Lithium ion battery and electrolyte preparation method

By using a combination of carbonate solvent, fluorine-containing organic solvent and specific electrolyte additives in lithium-ion batteries, a conjugated system is formed, which solves the stability of the electrolyte in a high-voltage environment, and significantly improves the cycle stability of the battery and Voltage resistance.

CN118645695BActive Publication Date: 2024-11-19SUZHOU QINGTAO NEW ENERGY TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411101638.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-19
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

Existing electrolytes are difficult to maintain stability and safety in high-voltage environments, and cannot meet the needs of high-voltage applications such as electric vehicles or energy storage systems.

Method used

A lithium-ion battery preparation method is adopted, including preparing the electrolyte using a carbonate solvent and a fluorine-containing organic solvent, and adding electrolyte additives of a specific structure to form a conjugated system to improve the pressure resistance and cycle stability of the electrolyte.

Benefits of technology

By forming a dense interface film, the oxidative decomposition of the electrolyte is inhibited, the mobility of ions is improved, gas production and heat are reduced, and the cycle stability and pressure resistance of the battery are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118645695B_ABST
    Figure CN118645695B_ABST
Patent Text Reader

Abstract

The present application provides a method for preparing a lithium-ion battery and an electrolyte. The lithium-ion battery includes a positive electrode, a negative electrode, a separator and an electrolyte. The positive electrode includes a positive electrode active material, and the positive electrode active material has a charge cut-off voltage higher than 4.5V; the electrolyte includes a solvent, a lithium salt, and an electrolyte additive, and the electrolyte additive has a general structural formula; the solvent includes at least one carbonate solvent and at least one fluorine-containing organic solvent; wherein the mass ratio of the carbonate solvent to the total mass of the solvent is not less than 50%, and the mass ratio of the fluorine-containing organic solvent to the total mass of the solvent is not higher than 50%; the mass ratio of the electrolyte additive to the total mass of the electrolyte is 0.01% to 20%. The electrolyte additive can generate a CEI membrane and a SEI membrane, improve ion mobility, and improve the cycle stability of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of energy storage technology, and in particular to a method for preparing a lithium ion battery and an electrolyte. Background Art

[0002] The electrolyte is a vital component of the battery. It acts as a conductive medium for ions in electrochemical reactions, enabling charge exchange between the positive and negative electrodes. For some battery systems with high-voltage applications, such as electric vehicles or energy storage systems, the high-voltage resistance of the electrolyte is particularly important.

[0003] The high-voltage resistance of an electrolyte refers to the stability and safety of the electrolyte when subjected to high voltage. In order to be able to be used in electric vehicles or energy storage systems with high-voltage applications, it is necessary to develop an electrolyte that can withstand high voltage. Summary of the invention

[0004] Based on this, it is necessary to provide a method for preparing a lithium-ion battery and an electrolyte that can be used in a high-voltage environment.

[0005] In a first aspect, the present application provides a lithium-ion battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode comprises a positive electrode active material, and the positive electrode active material has a charge cut-off voltage higher than 4.5V;

[0006] The electrolyte comprises a solvent, a lithium salt, and an electrolyte additive, wherein the electrolyte additive comprises one or more compounds having a structural formula shown in the following formula (I):

[0007]

[0008] In formula (I), R is independently selected from any one of a hydrogen atom, a nitrogen-containing group, and an unsubstituted C1-C3 hydrocarbon group;

[0009] The solvent comprises at least one carbonate solvent and at least one fluorine-containing organic solvent;

[0010] The mass ratio of carbonate solvent to the total mass of solvent is not less than 50%, and the mass ratio of fluorine-containing organic solvent to the total mass of solvent is not more than 50%;

[0011] The electrolyte additive accounts for 0.01% to 20% of the total mass of the electrolyte.

[0012] In some embodiments, the electrolyte additive accounts for 0.1% to 10% of the total mass of the electrolyte.

[0013] In some embodiments, the electrolyte additive accounts for 0.1% to 5% of the total mass of the electrolyte.

[0014] In some embodiments, the carbonate solvent includes one or both of a linear carbonate solvent and a cyclic carbonate solvent.

[0015] In some embodiments, the linear carbonate solvent includes any one or more combinations of ethyl methyl carbonate, dimethyl carbonate, and diethyl carbonate.

[0016] In some embodiments, the cyclic carbonate solvent includes any one or more combinations of ethylene carbonate, vinylene carbonate, and vinyl ethylene carbonate.

