPa. However, too high a C content will result in poor toughness and plasticity of the steel. Therefore, the C content is limited to 0.25-0.30%.

[0017] Si has the functions of deoxidation and solid solution strengthening in steel, which can improve the yield strength of steel plates. A proper amount of Si can improve the toughness and hardenability of steel plates, reduce the tough-brittle transition temperature, and also improve the corrosion resistance of steel. Therefore, the Si content is limited to 0.30-0.40%.

[0018] Mn improves strength and toughness in steel by substitution, grain refinement and increasing the amount of ferrite, and is dissolved in the Fe matrix to improve the strength of the steel plate. As the Mn content increases, it can stabilize the austenite structure in the steel and reduce the critical cooling rate. However, if the Mn content is too high, it is easy to form segregation in the steel plate, which is not good for the plasticity and toughness of the steel. The generated MnS is easy to reduce the hydrogen resistance of the steel plate. Therefore, Mn is limited to 0.90~1.00%.

[0019] P is a harmful element in steel and is also an element that is very easy to segregate. Therefore, during the steelmaking process, the P content in steel should be reduced as much as possible. However, considering the cost factor and meeting the use requirements, it is sufficient to control it within the range that does not affect the performance, so the P content is controlled below 0.010%.

[0020] S is a harmful element in steel. It forms sulfides in steel, which are detrimental to the toughness and hydrogen resistance of steel. However, considering the operability and cost of steelmaking, S is controlled below 0.005%.

[0021] Cr is the main element of the present invention. As a strong carbide-forming element, it can improve the toughness and hardenability of the steel plate. A higher Cr content can make the steel plate have good corrosion resistance, delay the occurrence of initial corrosion of the steel plate, and promote the formation of bainite, a low-temperature phase transformation product. During the normalizing heat treatment process, the precipitated Cr-containing carbides can be fully dissolved in the matrix and refine the grain size, so the Cr content is limited to between 0.30 and 0.50%.

[0022] Mo is the main element of the present invention, which can improve the strength, toughness and hardenability of steel. In the two-stage rolling process, it can reduce the austenite phase area, promote bainite transformation, and generate Mo-containing carbides to inhibit the formation of ferrite; through solid solution strengthening, it dissolves in austenite and ferrite to improve the yield strength of steel and the tempering resistance of steel plates; after quenching and tempering heat treatment, Mo can form stable carbides, improve the corrosion resistance of steel, and also improve the low-temperature toughness of steel. Therefore, the Mo content is limited to between 0.15 and 0.35%.

[0023] V is the main element of the present invention, which can be dissolved into austenite at high temperature, and improve the strength and hardenability of steel through solid solution strengthening; V exists in the form of carbonitride in steel, and the increase of vanadium carbide precipitation can also inhibit grain boundary movement and grain growth, which can ensure the strength and hardness of steel. Appropriate increase of V can improve the strength of the core of thick steel plate by dispersion strengthening; microalloying can promote the increase of V-containing carbides formed in steel, pinning at the grain boundary, reducing the expansion of hydrogen-induced cracks, and can improve the hydrogen storage capacity and hydrogen corrosion resistance of steel plate in low temperature and high pressure service environment. However, if the V content is too high, not only the cost will increase, but also the size of the precipitate will increase, so the V content is limited to 0.30-0.40%.

[0024] Al is the main deoxidizer in steel, which can fix N elements, refine grains, and improve the toughness of steel. Appropriate Al content can improve the steel's oxidation resistance and corrosion resistance to high-temperature gases, but too high Al content will affect the thermoplasticity of the steel plate. Therefore, the Al content is limited to 0.006-0.008%.

[0025] Cu is an element that expands the austenite zone. Its solubility in ferrite decreases as the temperature decreases. Through proper heat treatment, precipitation strengthening can occur in the structure. Cu can also help the steel plate obtain good low-temperature toughness and improve the corrosion resistance of the steel. Therefore, the Cu content is limited to 0.20-0.30%.

