A quantitative preparation method for a nano inorganic composite oxide high-selectivity heat-absorbing film layer

By adding nano-inorganic composite oxide materials in the preparation process of the heat-absorbing film layer and using radio frequency plasma technology to process it, the problems of low absorption, high emissivity and poor weather resistance of the heat-absorbing film layer are solved, and high selectivity and Improved weather resistance.

CN118639233BActive Publication Date: 2024-11-12DEZHOU JINNAIER NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411099817.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-12
Estimated Expiration
2044-08-12
Patent Text Reader

Abstract

The invention relates to a quantitative preparation method of a nano inorganic composite oxide high-selectivity heat absorption film layer, comprising the steps of: mixing manganese acetate, iron oxide, nickel chloride, copper oxide, nano carbon material, solvent, nano chromium trioxide powder, surfactant and film-forming aid, and obtaining slurry; coating the slurry evenly on an aluminum foil, drying, sintering, cooling to room temperature, and then soaking the slurry in an impregnation liquid, taking the slurry out, air-drying and performing plasma treatment to obtain a nano inorganic composite oxide high-selectivity heat absorption film layer; the nano inorganic composite oxide high-selectivity heat absorption film layer prepared by the invention has high absorptivity, low emissivity and high selectivity; after being exposed to the sun outdoors for 280 days, the surface of the film layer does not change, and no cracks or shedding occurs, and the film layer has excellent weather resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of heat absorption film preparation, in particular to a quantitative preparation method of a nano inorganic composite oxide high-selectivity heat absorption film layer. Background Art

[0002] Solar energy is a huge, permanent, pollution-free energy source. my country is extremely rich in solar energy resources. Vigorously developing and utilizing solar energy is of great significance to the national economy and people's lives. There are three main ways to apply solar energy: thermal utilization, light utilization, and photochemical action. From the current technical conditions, thermal utilization is an economical and realistic development direction. In the internal heat utilization of solar energy, researching and developing heat-absorbing films with excellent performance and low cost is an important topic in this field.

[0003] Chinese patent CN108610662A: Nano black chromium highly selective heat absorption film layer formula and preparation method thereof, the raw materials are composed of substrate, nano chromium trioxide powder and ethanol, the substrate includes manganese acetate, ferric chloride, nickel chloride and cupric chloride, and the mass ratio of each component used in the substrate is: manganese acetate: ferric chloride: cupric chloride: nickel chloride is 3~5:1~3:2~4:1.

[0004] Chinese patent CN112063260A: relates to the field of heat-absorbing film production, specifically to a method for preparing a nano black chromium highly selective heat-absorbing film layer; the highly selective heat-absorbing film layer of the present invention is prepared by fully dispersing the light-absorbing material in an isopropanol solution and then using a coating process to prepare the heat-absorbing film layer.

[0005] Chinese patent CN113583517A: discloses a method for preparing a selective heat-absorbing film layer for a high-efficiency large-area flat-plate solar collector, wherein a transition metal composite oxide pigment is prepared by a solid phase method through high-temperature calcination, grinding, crystallization, re-calcination, crushing, and filtering, and then a color paste is prepared and then a film layer is prepared. The side of the substrate to be coated is heated to a semi-molten state, and the color paste is placed in an ultrasonic generator, and the slurry is atomized by ultrasonic cavitation effect, and then transported to a spiral magnetic field accelerator by compressed air. Under the condition of magnetic field acceleration, it bombards the surface of the semi-molten substrate, and the color paste will penetrate into the semi-molten substrate molecules. During the penetration process, the diluent and auxiliary agent in the color paste will volatilize rapidly and cool the substrate, forming a transition metal composite oxide embedded in the surface of the substrate; through the atomization effect, the pigment molecules are evenly distributed on the surface of the substrate, and a uniform, dense, heat-absorbing film layer with a thickness not exceeding 100 nanometers is obtained.

