A lithium composite negative electrode and its preparation method and use

By combining the modified graphitized film with metal lithium or lithium alloy foil, a lithium storage supplement layer is formed, which solves the problem of capacity attenuation of lithium-ion batteries in the later cycle, extends the battery cycle life and improves the cycling performance of the battery cell .

CN118645712BActive Publication Date: 2024-12-03CHINA ENERGY LITHIUM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411118612.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-12-03
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

When the existing lithium-ion battery is cycled for about 100 cycles, the capacity of the metal lithium negative electrode is rapidly decayed and there are safety risks, making it difficult to meet the needs of high specific capacity and long cycle life.

Method used

The modified graphitized film is combined with metal lithium or lithium alloy foil, and a lithium storage supplementary layer is formed by hot pressing to extend the battery cycle life. The modified graphitized film consists of graphite, modifiers and structural enhancers. Modifiers such as single-wall carbon nanotubes and nanocarbon fibers improve the ability of lithium atoms, and structural enhancers such as polytetrafluoroethylene enhance mechanical strength.

Benefits of technology

In the later stage of battery cycle, the lithium metal in the lithium storage supplement layer plays a role, improving the cell circulation performance, increasing the cycle life by more than 10%, and the material is lightweight and has a high tensile strength, which is suitable for the needs of high-specific energy lightweight negative electrodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118645712B_ABST
    Figure CN118645712B_ABST
Patent Text Reader

Abstract

The present application relates to a lithium composite negative electrode and its preparation method and use. The lithium composite negative electrode comprises: a modified graphitized film material as a current collector; an active material layer composited on at least one surface of the modified graphitized film material, wherein the active material layer is a continuous or intermittently distributed metallic lithium or lithium alloy foil; and a lithium storage supplement layer formed by lithium atoms diffusing into the modified graphitized film material, wherein the thickness of the lithium storage supplement layer is 2-25 μm. In the late stage of the battery reaction, when the active metallic lithium almost disappears, the lithium storage supplement layer begins to play a role, extending the cycle life of the battery by more than 10%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrochemical energy storage, and in particular to a lithium composite negative electrode for a lithium secondary battery. Background Art

[0002] As society demands ever-higher energy density from lithium-ion batteries, research is currently shifting towards anode materials with higher specific capacities. Metallic lithium is considered the optimal anode material due to its capacity of 3860 mAh / g and low potential of -3.04V. Currently, lithium metal ribbons or lithium-copper composite ribbons are used as anode materials, and the positive electrode material is a ternary positive electrode. However, after approximately 100 cycles, the capacity of lithium metal decays to below 80%, making it far from practical application. After approximately 100 cycles, the capacity of lithium metal as the anode decays rapidly due to the pulverization of the lithium metal and the formation of dead lithium, posing a safety hazard. Therefore, the search continues for materials that can assist in the later stages of lithium metal cycling and extend the battery's cycle life during the later stages of lithium metal anode cycling. Summary of the Invention

[0003] To address the above issues, the inventors conducted in-depth and detailed research and discovered a type of membrane material that can form a lithium storage supplement layer when combined with metallic lithium. The lithium storage supplement layer can extend the cycle life of the battery in the later stage of the battery cycle.

[0004] Specifically, one aspect of the present invention relates to a lithium composite negative electrode, comprising:

[0005] Modified graphitized film as current collector;

[0006] An active material layer composited on at least one surface of the modified graphitized film, wherein the active material layer is a continuous or intermittently distributed metallic lithium or lithium alloy foil; and

[0007] Through hot pressing and compounding, lithium atoms diffuse into the modified graphitized film to form a lithium storage supplement layer.

[0008] According to certain embodiments, the thickness of the lithium storage supplementary layer is 2-25 μm, preferably 3-20 μm, and more preferably 5-15 μm.

[0009] According to certain embodiments, the modified graphitized film material comprises graphite or a graphitized organic polymer and a modifier and a structural reinforcer, or is obtained by graphitizing a film material made of graphene, a modifier and a structural reinforcer, wherein the modifier is selected from at least one of single-walled carbon nanotubes, multi-walled carbon nanotubes and nano-carbon fibers, the structural reinforcer is selected from at least one of polytetrafluoroethylene, polyvinylidene fluoride, styrene-butadiene rubber, carboxymethyl cellulose sodium and polyacrylic acid, and the organic polymer is selected from polyimide or polyacrylonitrile.