[0026] The present invention also provides a method for preparing a high-vanadium content hydrogen-induced cracking resistant container steel plate, the main method comprising smelting, continuous casting, heating, rolling and heat treatment; the specific steps are as follows:

[0027] Smelting: Before smelting, the molten iron is pretreated for desulfurization to control the S element below 0.005%; after blowing argon through the ladle, the LF furnace is used for refining to adjust the composition and deep dephosphorization and desulfurization are carried out to remove harmful elements in the molten iron, and the P element is controlled below 0.010%. During this period, the argon soft blowing time is guaranteed to be ≥10min, and the refining time is 60-80min; RH vacuum treatment is used for further refining and composition adjustment, and the vacuum treatment time is 60-90min through bottom argon blowing, and the vacuum degree is ≤5.0mbar to remove gas and inclusions in the molten steel, and control the gas elements H in the molten steel to be ≤0.0005%, O ≤0.0010%, and N ≤0.006%;

[0028] Continuous casting: The casting temperature of molten steel in the tundish is 1360~1420℃. Argon is used to protect the casting process. The light reduction technology is adopted. The reduction is controlled at 1~5mm, and the billet drawing speed is controlled at 0.6~1.0m / min. The secondary cooling water parameter is controlled at 5000~5900L / min, the casting superheat is guaranteed at 20~25℃, and the billet straightening temperature is controlled at 1000±30℃ to obtain a continuous casting billet with a thickness of 250~360mm.

[0029] Heating: The continuous casting billet is heated after being slowly cooled in the stack. The heating is divided into preheating section, heating section and soaking section.

[0030] Rolling: After the billet is out of the furnace, a two-stage controlled rolling and controlled cooling technology is adopted; the starting temperature of rough rolling is controlled at 1150~1180℃, the rolling speed is controlled at 2.1~2.8m / s, and the single-pass reduction rate of rough rolling is controlled at 12%~18%, and the total reduction rate of rough rolling is ≥60%; the starting temperature of finishing rolling is 890~920℃, the rolling speed is controlled at 3.0~4.2m / s, the rolling temperature of the final rolling pass is controlled at 815~835℃, the single-pass reduction rate of finishing rolling is ≥10%, and the total reduction rate of finishing rolling is ≥55%; controlled cooling is carried out after rolling, the starting cooling temperature is 740~770℃, the red return temperature is 440~490℃, the cooling rate is 13~25℃ / s, and then the steel plate is stacked and slowly cooled;

[0031] Heat treatment: The rolled steel plate is stacked and slowly cooled before normalizing. The normalizing temperature is 880-900°C, and the normalizing heating rate is 2.2-3.5min / mm. After the heat treatment, it is weakly cooled to 450-500°C, with a cooling rate of 5-16°C / s, and finally air-cooled to room temperature.

[0032] In the step 3), the temperature range of the preheating section is 600-750°C, the temperature range of the heating section is 1240-1280°C, and the temperature range of the soaking section is 1180-1220°C; the total time in the furnace is 240-300 minutes.

[0033] In the step 4), the stacking slow cooling temperature is 350-400° C., the stacking quantity is 8-13 sheets, and the stacking time is 24-36 hours.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] The present invention reduces the Mn content in the steel and appropriately increases the C content, thereby ensuring that the steel plate has sufficient strength and reducing the cost of preparing the steel plate.

[0036] The present invention increases the V content of the steel, and V ensures that the steel plate has high strength and sufficient low-temperature toughness after normalizing through the effects of solid solution strengthening, precipitation strengthening and grain refinement. After grain refinement, large-angle grain boundaries in the structure increase, thereby inhibiting the extension of cracks. The V carbide content in the steel increases, so that it is pinned at the grain boundaries, reducing the extension of hydrogen-induced cracks in the steel, and can also improve the hydrogen storage capacity and hydrogen corrosion resistance of the steel plate in a low-temperature and high-pressure service environment.

[0037] The present invention can improve the hardenability and strength of the steel plate by increasing the Cr and Mo elements, generate strong carbides to stabilize the carbon in the steel, and enable the steel plate to have good resistance to hydrogen-induced cracking in a hydrogen sulfide environment medium. The Cr and Mo elements promote the formation of bainite, a low-temperature phase transformation product, during the two-stage rolling process, and the formation of Mo-containing carbides can inhibit the formation of ferrite.

[0038] The present invention adopts two-stage controlled rolling and controlled cooling, combined with normalizing heat treatment, to ensure that the finished product structure is bainite + ferrite structure, the microstructure grain size is 8-10 levels, the carbide size in the structure is between 1-5 μm, and the distribution is uniform, thereby reducing the damage of ferrite to the strength of the steel plate, so that the steel plate has excellent strength and toughness, refines the grains, promotes the formation of carbides, and improves the performance of resistance to hydrogen-induced cracking. DETAILED DESCRIPTION

[0039] The specific embodiments of the present invention are further described below:

[0040] The present invention provides a high-vanadium content hydrogen-induced cracking resistant container steel plate, the chemical composition and weight percentage content of the steel plate are:

[0041] C: 0.25% ~ 0.30%, Si: 0.30% ~ 0.40%, Mn: 0.90% ~ 1.00%, P: ≤ 0.010%, S: ≤ 0.005%, Cr: 0.30% ~ 0.50%, Mo: 0.15% ~ 0.35%, V: 0.30% ~ 0.40%, Al: 0.006% ~ 0.008%, Cu: 0.20% ~ 0.30%, the balance is Fe and unavoidable impurities.