[0017] In some embodiments, the fluorine-containing organic solvent includes any one or more combinations of fluoroethylene carbonate, difluoroethylene carbonate, di(2,2,2-trifluoroethyl) carbonate, trifluoroethyl methyl carbonate, ethyl 2,2,2-trifluoroacetate, perfluorobis(2,2,2-trifluoroethyl) ether, bis(difluoroethyl) ether, 2,2,2-trifluoroethyl 2-fluoroethyl ether, and 1,1-difluoroethyl 2-fluoroethyl ether.

[0018] In some embodiments, the concentration of the lithium salt in the electrolyte is 0.5 mol / L to 1.5 mol / L.

[0019] In a second aspect, the present application also provides a method for preparing the electrolyte in the lithium ion battery, comprising the following steps:

[0020] Mixing the carbonate solvent, the fluorine-containing organic solvent and the electrolyte additive to obtain an intermediate;

[0021] The lithium salt is added to the intermediate and then stirred to obtain an electrolyte.

[0022] In some embodiments, the mixing process and / or the stirring process is performed in a closed space; wherein,

[0023] The dew point of the enclosed space is lower than 60°C; and / or

[0024] The oxygen content of the enclosed space is less than 1 ppm; and / or

[0025] The enclosed space is filled with an inert gas.

[0026] In the above-mentioned lithium-ion battery, the electrolyte additive is added to the electrolyte, which can cooperate with the carbonate-based electrolyte to improve the pressure resistance of conventional carbonate electrolytes. The conjugated system formed by the electrolyte additive exhibits a strong electron-withdrawing ability and is easy to polymerize on the electrode surface to form an interface film, thereby inhibiting the oxidative decomposition of the electrolyte. Specifically, a dense and uniform CEI (Cathode Electrolyte Interphase) film and SEI (Solid Electrolyte Interphase) film can be generated at the positive electrode and the negative electrode respectively, improving the mobility of ions, effectively preventing the carbonate electrolyte from undergoing oxidation reactions with the electrode material during the cycle, reducing and lowering the gas production and heat of the battery, and being able to inhibit the decomposition of the electrolyte and improve the cycle stability of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 A schematic diagram of a method for preparing an electrolyte according to one embodiment. DETAILED DESCRIPTION

[0028] References to embodiments of the present application will now be provided in detail, one or more examples of which are described below. Each example is provided as an explanation rather than a limitation of the present application. In fact, it will be apparent to those skilled in the art that various modifications and variations may be made to the present application without departing from the scope or spirit of the present application. For example, a feature described or described as part of one embodiment may be used in another embodiment to produce a further embodiment.

[0029] Therefore, it is intended that the present application covers such modifications and variations that fall within the scope of the appended claims and their equivalents. Other objects, features and aspects of the present application are disclosed in or are apparent from the following detailed description. It will be appreciated by those of ordinary skill in the art that this discussion is merely a description of exemplary embodiments and is not intended to limit the broader aspects of the present application.

[0030] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0031] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0032] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0033] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0034] If there is no special explanation, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps S12 and S14, which means that the method may include steps S12 and S14 performed sequentially, or may include steps S14 and S12 performed sequentially. For example, it is mentioned that the method may also include step S16, which means that step S16 may be added to the method in any order, for example, the method may include steps S12, S14 and S16, or may include steps S12, S16 and S14, or may include steps S16, S12 and S14, etc.

[0035] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0036] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0037] The present application provides a lithium ion battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode comprises a positive electrode active material, and the positive electrode active material has a charge cut-off voltage higher than 4.5V; the electrolyte comprises a solvent, a lithium salt, and an electrolyte additive, and the electrolyte additive comprises one or more compounds having a structural formula shown in the following formula (I):

[0038] ;

[0039] In formula (I), R is independently selected from any one of a hydrogen atom, a nitrogen-containing group, and an unsubstituted C1~C3 hydrocarbon group; the solvent includes at least one carbonate solvent and at least one fluorine-containing organic solvent; wherein the mass ratio of the carbonate solvent to the total mass of the solvent is not less than 50%, and the mass ratio of the fluorine-containing organic solvent to the total mass of the solvent is not more than 50%; the mass ratio of the electrolyte additive to the total mass of the electrolyte is 0.01%~20%.