[0006] However, the heat-absorbing film layer prepared by the prior art has the technical problems of low absorptivity, high emissivity and poor selectivity; the film layer is prone to fall off over time and has poor weather resistance. Summary of the invention

[0007] The purpose of the present invention is to provide a quantitative preparation method of a nano inorganic composite oxide highly selective heat absorption film layer, and also to provide a method for preparing an impregnation liquid, so as to solve the technical problems in the above-mentioned background technology.

[0008] The objective of the present invention is achieved through the following technical solutions:

[0009] A quantitative preparation method of a nano inorganic composite oxide high-selectivity heat-absorbing film layer, the operating steps of which are:

[0010] S1: Weigh 1-5 parts of manganese acetate, 1-5 parts of iron oxide, 0.1-1 parts of nickel chloride, 1-5 parts of copper oxide, 5-10 parts of nanocarbon material, and 80-100 parts of solvent by weight, add them into a reaction kettle, and stir and mix evenly for 70-100 minutes;

[0011] S2: Continue to add 5-10 parts of nano chromium trioxide powder, 0.1-1 parts of surfactant, and 0.1-1 parts of film-forming aid into the reactor, and stir and mix for 20-50 minutes to obtain slurry;

[0012] S3: The slurry is evenly coated on the aluminum foil, dried, sintered, cooled to room temperature, and then immersed in an impregnation liquid, the temperature is increased to 40-50°C, the immersion time is 10-20 hours, taken out, and dried to obtain a heat-absorbing film layer substrate;

[0013] S4: Plasma treatment, placing the heat-absorbing film layer substrate obtained in step S3 in a radio frequency plasma device, setting the radio frequency power to 100-200 watts, and controlling the volume ratio of ammonia: tungsten hexafluoride mixed gas to (1-1.5): (0.03-0.06), and the flow rate of the mixed gas to 10-20 ml per minute; using a radio frequency glow plasma technology with a frequency of 13.56 MHz for 20-40 minutes to treat the heat-absorbing film layer substrate. Through this process, a nano-inorganic composite oxide film layer with high selective heat absorption performance is finally prepared.

[0014] Furthermore, the nano-carbon material is one of carbon fiber, carbon black, graphene, carbon nanotube, carbon nanohorn, and onion-shaped carbon.

[0015] Furthermore, the solvent is selected from methanol, ethanol, propanol or isopropanol.

[0016] Furthermore, the surfactant is one of linear alkylbenzene sulfonate sodium, fatty alcohol polyoxyethylene ether sodium sulfate, fatty alcohol polyoxyethylene ether ammonium sulfate, sodium lauryl sulfate, nonylphenol polyoxyethylene ether, diethanolamide stearic acid glycerol monoester, and fatty alcohol polyoxyethylene ether.

[0017] Furthermore, the film-forming aid is one of ethylene glycol, propylene glycol, hexylene glycol, methyl benzyl alcohol, dodecyl alcohol, ethylene glycol ether, propylene glycol ethyl ether, ethylene glycol butyl ether, propylene glycol butyl ether, glycol ethers and acetate, turpentine, and dipentene pine oil.

[0018] Furthermore, the drying temperature of S3 is 60-80° C. and the drying time is 5-10 hours.

[0019] Furthermore, the sintering of S3 is firstly heated to 110-150°C, kept at this temperature for 1-3 hours, and then heated to 400-600°C, kept at this temperature for 3-5 hours.

[0020] Furthermore, the composition of the impregnation solution is: 0.005-0.05 parts of 2-allyl-5,5-dimethyl-1,3,2-dioxaborol CAS No.: 911482-75-2, 0.7-3 parts of zirconium acrylate, 100-120 parts of DMF, stirred at 50-70°C for 1-3h to obtain the impregnation solution.

[0021] Reaction mechanism:

[0022] 1. Addition reaction between amino group and alkenyl group: Under alkaline environment, through the action of ammonia, amino group reacts with olefins in 2-allyl-5,5-dimethyl-1,3,2-dioxaborol and zirconium acrylate. This step is the key process to form new chemical bonds.