[0042] The microstructure of the steel plate is bainite+ferrite structure, the grain size of the microstructure is 8-10 levels, and the size of carbides in the structure is 1-5 μm.

[0043] The thickness of the steel plate is 28-56 mm.

[0044] The mechanical properties of the steel plate are as follows: yield strength ReL≥540MPa, tensile strength Rm: 700-830MPa, elongation A≥19%, and -40°C impact absorption energy KV2≥100J.

[0045] The present invention also provides a method for preparing a high-vanadium content hydrogen-induced cracking resistant container steel plate, the main method comprising smelting, continuous casting, heating, rolling and heat treatment; the specific steps are as follows:

[0046] Smelting: Before smelting, the molten iron is pretreated for desulfurization to control the S element below 0.005%; after blowing argon through the ladle, the LF furnace is used for refining to adjust the composition and deep dephosphorization and desulfurization are carried out to remove harmful elements in the molten iron, and the P element is controlled below 0.010%. During this period, the argon soft blowing time is ensured to be ≥10min, and the refining time is 60-80min; RH vacuum treatment is used for further refining and composition adjustment, and the vacuum treatment time is 60-90min through bottom argon blowing, and the vacuum degree is ≤5.0mbar to remove gas and inclusions in the molten steel, and control the gas elements H in the molten steel to be ≤0.0005%, O ≤0.0010%, and N ≤0.006%.

[0047] Continuous casting: The casting temperature of molten steel in the tundish is 1360~1420℃. Argon is used to protect the pouring throughout the pouring process. The light reduction technology is adopted, and the reduction amount is controlled at 1~5mm. The billet drawing speed is controlled at 0.6~1.0m / min. This technology is conducive to eliminating internal defects of the billet, improving the surface quality of the billet, and refining the billet grains. The secondary cooling water parameters are controlled at 5000~5900L / min, the pouring superheat is guaranteed to be 20~25℃, and the billet straightening temperature is controlled at 1000±30℃ to improve the center segregation and center looseness of the billet, improve the quality of the continuous casting billet, and obtain a continuous casting billet with a thickness of 250~360mm. Finally, the slab is cleaned, slowly cooled, and the quality of the continuous casting billet is inspected.

[0048] Heating: The continuous casting billet is heated after being slowly cooled in the stack. The heating is divided into preheating section, heating section and soaking section.

[0049] Rolling: After the billet is out of the furnace, a two-stage controlled rolling and controlled cooling technology is adopted; the rough rolling start temperature is controlled at 1150~1180℃, the rolling speed is controlled at 2.1~2.8m / s, and the rough rolling single pass reduction rate is controlled at 12%~18%, and the total rough rolling reduction rate is ≥60%, so as to fully refine the austenite grains and ensure that the dynamic recrystallization of the steel plate in the first stage of rolling process is complete; the finishing rolling start temperature is 890~920℃, the rolling speed is controlled at 3.0~4.2m / s, the final rolling pass rolling temperature is controlled at 815~835℃, and the finishing rolling single pass rolling speed is controlled at 120~180℃. The reduction rate of each pass is ≥10%, and the total reduction rate of the finishing pass is ≥55%. The grains are further flattened and elongated. The increase in the grain boundary area provides more nucleation sites for the subsequent phase transformation process. By controlling the total reduction rate of rough rolling and finishing rolling, the grains of the steel plate are guaranteed to be sufficiently refined and the internal defects of the steel plate are eliminated. After rolling, controlled cooling is carried out, with a cooling start temperature of 740-770°C, a red return temperature of 440-490°C, and a cooling rate of 13-25°C / s to ensure fine grains, promote the formation of fine precipitates, and improve the mechanical properties of the steel plate. The steel plate is then stacked and slowly cooled.

[0050] Heat treatment: After rolling, the steel plate is stacked and slowly cooled before normalizing. The normalizing temperature is 880-900℃, and the normalizing heating rate is 2.2-3.5min / mm. After the heat treatment, it is weakly cooled to 450-500℃, with a cooling rate of 5-16℃ / s, and finally air-cooled to room temperature. Through normalizing heat treatment + weak cooling, the steel plate structure is uniform, and the carbides in the structure are evenly distributed, ensuring that the steel plate has high strength and good low-temperature performance. The structure is bainite + ferrite, the grain size is 8-10, and the average size of carbides is between 1 and 5μm.