[0040] In the above-mentioned lithium-ion battery, an electrolyte additive having a structure as shown in formula (I) is added to the electrolyte, which can cooperate with the carbonate-based electrolyte to improve the pressure resistance of conventional carbonate electrolytes, and improve the cycle stability of batteries with a charging cut-off voltage higher than 4.5V. The conjugated system formed by the electrolyte additive exhibits a strong electron-withdrawing ability, is easy to polymerize on the electrode surface, and forms an interface film, thereby inhibiting the oxidative decomposition of the electrolyte. Specifically, a dense and uniform CEI and SEI film can be generated at the positive electrode and the negative electrode respectively, improving the mobility of ions, effectively preventing the carbonate electrolyte from reacting with the electrode material during the cycle, reducing and lowering the gas production and heat of the battery, and being able to inhibit the decomposition of the electrolyte and improve the cycle stability of the battery.

[0041] The above is only a possible speculation on the mechanism of the present application and does not constitute a limitation on the scope of protection of the present application.

[0042] In some embodiments, R in formula (I) may be hydrogen.

[0043] In some embodiments, R in formula (I) may be, but is not limited to, a nitrogen-containing group selected from nitro, cyano, isocyano, amino, and amine.

[0044] In some embodiments, R in formula (I) may be, but is not limited to, an unsubstituted C1-C3 hydrocarbon group. "Hydrocarbon group" refers to a group containing only carbon and hydrogen atoms, including but not limited to alkyl, alkenyl, alkynyl, aryl, etc.

[0045] "Alkyl" refers to a saturated hydrocarbon containing carbon atoms. Phrases containing this term, for example, "C1~C3 alkyl" refers to an alkyl group containing 1 to 3 carbon atoms, and each occurrence can be independently C1 alkyl, C2 alkyl, or C3 alkyl. Suitable examples include, but are not limited to, methyl (Me, -CH3), ethyl (Et, -CH2CH3), 1-propyl (n-Pr, n-propyl, -CH2CH2CH3), 2-propyl (i-Pr, i-propyl, -CH(CH3)2).

[0046] "Alkenyl" refers to a hydrocarbon containing carbon atoms having at least one unsaturated site, i.e., a carbon-carbon sp2 double bond. Phrases containing this term, for example, "C2~C3 alkenyl" refers to an alkenyl group containing 2 to 3 carbon atoms, each occurrence of which can be independently C2 alkenyl or C3 alkenyl. Suitable examples include, but are not limited to, vinyl (-CH=CH2), allyl (-CH2CH=CH2), etc.

[0047] "Alkynyl" refers to a hydrocarbon containing at least one unsaturated site, i.e., a carbon-carbon sp triple bond. Phrases containing this term, for example, "C2-C3 alkynyl" refers to an alkynyl containing 2 to 3 carbon atoms, each occurrence of which can be independently C2 alkynyl or C3 alkynyl. Suitable examples include, but are not limited to, ethynyl (-C≡CH) and propargyl (-CH2C≡CH).

[0048] Exemplarily, the electrolyte additive is any one of the compounds represented by formula (I-1) to formula (I-4), wherein R in formula (I-1) to formula (I-4) is selected from hydrogen, methyl, amino, chlorine and n-propyl respectively:

[0049] Formula (I-1), Formula (I-2),

[0050] Formula (I-3), Formula (I-4).

[0051] In some embodiments, the mass ratio of the electrolyte additive to the total mass of the electrolyte can be, but is not limited to, 0.01%, 0.02%, 0.05%, 0.08%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.8%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%. Further, the mass ratio of the electrolyte additive to the total mass of the electrolyte is 0.1% to 10%. Further, the mass ratio of the electrolyte additive to the total mass of the electrolyte is 0.1% to 5%. Within the above range, the electrolyte additive can form a CEI film and a SEI film of suitable thickness to improve the cycle stability of the lithium-ion battery.

[0052] In some of the embodiments, the mass ratio of the carbonate solvent in the solvent to the total mass of the solvent may be, but is not limited to, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90% or 95%, etc.

[0053] In some of the embodiments, the mass ratio of the fluorinated organic solvent to the total mass of the solvent may be, but is not limited to, 50%, 45%, 40%, 35%, 30%, 25%, 20%, 15%, 10% or 5%, etc.

[0054] In some embodiments, the carbonate solvent includes one or both of a linear carbonate solvent and a cyclic carbonate solvent.

[0055] In some embodiments, the linear carbonate solvent includes any one or more combinations of ethyl methyl carbonate, dimethyl carbonate, and diethyl carbonate.