[0023] 2. Introduction of complexes: Through the action of plasma tungsten hexafluoride, tungsten complexes are introduced into the film layer, which may have an important impact on the structure and performance of the film layer;

[0024] 3. Introduction of borane and zirconium complexes: In the previous steps, borane and zirconium complexes were also introduced into the membrane layer. The addition of these substances further enriched the chemical composition of the membrane layer and provided a basis for subsequent performance optimization.

[0025] Technical effects:

[0026] 1. Improve the absorption rate: Through the above chemical reaction, the absorption rate of the film layer is significantly improved, enabling it to absorb heat more effectively;

[0027] 2. Reduce emissivity: The emissivity of the film layer is reduced, which helps to retain the absorbed heat, reduce energy loss, and thus improve energy utilization efficiency;

[0028] 3. Enhanced selectivity: The prepared nano-inorganic composite oxide heat-absorbing film layer has high selectivity and can effectively absorb heat within a specific wavelength range, while having low emissivity for other wavelengths. DETAILED DESCRIPTION

[0029] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the following is a detailed description in combination with embodiments and comparative examples:

[0030] 1. Absorption and emissivity test: using Platinum Elmer UV-visible near-infrared spectrophotometer;

[0031] 2. Weather resistance test: After the heat-absorbing film layer is exposed to the sun outdoors for 280 days, observe the surface appearance.

[0032] Example 1: A quantitative preparation method of a nano inorganic composite oxide high-selectivity heat absorption film layer, the operation steps are as follows:

[0033] S1: Weigh 1g manganese acetate, 1g iron oxide, 0.1g nickel chloride, 1g copper oxide, 5g nanocarbon material, and 80g solvent, add them into a reactor, and stir and mix evenly for 70min;

[0034] S2: Continue to add 5g of nano chromium trioxide powder, 0.1g of surfactant, and 0.1g of film-forming aid into the reactor, stir and mix for 20min to obtain slurry;

[0035] S3: The slurry is evenly coated on the aluminum foil, dried, sintered, cooled to room temperature, and then immersed in an impregnation liquid, the temperature is raised to 40°C, the immersion time is 10 hours, taken out, and dried to obtain a heat-absorbing film layer substrate;

[0036] S4: Plasma treatment, placing the heat-absorbing film layer substrate obtained in step S3 in a radio frequency plasma device, setting the radio frequency power to 100 watts, and controlling the volume ratio of ammonia: tungsten hexafluoride mixed gas to 1:0.03, and the flow rate of the mixed gas to 10 ml per minute; using a radio frequency glow plasma technology with a frequency of 13.56 MHz for 20 minutes to treat the heat-absorbing film layer substrate. Through this process, a nano-inorganic composite oxide film layer with high selective heat absorption performance is finally prepared.

[0037] The nano carbon material is carbon fiber.

[0038] The solvent is methanol.

[0039] The surfactant is linear sodium alkylbenzene sulfonate.

[0040] The film-forming aid is ethylene glycol.

[0041] The drying temperature of S3 is 60° C. and the drying time is 5 hours.

[0042] The sintering of S3 is firstly heated to 110°C, kept at this temperature for 1 hour, and then heated to 400°C, kept at this temperature for 3 hours.

[0043] The composition of the impregnation solution is as follows: 0.005 g of 2-allyl-5,5-dimethyl-1,3,2-dioxaborol CAS No.: 911482-75-2, 0.7 g of zirconium acrylate, and 100 g of DMF are stirred at 50° C. for 1 hour to obtain the impregnation solution.