[0051] In step 3), the temperature range of the preheating section is 600-750°C, the temperature range of the heating section is 1240-1280°C, and the temperature range of the soaking section is 1180-1220°C; the total time in the furnace is 240-300 minutes. By heating the ingot in three stages, the temperature of the core of the ingot reaches 1180-1220°C, ensuring that the ingot structure is completely austenitic.

[0052] In step 4), the stacking slow cooling temperature is 350-400°C, the stacking quantity is 8-13 sheets, and the stacking time is 24-36 hours, so that H and O in the steel plate have enough time to be eliminated.

[0053] The specific values ​​of the element contents of each embodiment and comparative example are listed in Table 1. Each embodiment is prepared according to the above-mentioned preparation method to prepare a high-vanadium content hydrogen-induced cracking resistant container steel plate. The smelting and continuous casting process parameters of each embodiment and comparative example are shown in Table 2. The rolling process parameters of each embodiment and comparative example are shown in Table 3. The cooling and heat treatment process parameters of each embodiment and comparative example are shown in Table 4. The mechanical properties of each embodiment and comparative example are shown in Table 5. The test results of carbide size, grain size and non-metallic inclusions of each embodiment and comparative example are shown in Table 6.

[0054] Table 1 Chemical composition of the examples (wt%)

[0055] Example C Si Mn P S Cr Mo V Al Cu 1 0.25 0.32 0.93 0.010 0.005 0.35 0.35 0.40 0.006 0.24 2 0.25 0.33 0.95 0.010 0.005 0.31 0.34 0.38 0.006 0.29 3 0.26 0.35 0.95 0.009 0.005 0.49 0.24 0.38 0.006 0.21 4 0.27 0.35 0.96 0.010 0.005 0.41 0.28 0.35 0.007 0.28 5 0.29 0.37 0.97 0.009 0.005 0.45 0.35 0.36 0.007 0.23 6 0.29 0.39 1.00 0.009 0.005 0.33 0.20 0.35 0.007 0.26 7 0.25 0.38 1.00 0.008 0.004 0.45 0.25 0.31 0.008 0.21 8 0.28 0.39 1.00 0.008 0.004 0.38 0.22 0.30 0.008 0.30 9 0.26 0.39 0.91 0.008 0.003 0.39 0.18 0.40 0.006 0.20 10 0.30 0.39 0.90 0.008 0.003 0.44 0.27 0.40 0.008 0.27 11 0.28 0.40 0.92 0.009 0.003 0.45 0.31 0.32 0.007 0.25 Comparative Example 0.30 0.31 0.95 0.009 0.004 0.36 0.15 0.24 0.006 0.22

[0056] Table 2 Smelting and continuous casting process parameters of the embodiment

[0057]

[0058] Table 3 Rolling process parameters of the embodiment

[0059]

[0060] Table 4 Cooling and heat treatment process parameters of the embodiment

[0061]

[0062] Table 5 Mechanical properties of the examples

[0063]

[0064] Note: The sample is immersed in solution A, filled with nitrogen for 60-80 minutes, immersed for 96-98 hours, and the solution temperature is 25±3°C. Solution A is (5% by mass NaCl + 0.5% by mass acetic acid solution).

[0065] Table 6 Carbide size, grain size and non-metallic inclusion test results of the examples

[0066]

[0067] The HIC resistance of the steel plate was measured according to GB / T 8650-2015 "Evaluation Method for Hydrogen-Induced Cracking Resistance of Pipeline Steel and Pressure Vessel Steel". The measurement results all meet the requirements of crack length percentage CLR≤5%, crack thickness percentage CTR≤1.5%, and crack sensitivity percentage CSR≤1%, indicating good hydrogen-induced cracking resistance. According to the above results, it can be concluded that the high-vanadium hydrogen-induced cracking resistance container steel plate prepared by the present invention has good strength, low-temperature toughness and hydrogen-induced cracking resistance.