[0056] In some embodiments, the cyclic carbonate solvent includes any one or more combinations of ethylene carbonate, vinylene carbonate, and vinyl ethylene carbonate.

[0057] In some embodiments, the fluorine-containing organic solvent includes any one or more combinations of fluoroethylene carbonate, difluoroethylene carbonate, di(2,2,2-trifluoroethyl) carbonate, trifluoroethyl methyl carbonate, ethyl 2,2,2-trifluoroacetate, perfluorobis(2,2,2-trifluoroethyl) ether, bis(difluoroethyl) ether, 2,2,2-trifluoroethyl 2-fluoroethyl ether, and 1,1-difluoroethyl 2-fluoroethyl ether.

[0058] In some embodiments, the concentration of the lithium salt in the electrolyte is 0.5 mol / L to 1.5 mol / L. For example, the concentration of the lithium salt in the electrolyte may be, but is not limited to, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1 mol / L, 1.2 mol / L, 1.3 mol / L, 1.4 mol / L or 1.5 mol / L. For example, the lithium salt may include any one or a mixture of LiPF6, LiFSI, LiPO2F2, LiTFSI, LiBF4, LiBOB, LiDFOB, and LiCF3SO3. Further, the concentration of the lithium salt in the electrolyte is 0.8 mol / L to 1.3 mol / L.

[0059] In some embodiments, the positive electrode active material includes LiCo 1-y M y O2、LiNi 1-y M y O2、LiMn 2-y M y O4、LiNi x Co y Mn z M 1-x-y-z One or more of O2, wherein M is selected from one or more of Fe, Co, Ni, Mn, Mg, Cu, Zn, Al, Sn, B, Ga, Cr, Sr, V and Ti, and 0≤y≤1, 0≤x≤1, 0≤z≤1, x+y+z≤1.

[0060] In some embodiments, the negative electrode includes a negative electrode active material, and the negative electrode active material includes but is not limited to one or more of artificial graphite, natural graphite, soft carbon, hard carbon, silicon, silicon carbon, silicon oxygen, and lithium titanate.

[0061] In some embodiments, the positive electrode further includes a conductive agent, which includes but is not limited to one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, carbon nanofibers, and graphene.

[0062] In some embodiments, the positive electrode further comprises a positive electrode binder. The positive electrode binder comprises one or more of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyvinylidene fluoride hexafluoropropylene (PVDF-HFP), polypropylene (PP), polyethylene (PE), styrene-butadiene rubber (SBR), nitrile rubber (NBR), sodium hydroxymethyl cellulose (CMC), polyacrylic acid, polyacrylonitrile, and sodium alginate.

[0063] See also Figure 1 The present application also provides a method for preparing the electrolyte in the above-mentioned lithium-ion battery, comprising the following steps S11~S12.

[0064] S11, mixing a carbonate solvent, a fluorine-containing organic solvent and an electrolyte additive to obtain an intermediate.

[0065] S12, adding lithium salt to the intermediate and stirring to obtain an electrolyte.

[0066] In some embodiments, the mixing process and / or the stirring process is performed in a closed space; wherein the dew point of the closed space is lower than 60° C.; and / or the oxygen content of the closed space is lower than 1 ppm; and / or the closed space is filled with an inert gas. For example, the inert gas may be nitrogen, helium, argon, or the like.

[0067] The electrolyte prepared by the above method, by adding an electrolyte additive having a structure as shown in formula (I) to the electrolyte, can be combined with a carbonate-based electrolyte to improve the pressure resistance of conventional carbonate electrolytes, and improve the cycle stability of batteries with a charging cut-off voltage higher than 4.5V. The conjugated system formed by the electrolyte additive exhibits a strong electron-withdrawing ability, is easy to polymerize on the electrode surface, and forms an interface film, thereby inhibiting the oxidative decomposition of the electrolyte. Specifically, a dense and uniform CEI and SEI film can be generated at the positive electrode and the negative electrode, respectively, to improve the mobility of ions, effectively prevent the carbonate electrolyte from reacting with the electrode material during the cycle, reduce and lower the gas production and heat of the battery, and can inhibit the decomposition of the electrolyte, thereby improving the cycle stability of the battery.

[0068] The following are specific embodiments.