[0044] Example 2: A quantitative preparation method of a nano inorganic composite oxide high-selectivity heat absorption film layer, the operation steps are as follows:

[0045] S1: Weigh 2g manganese acetate, 2g iron oxide, 0.5g nickel chloride, 2g copper oxide, 6g nanocarbon material, and 85g solvent, add them into a reactor, and stir and mix evenly for 80min;

[0046] S2: Continue to add 6g of nano chromium trioxide powder, 0.5g of surfactant, and 0.5g of film-forming aid into the reactor, stir and mix for 30min to obtain slurry;

[0047] S3: The slurry is evenly coated on the aluminum foil, dried, sintered, cooled to room temperature, and then immersed in an impregnation liquid, heated to 45°C, immersed for 14 hours, taken out, and dried to obtain a heat-absorbing film layer substrate;

[0048] S4: Plasma treatment, placing the heat-absorbing film layer substrate obtained in step S3 in a radio frequency plasma device, setting the radio frequency power to 150 watts, and controlling the volume ratio of ammonia: tungsten hexafluoride mixed gas to 1.2:0.04, and the flow rate of the mixed gas to 14 ml per minute; using a radio frequency glow plasma technology with a frequency of 13.56 MHz for 25 minutes to treat the heat-absorbing film layer substrate. Through this process, a nano-inorganic composite oxide film layer with high selective heat absorption performance is finally prepared.

[0049] The nano carbon material is carbon black.

[0050] The solvent is ethanol.

[0051] The surfactant is fatty alcohol polyoxyethylene ether sodium sulfate.

[0052] The film-forming aid is propylene glycol.

[0053] The drying temperature of S3 is 65° C. and the drying time is 6 hours.

[0054] The sintering of S3 is firstly heated to 120°C, kept at this temperature for 2 hours, and then heated to 450°C, kept at this temperature for 4 hours.

[0055] The composition of the impregnation solution is as follows: 0.02g of 2-allyl-5,5-dimethyl-1,3,2-dioxaborol CAS No.: 911482-75-2, 1g of zirconium acrylate, and 105g of DMF are stirred at 55°C for 2h to obtain the impregnation solution.

[0056] Example 3: A quantitative preparation method of a nano inorganic composite oxide high-selectivity heat absorption film layer, the operation steps are as follows:

[0057] S1: Weigh 4g manganese acetate, 4g iron oxide, 0.8g nickel chloride, 4g copper oxide, 8g nanocarbon material, and 95g solvent, add them into a reactor, and stir and mix evenly for 90min;

[0058] S2: Continue to add 9 g of nano chromium trioxide powder, 0.8 g of surfactant, and 0.8 g of film-forming aid into the reactor, stir and mix for 40 min to obtain slurry;

[0059] S3: The slurry is evenly coated on the aluminum foil, dried, sintered, cooled to room temperature, and then immersed in an impregnation liquid, the temperature is raised to 45°C, the immersion time is 18 hours, taken out, and dried to obtain a heat-absorbing film layer substrate;

[0060] S4: Plasma treatment, placing the heat-absorbing film layer substrate obtained in step S3 in a radio frequency plasma device, setting the radio frequency power to 150 watts, and controlling the volume ratio of ammonia: tungsten hexafluoride mixed gas to 1.4:0.05, and the flow rate of the mixed gas to 18 ml per minute; using a radio frequency glow plasma technology with a frequency of 13.56 MHz for 35 minutes to treat the heat-absorbing film layer substrate. Through this process, a nano-inorganic composite oxide film layer with high selective heat absorption performance is finally prepared.

[0061] The nano carbon material is graphene.

[0062] The solvent is propanol.

[0063] The surfactant is fatty alcohol polyoxyethylene ether ammonium sulfate.

[0064] The film-forming aid is hexanediol.

[0065] The drying temperature of S3 is 75° C. and the drying time is 8 hours.

[0066] The sintering of S3 is firstly heated to 140°C, kept at this temperature for 2 hours, and then heated to 550°C, kept at this temperature for 4 hours.

[0067] The composition of the impregnation solution is as follows: 0.04g of 2-allyl-5,5-dimethyl-1,3,2-dioxaborol CAS No.: 911482-75-2, 2g of zirconium acrylate, and 115g of DMF are stirred at 65°C for 2h to obtain the impregnation solution.