[0068] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, and these simple modifications all belong to the protection scope of the present invention. It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations. In addition, the various different embodiments of the present invention can also be arbitrarily combined, as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A high vanadium content hydrogen-induced cracking resistant container steel plate, characterized in that: The chemical composition and weight percentage of the steel plate are: C: 0.25% to 0.30%, Si: 0.30% to 0.40%, Mn: 0.90% to 1.00%, P: ≤ 0.010%, S: ≤ 0.005%, Cr: 0.30% to 0.50%, Mo: 0.15% to 0.35%, V: 0.30% to 0.40%, Al: 0.006% to 0.008%, Cu: 0.20% to 0.30%, the balance is Fe and unavoidable impurities; The method for preparing the steel plate mainly includes smelting, continuous casting, heating, rolling and heat treatment; the specific steps are as follows: 1) Smelting: Before smelting, the molten iron is pretreated for desulfurization to control the S element below 0.005%; after blowing argon through the ladle, the LF furnace is used for refining to adjust the composition and deep dephosphorization and desulfurization are carried out to remove harmful elements in the molten iron, and the P element is controlled below 0.010%. During this period, the argon soft blowing time is guaranteed to be ≥10min, and the refining time is 60-80min; RH vacuum treatment is used for further refining and composition adjustment, and the vacuum treatment time is 60-90min through bottom argon blowing, and the vacuum degree is ≤5.0mbar to remove gas and inclusions in the molten steel, and control the gas elements H in the molten steel to be ≤0.0005%, O ≤0.0010%, and N ≤0.006%; 2) Continuous casting: The casting temperature of the molten steel in the tundish is 1360~1420℃. Argon is used to protect the casting process. The light reduction technology is adopted. The reduction is controlled at 1~5mm, and the billet drawing speed is controlled at 0.6~1.0m / min. The secondary cooling water parameter is controlled at 5000~5900L / min, the pouring superheat is guaranteed at 20~25℃, and the billet straightening temperature is controlled at 1000±30℃ to obtain a continuous casting billet with a thickness of 250~360mm. 3) Heating: The continuous casting billet is heated after being slowly cooled in the stack. The heating is divided into preheating section, heating section and soaking section; 4) Rolling: After the billet is out of the furnace, a two-stage controlled rolling and controlled cooling technology is adopted; the rough rolling start temperature is controlled at 1150~1180℃, the rolling speed is controlled at 2.1~2.8m / s, and the rough rolling single pass reduction rate is controlled at 12%~18%, and the rough rolling total reduction rate is ≥60%; the finishing rolling start temperature is 890~920℃, the rolling speed is controlled at 3.0~4.2m / s, the final rolling pass rolling temperature is controlled at 815~835℃, the finishing single pass reduction rate is ≥10%, and the finishing pass total reduction rate is ≥55%; controlled cooling is carried out after rolling, the start cooling temperature is 740~770℃, the red return temperature is 440~490℃, the cooling rate is 13~25℃ / s, and then the steel plate is stacked and slowly cooled; 5) Heat treatment: The rolled steel plate is stacked and slowly cooled before normalizing. The normalizing temperature is 880-900°C, and the normalizing heating rate is 2.2-3.5min / mm. After the heat treatment, it is weakly cooled to 450-500°C, with a cooling rate of 5-16°C / s, and finally air-cooled to room temperature.

2. The high vanadium content hydrogen-induced cracking resistant container steel plate according to claim 1, characterized in that: The microstructure of the steel plate is bainite+ferrite structure, the grain size of the microstructure is 8-10 levels, and the size of carbides in the structure is 1-5 μm.

3. The high vanadium content hydrogen-induced cracking resistant container steel plate according to claim 1, characterized in that: The thickness of the steel plate is 28-56 mm.

4. The high vanadium content hydrogen-induced cracking resistant container steel plate according to claim 1, characterized in that: The mechanical properties of the steel plate are as follows: yield strength ReL≥540MPa, tensile strength Rm: 700-830MPa, elongation A≥19%, and -40°C impact absorption energy KV2≥100J.

5. The high vanadium content hydrogen-induced cracking resistant container steel plate according to claim 1, characterized in that: In the step 3), the temperature range of the preheating section is 600-750°C, the temperature range of the heating section is 1240-1280°C, and the temperature range of the soaking section is 1180-1220°C; the total time in the furnace is 240-300 minutes.

6. The high vanadium content hydrogen-induced cracking resistant container steel plate according to claim 1, characterized in that: In the step 4), the stacking slow cooling temperature is 350-400° C., the stacking quantity is 8-13 sheets, and the stacking time is 24-36 hours.

Citation Information

Patent Citations

  • Corrosion-resistant steel for railway tank car and production method thereof

    CN111748743A

  • 345MPa-grade container steel plate with hydrogen induced cracking resistance and preparation method of 345MPa-grade container steel plate

    CN114318159A

  • Normalizing pressure vessel steel plate easy to weld and manufacturing method

    CN115896616A

  • Nitrocarburized crankshaft and method of manufacturing the same

    CN104131248A

  • Steel for hot stamping forming, hot stamping forming process and hot stamping forming component