[0069] Example 1

[0070] Preparation of electrolyte

[0071] (1) A carbonate solvent, ethyl methyl carbonate, and a fluorinated organic solvent, fluoroethylene carbonate, are mixed at a mass ratio of 5:5 to obtain an electrolyte solvent. An electrolyte additive is added to the solvent so that the electrolyte additive accounts for 0.5% of the total mass of the electrolyte, and the mixture is treated to obtain an intermediate. The electrolyte additive has a compound having a structure as shown in formula (I-2), that is, R is a methyl group.

[0072] (2) Add lithium salt LiPF6 to the intermediate and stir to obtain an electrolyte solution, wherein the concentration of LiPF6 is 1 mol / L.

[0073] Lithium-ion battery

[0074] The lithium-ion battery includes a positive electrode, a negative electrode separator and the above electrolyte. The positive electrode includes a positive electrode active material, which is LiNi 0.8 Co 0.1 Mn 0.1 O2; the negative electrode includes a negative electrode active material, and the negative electrode active material is graphite.

[0075] Example 2

[0076] The preparation method of Example 2 is basically the same as the preparation method of Example 1, except that the mass ratio of ethyl methyl carbonate to fluoroethylene carbonate is 6:4, and the electrolyte additive has a compound with a structure as shown in formula (I-1), that is, R is hydrogen.

[0077] Example 3

[0078] The preparation method of Example 3 is substantially the same as that of Example 1, except that the mass ratio of ethyl methyl carbonate to fluoroethylene carbonate is 6:4.

[0079] Example 4

[0080] The preparation method of Example 4 is substantially the same as that of Example 1, except that the mass ratio of ethyl methyl carbonate to fluoroethylene carbonate is 7:3, and the mass ratio of the electrolyte additive to the total mass of the electrolyte is 1%.

[0081] Example 5

[0082] The preparation method of Example 5 is substantially the same as that of Example 1, except that the mass ratio of ethyl methyl carbonate to fluoroethylene carbonate is 8:2, and the mass ratio of the electrolyte additive to the total mass of the electrolyte is 1%.

[0083] Example 6

[0084] The preparation method of Example 6 is basically the same as the preparation method of Example 1, except that the mass ratio of ethyl methyl carbonate to fluoroethylene carbonate is 9:1, and the mass proportion of the electrolyte additive to the total mass of the electrolyte is 2%.

[0085] Example 7

[0086] The preparation method of Example 7 is substantially the same as that of Example 1, except that the mass ratio of ethyl methyl carbonate to fluoroethylene carbonate is 95:5, and the mass ratio of the electrolyte additive to the total mass of the electrolyte is 3%.

[0087] Example 8

[0088] The preparation method of Example 8 is basically the same as the preparation method of Example 1, except that the mass ratio of ethyl methyl carbonate to fluoroethylene carbonate is 7:3, the mass proportion of the electrolyte additive to the total mass of the electrolyte is 1%, and the electrolyte additive has a compound with a structure shown in formula (I-3), that is, R is an amino group.

[0089] Example 9

[0090] The preparation method of Example 9 is basically the same as the preparation method of Example 1, except that the mass ratio of ethyl methyl carbonate to fluoroethylene carbonate is 7:3, the mass proportion of the electrolyte additive to the total mass of the electrolyte is 1%, and the electrolyte additive has a compound with a structure shown in formula (I-4), that is, R is n-propyl.

[0091] Example 10

[0092] The preparation method of Example 10 is basically the same as the preparation method of Example 1, except that the carbonate solvent is dimethyl carbonate, the fluorine-containing organic solvent is di(2,2,2-trifluoroethyl) carbonate, and the mass ratio of dimethyl carbonate to di(2,2,2-trifluoroethyl) carbonate is 7:3.

[0093] Comparative Example 1

[0094] The preparation method of Comparative Example 1 is substantially the same as that of Example 1, except that the mass ratio of ethyl methyl carbonate to fluoroethylene carbonate is 3:7, and the compound of formula (I) is not added.

[0095] Comparative Example 2

[0096] The preparation method of Comparative Example 2 is substantially the same as that of Example 1, except that the mass ratio of ethyl methyl carbonate to fluoroethylene carbonate is 6:4, and the compound of formula (I) is not added.

[0097] The types of carbonate solvents and their mass contents in the electrolyte solvent, the types of fluorinated organic solvents and their mass contents in the electrolyte solvent, the types of R groups of electrolyte additives, and the mass ratio of the mass of the electrolyte additives to the mass of the electrolyte in the preparation methods of Examples 1 to 10 and Comparative Examples 1 to 2 are shown in Table 1. The lithium ion batteries prepared in Examples 1 to 10 and Comparative Examples 1 to 2 were subjected to room temperature cycle retention rate tests and high temperature cycle retention rate tests, and the test results are shown in Table 1.