[0010] According to certain embodiments, the graphitization treatment is performed at a temperature of 2300-3000° C. and for a time of 0.5-2 h.

[0011] According to certain embodiments, in the modified graphitized film, the mass percentage of the modifier is 0.1%-10%, and the mass percentage of the structural reinforcing agent is 0.1%-10%. Preferably, the mass percentage of the modifier is 0.5%-5%, and the mass percentage of the structural reinforcing agent is 0.5%-5%.

[0012] According to certain embodiments, the sheet resistance of the modified graphitized film is 0.1-100 mΩ / cm 2 , the film thickness is 5-25μm, and the film density is 1.3-2.0g / cm 3 , the tensile strength of the membrane material is 15-100MPa.

[0013] According to certain embodiments, the thickness of the metallic lithium or lithium alloy foil is 1-100 μm, preferably 1-20 μm; and the width is 50-1400 mm, preferably 200-700 mm.

[0014] According to certain embodiments, the lithium alloy foil is a foil formed by combining metallic lithium with any one or at least two elements of Ag, Au, Sn, Si, Zn, Al, Mg, In, Ga, B, Mn, Sb, Cr, C, V, Cu, Fe or Ti.

[0015] According to certain embodiments, both sides of the modified graphitized membrane are compounded with active material layers.

[0016] In certain embodiments, the modifier is selected from single-walled carbon nanotubes, multi-walled carbon nanotubes, and carbon nanofibers, all of which exhibit lithium conductivity. After modification with the modifier, lithium atoms are more easily inserted into the interlayer gaps of graphite or between graphene layers, thereby facilitating the formation of a lithium storage supplementary layer. Furthermore, the modifier and structural reinforcement (such as polytetrafluoroethylene and polyvinylidene fluoride) can facilitate film formation and improve the mechanical strength of the mixed material, facilitating roll-to-roll large-scale production.

[0017] Another aspect of the present invention provides a method for preparing the above-mentioned lithium composite negative electrode, the method comprising the following steps:

[0018] Step 1: Prepare the modified graphitized film material, laminate one side of the film with the release film and roll it up together;

[0019] Step 2: Unwinding the metallic lithium / lithium alloy foil and the modified graphitized film, laminating the modified graphitized film with the side not attached to the release film facing the metallic lithium / lithium alloy foil under a small pressure of 1-2 MPa, and removing the release film to obtain a single-sided lithium composite negative electrode;

[0020] Step 3: Unwind another roll of lithium metal / lithium alloy foil, and press-combine the side of the single-sided lithium composite negative electrode without composite lithium with the unwound lithium metal / lithium alloy foil at a pressure of 3-5 MPa to obtain a preliminary double-sided lithium composite negative electrode;

[0021] Step 4: The preliminary double-sided lithium composite negative electrode is rolled by a hot roller with a temperature of 40-60° C. and a pressure of 1-2 MPa to obtain the lithium composite negative electrode.

[0022] The reason for using low pressure during the second step of laminating the lithium metal / lithium alloy foil is that, in the subsequent third step, the other side of the lithium metal / lithium alloy foil is laminated to the negative electrode using pressure again. This prevents overpressure from occurring when the already laminated lithium metal / lithium alloy foil is laminated again. Overpressure can cause wrinkles and unevenness on the surface of the lithium metal / lithium alloy foil.

[0023] The lithium storage supplement layer is slowly formed after metallic lithium and modified graphitized film are rolled by hot rollers.

[0024] According to certain embodiments, the modified graphitized membrane is obtained by the following method: flake graphite raw material (which has been graphitized) is treated with acid, then washed with water until neutral, and then a modifier (at least one of single-walled carbon nanotubes, multi-walled carbon nanotubes and carbon fibers) is added, with a mass percentage of 0.1%-10%, and then a structural reinforcing agent (at least one of polytetrafluoroethylene, polyvinylidene fluoride, styrene-butadiene rubber, carboxymethyl cellulose sodium, and polyacrylic acid) is added, with a mass percentage of 0.1%-10%, and a trace amount of solvent (at least one of NMP / n-hexane / water) (mass percentage less than 3%) is added, mixed into a uniform material, and then calendered to obtain a modified graphitized membrane.