[0068] Example 4: A quantitative preparation method of a nano inorganic composite oxide high-selectivity heat absorption film layer, the operation steps are as follows:

[0069] S1: Weigh 5g manganese acetate, 5g iron oxide, 1g nickel chloride, 5g copper oxide, 10g nanocarbon material, and 100g solvent, add them into a reactor, and stir and mix evenly for 100min;

[0070] S2: Continue to add 10g of nano chromium trioxide powder, 1g of surfactant, and 1g of film-forming aid into the reactor, stir and mix for 50min to obtain slurry;

[0071] S3: The slurry is evenly coated on the aluminum foil, dried, sintered, cooled to room temperature, and then immersed in an impregnation liquid, the temperature is increased by 50°C, the immersion time is 20 hours, taken out, and dried to obtain a heat-absorbing film layer substrate;

[0072] S4: Plasma treatment, placing the heat-absorbing film layer substrate obtained in step S3 in a radio frequency plasma device, setting the radio frequency power to 200 watts, and controlling the volume ratio of ammonia: tungsten hexafluoride mixed gas to 1.5:0.06, and the flow rate of the mixed gas to 20 ml per minute; using a radio frequency glow plasma technology with a frequency of 13.56 MHz for 40 minutes to treat the heat-absorbing film layer substrate. Through this process, a nano-inorganic composite oxide film layer with high selective heat absorption performance is finally prepared.

[0073] The nano carbon material is carbon nano tube.

[0074] The solvent is isopropanol.

[0075] The surfactant is fatty alcohol polyoxyethylene ether.

[0076] The film-forming aid is dipentene pine oil.

[0077] The drying temperature of S3 is 80° C. and the drying time is 10 hours.

[0078] The sintering of S3 is firstly heated to 150°C, kept at this temperature for 3 hours, and then heated to 600°C, kept at this temperature for 5 hours.

[0079] The composition of the impregnation solution is as follows: 0.05 g of 2-allyl-5,5-dimethyl-1,3,2-dioxaborol CAS No.: 911482-75-2, 3 g of zirconium acrylate, and 120 g of DMF are stirred at 70° C. for 3 hours to obtain the impregnation solution.

[0080] Comparative Example 1

[0081] A quantitative preparation method of a nano inorganic composite oxide high-selectivity heat-absorbing film layer, the operating steps of which are:

[0082] S1: Weigh 1g manganese acetate, 1g iron oxide, 0.1g nickel chloride, 1g copper oxide, 5g nanocarbon material, and 80g solvent, add them into a reactor, and stir and mix evenly for 70min;

[0083] S2: Continue to add 5g of nano chromium trioxide powder, 0.1g of surfactant, and 0.1g of film-forming aid into the reactor, stir and mix for 20min to obtain slurry;

[0084] S3: The slurry is evenly coated on the aluminum foil, dried, sintered, cooled to room temperature, and then immersed in an impregnation liquid, heated to 40°C, immersed for 10 hours, taken out, and dried to obtain a nano-inorganic composite oxide film layer with heat absorption properties.

[0085] The nano carbon material is carbon fiber.

[0086] The solvent is methanol.

[0087] The surfactant is linear sodium alkylbenzene sulfonate.

[0088] The film-forming aid is ethylene glycol.

[0089] The drying temperature of S3 is 60° C. and the drying time is 5 hours.

[0090] The sintering of S3 is firstly heated to 110°C, kept at this temperature for 1 hour, and then heated to 400°C, kept at this temperature for 3 hours.