[0098] The test methods for the normal temperature cycle retention rate test and the high temperature cycle retention rate test are as follows: first, the lithium-ion battery is charged to 4.25V at a constant current and constant voltage of 0.33C, and the cut-off current is 0.05C. Then, it is discharged to 2.4V at 0.33C, and then the normal temperature cycle retention rate test or the high temperature cycle retention rate test is performed at a current of 1C. The normal temperature condition is 25°C, and the high temperature condition is 45°C, and the cycle test is continued for 500 times.

[0099] Table 1

[0100]

[0101] By comparing Examples 1 to 10 with Comparative Examples 1 to 2, it can be seen that the electrolyte additive of the present application improves the room temperature cycle performance and high temperature cycle performance of the lithium ion battery.

[0102] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0103] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.

Claims

1. A lithium-ion battery comprising a positive electrode, a negative electrode, a separator and an electrolyte, It is characterized in that The positive electrode comprises a positive electrode active material, and the positive electrode active material has a charge cut-off voltage higher than 4.5V; The electrolyte comprises a solvent, a lithium salt, and an electrolyte additive, wherein the electrolyte additive comprises one or more compounds having a structural formula shown in the following formula (I): ; In formula (I), R is selected from a hydrogen atom, a nitrogen-containing group, an unsubstituted C 1 ~C 3 Any one of the hydrocarbon groups; the nitrogen-containing group is selected from nitro, cyano, isocyano, amino, and amine; The solvent comprises at least one carbonate solvent and at least one fluorine-containing organic solvent; The mass ratio of carbonate solvent to the total mass of solvent is not less than 50%, and the mass ratio of fluorine-containing organic solvent to the total mass of solvent is not more than 50%; The electrolyte additive accounts for 0.01% to 20% of the total mass of the electrolyte.

2. The lithium ion battery according to claim 1, It is characterized in that The electrolyte additive accounts for 0.1% to 10% of the total mass of the electrolyte.

3. The lithium ion battery according to claim 2, It is characterized in that The electrolyte additive accounts for 0.1% to 5% of the total mass of the electrolyte.

4. The lithium ion battery according to claim 1, It is characterized in that The carbonate solvent includes one or both of a chain carbonate solvent and a cyclic carbonate solvent.

5. The lithium ion battery according to claim 4, It is characterized in that The linear carbonate solvent includes any one or more combinations of ethyl methyl carbonate, dimethyl carbonate and diethyl carbonate.

6. The lithium ion battery according to claim 4, It is characterized in that The cyclic carbonate solvent includes any one or more combinations of ethylene carbonate, vinylene carbonate, and vinyl ethylene carbonate.

7. The lithium ion battery according to any one of claims 4 to 6, It is characterized in that The fluorine-containing organic solvent includes any one or more combinations of fluoroethylene carbonate, difluoroethylene carbonate, bis(2,2,2-trifluoroethyl) carbonate, trifluoroethyl methyl carbonate, ethyl 2,2,2-trifluoroacetate, perfluorobis(2,2,2-trifluoroethyl) ether, bis(difluoroethyl) ether, 2,2,2-trifluoroethyl 2-fluoroethyl ether, and 1,1-difluoroethyl 2-fluoroethyl ether.

8. The lithium ion battery according to claim 1, It is characterized in that The concentration of the lithium salt in the electrolyte is 0.5 mol / L to 1.5 mol / L.

9. A method for preparing an electrolyte in a lithium ion battery according to any one of claims 1 to 8, It is characterized in that The following steps are involved: Mixing the carbonate solvent, the fluorine-containing organic solvent and the electrolyte additive to obtain an intermediate; The lithium salt is added to the intermediate and then stirred to obtain an electrolyte.

10. The preparation method according to claim 9, It is characterized in that The mixing process and / or the stirring process is carried out in a closed space; wherein, The dew point of the enclosed space is lower than 60°C; and / or The oxygen content of the enclosed space is less than 1 ppm; and / or The enclosed space is filled with an inert gas.

Citation Information

Patent Citations

  • Non-aqueous electrolyte and lithium ion battery

    CN103972588A

  • Non-aqueous electrolyte and non-aqueous electrolyte secondary cell employing same

    WO2013008439A1

  • Hexahydropyrido[4,3-b]indolyl ketone derivatives useful as cgas modulators