[0091] Comparative Example 2

[0092] A quantitative preparation method of a nano inorganic composite oxide high-selectivity heat-absorbing film layer, the operating steps of which are:

[0093] S1: Weigh 1g manganese acetate, 1g iron oxide, 0.1g nickel chloride, 1g copper oxide, 5g nanocarbon material, and 80g solvent, add them into a reactor, and stir and mix evenly for 70min;

[0094] S2: Continue to add 5g of nano chromium trioxide powder, 0.1g of surfactant, and 0.1g of film-forming aid into the reactor, stir and mix for 20min to obtain slurry;

[0095] S3: The slurry is evenly coated on the aluminum foil, dried, sintered, cooled to room temperature, and then immersed in an impregnation liquid, the temperature is raised to 40°C, the immersion time is 10 hours, taken out, and dried to obtain a heat-absorbing film layer substrate;

[0096] S4: Plasma treatment, placing the heat-absorbing film layer substrate obtained in step S3 in a radio frequency plasma device, setting the radio frequency power to 100 watts, and controlling the volume ratio of ammonia: tungsten hexafluoride mixed gas to 1:0.03, and the flow rate of the mixed gas to 10 ml per minute; using a radio frequency glow plasma technology with a frequency of 13.56 MHz for 20 minutes to treat the heat-absorbing film layer substrate. Through this process, a nano-inorganic composite oxide film layer with high selective heat absorption performance is finally prepared.

[0097] The nano carbon material is carbon fiber.

[0098] The solvent is methanol.

[0099] The surfactant is linear sodium alkylbenzene sulfonate.

[0100] The film-forming aid is ethylene glycol.

[0101] The drying temperature of S3 is 60° C. and the drying time is 5 hours.

[0102] The sintering of S3 is firstly heated to 110°C, kept at this temperature for 1 hour, and then heated to 400°C, kept at this temperature for 3 hours.

[0103] The composition of the impregnation solution is as follows: 0.7 g of zirconium acrylate and 100 g of DMF are stirred at 50° C. for 1 hour to obtain the impregnation solution.

[0104] Comparative Example 3

[0105] A quantitative preparation method of a nano inorganic composite oxide high-selectivity heat-absorbing film layer, the operating steps of which are:

[0106] S1: Weigh 1g manganese acetate, 1g iron oxide, 0.1g nickel chloride, 1g copper oxide, 5g nanocarbon material, and 80g solvent, add them into a reactor, and stir and mix evenly for 70min;

[0107] S2: Continue to add 5g of nano chromium trioxide powder, 0.1g of surfactant, and 0.1g of film-forming aid into the reactor, stir and mix for 20min to obtain slurry;

[0108] S3: The slurry is evenly coated on the aluminum foil, dried, sintered, cooled to room temperature, and then immersed in an impregnation liquid, the temperature is raised to 40°C, the immersion time is 10 hours, taken out, and dried to obtain a heat-absorbing film layer substrate;

[0109] S4: Plasma treatment, placing the heat-absorbing film layer substrate obtained in step S3 in a radio frequency plasma device, setting the radio frequency power to 100 watts, and controlling the volume ratio of ammonia: tungsten hexafluoride mixed gas to 1:0.03, and the flow rate of the mixed gas to 10 ml per minute; using a radio frequency glow plasma technology with a frequency of 13.56 MHz for 20 minutes to treat the heat-absorbing film layer substrate. Through this process, a nano-inorganic composite oxide film layer with high selective heat absorption performance is finally prepared.

[0110] The nano carbon material is carbon fiber.

[0111] The solvent is methanol.

[0112] The surfactant is linear sodium alkylbenzene sulfonate.

[0113] The film-forming aid is ethylene glycol.

[0114] The drying temperature of S3 is 60° C. and the drying time is 5 hours.

[0115] The sintering of S3 is firstly heated to 110°C, kept at this temperature for 1 hour, and then heated to 400°C, kept at this temperature for 3 hours.

[0116] The composition of the impregnation solution is as follows: 0.005 g of 2-allyl-5,5-dimethyl-1,3,2-dioxaborol (CAS No.: 911482-75-2) and 100 g of DMF are stirred at 50° C. for 1 hour to obtain the impregnation solution.

[0117] Test results:

[0118] .

[0119] Through the data analysis of the above embodiments and comparative examples, the heat absorption film layer prepared by the present invention has high absorptivity, low emissivity and good weather resistance.

[0120] Note that the above are only preferred embodiments of the present invention and the technical principles used. Those skilled in the art will understand that the present invention is not limited to the specific embodiments described herein, and that various obvious changes, readjustments and substitutions can be made by those skilled in the art without departing from the scope of protection of the present invention. Therefore, although the present invention has been described in more detail through the above embodiments, the present invention is not limited to the above embodiments, and may include more other equivalent embodiments without departing from the concept of the present invention, and the scope of the present invention is determined by the scope of the appended claims.

Claims

1. A quantitative preparation method of a nano inorganic composite oxide highly selective heat absorption film layer, the operating steps of which are: S1: Weigh 1-5 parts of manganese acetate, 1-5 parts of iron oxide, 0.1-1 parts of nickel chloride, 1-5 parts of copper oxide, 5-10 parts of nanocarbon material, and 80-100 parts of solvent by weight, add them into a reaction kettle, and stir and mix evenly for 70-100 minutes; S2: Continue to add 5-10 parts of nano chromium trioxide powder, 0.1-1 parts of surfactant, and 0.1-1 parts of film-forming aid into the reactor, and stir and mix for 20-50 minutes to obtain slurry; S3: The slurry is evenly coated on the aluminum foil, dried, sintered, cooled to room temperature, and then immersed in an impregnation liquid, heated to 40-50°C, immersed for 10-20 hours, taken out, dried, and a heat-absorbing film layer substrate is obtained; the impregnation liquid is: 0.005-0.05 parts of 2-allyl-5,5-dimethyl-1,3,2-dioxaborol, 0.7-3 parts of zirconium acrylate, and 100-120 parts of DMF are stirred at 50-70° C. for 1-3 hours to obtain an impregnation solution; S4: Plasma treatment, placing the heat-absorbing film layer substrate obtained in step S3 in a radio frequency plasma device, setting the radio frequency power to 100-200 watts, and controlling the volume ratio of ammonia: tungsten hexafluoride mixed gas to 1-1.5:0.03-0.06, and the flow rate of the mixed gas to 10-20 ml per minute; using a radio frequency glow plasma technology with a frequency of 13.56 MHz for 20-40 minutes to treat the heat-absorbing film layer substrate. Through this process, a nano-inorganic composite oxide film layer with high selective heat absorption performance is finally prepared.

2. The quantitative preparation method of a nano inorganic composite oxide high-selectivity heat absorption film layer according to claim 1, characterized in that: The nano carbon material is one of graphene, carbon nano tube, carbon nano horn and onion-shaped carbon.

3. The quantitative preparation method of a nano inorganic composite oxide highly selective heat absorption film layer according to claim 1, characterized in that: The solvent is one of methanol, ethanol, propanol and isopropanol.

4. The quantitative preparation method of a nano inorganic composite oxide highly selective heat absorption film layer according to claim 1, characterized in that: The surfactant is one of linear alkylbenzene sodium sulfonate, fatty alcohol polyoxyethylene ether sodium sulfate, fatty alcohol polyoxyethylene ether ammonium sulfate, sodium lauryl sulfate, nonylphenol polyoxyethylene ether, diethanolamide stearic acid glycerol monoester, and fatty alcohol polyoxyethylene ether.

5. The quantitative preparation method of a nano inorganic composite oxide high-selectivity heat absorption film layer according to claim 1, characterized in that: The film-forming aid is one of ethylene glycol, propylene glycol, hexylene glycol, ethylene glycol ether, propylene glycol ethyl ether, ethylene glycol butyl ether, propylene glycol butyl ether and turpentine.

6. The quantitative preparation method of a nano inorganic composite oxide high-selectivity heat absorption film layer according to claim 1, characterized in that: The drying temperature of S3 is 60-80°C and the drying time is 5-10h.

7. The quantitative preparation method of a nano inorganic composite oxide high-selectivity heat absorption film layer according to claim 1, characterized in that: The sintering of S3 is firstly heated to 110-150°C, kept warm for 1-3h, then heated to 400-600°C, kept warm for 3-5h.