[0025] According to certain embodiments, the modified graphitized film is obtained by the following method: a polyimide polymer or a polyacrylonitrile polymer is carbonized at 1200-1500°C for 1-2 hours, then graphitized at 2300-3000°C for 0.5-2 hours, a modifier is added at a mass percentage of 0.1%-10%, and then a structural reinforcing agent is added at a mass percentage of 0.1%-10%, and a trace amount of solvent (less than 3% by mass) is added, mixed into a uniform material, and then calendered to obtain a modified graphitized film.

[0026] According to certain embodiments, a modified graphitized film is obtained by the following method: a graphene oxide slurry with a certain solid content (about 5%) is mixed with a modifier with a mass percentage of 0.1%-10%, and then a structural enhancer is added with a mass percentage of 0.1%-10%; the slurry is coated on a release film and dried to obtain a graphene oxide film, which is then dried at low temperature and reduced (with hydrazine hydrate and vitamin C) to obtain a reduced graphene film, which is then subjected to a high-temperature graphitization treatment at 2300-3000°C for 0.5-2h to obtain a modified graphitized film.

[0027] According to certain embodiments, the release film is a polyethylene terephthalate, polypropylene, or polyethylene plastic film having one surface (the bonding surface of the modified graphitized film material) treated with a silicone oil coating.

[0028] The graphitized film is very thin. One side of the graphitized film is laminated to the plastic film and rolled together. The side of the plastic film that is laminated to the graphitized film is coated with a thin layer of silicone oil. This allows the plastic and graphitized films to be easily separated during use. The silicone oil layer is very thin, at the nanometer level.

[0029] Another aspect of the present invention relates to the use of the above-mentioned lithium composite negative electrode, wherein the lithium composite negative electrode is directly used as the negative electrode of a liquid or solid lithium battery.

[0030] In the late stage of the battery reaction, when the active metallic lithium is almost completely gone, the lithium in the lithium storage supplement layer of the lithium composite negative electrode is released to play a role.

[0031] According to certain embodiments, the positive electrode of the lithium battery uses lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium-rich manganese-based positive electrode material, lithium iron phosphate, lithium manganese iron phosphate, sulfur-carbon positive electrode, sulfurized polyacrylonitrile or lithium cobalt oxide, etc.

[0032] According to certain embodiments, the lithium battery is a liquid lithium ion battery or a solid lithium ion battery.

[0033] According to certain embodiments, the electrolyte of the lithium battery can be a liquid electrolyte or a solid electrolyte; the liquid electrolyte can be an ester or an ether; the solid electrolyte can be an inorganic solid electrolyte, such as an oxide solid electrolyte, a halide solid electrolyte, or a sulfide solid electrolyte; the solid electrolyte can be a polymer electrolyte (polyethylene oxide, polysiloxane, polyacrylonitrile, polyvinylidene fluoride, etc.) or an electrolyte mixed with a polymer electrolyte and an inorganic solid electrolyte, such as polyethylene oxide mixed with oxide, halide, and sulfide electrolytes.

[0034] According to certain embodiments, the separator of the liquid battery is selected from PP (polypropylene), PE (polyethylene) or a three-layer laminated separator of PP and PE. The separator may be coated with ceramic, PVDF (polyvinylidene fluoride), boehmite or inorganic solid electrolyte powder.

[0035] According to certain embodiments, the battery can be configured as a prismatic, pouch, or cylindrical battery.

[0036] Compared with the prior art, the present invention has at least one of the following beneficial effects:

[0037] 1. The lithium storage supplement layer formed between the metallic lithium / lithium alloy and the modified graphitized membrane. In the battery cell with metallic lithium / lithium alloy as the negative electrode active material, in the later stage of the battery cycle, the metallic lithium in the lithium storage supplement layer plays a role, improving the cycle performance of the battery cell and increasing the cycle life by more than 10%.

[0038] 2. Modifiers (single-walled carbon nanotubes, multi-walled carbon nanotubes, and carbon nanofibers) exhibit lithium conductivity. After modification, lithium atoms more easily insert into the interlayer gaps of graphite or between graphene layers, thereby facilitating the formation of a lithium storage layer. Furthermore, modifiers and structural reinforcements (such as polytetrafluoroethylene and polyvinylidene fluoride) can make the mixed material easier to form a film and improve the mechanical strength of the film, making it easier to roll and mass-produce.

[0039] 3. The graphitized film material is light in weight and has high tensile strength. It can be rolled up and used in large quantities to prepare lithium composite negative electrodes, meeting the demand for high specific energy and lightweight negative electrodes. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 Schematic diagram of the reaction mechanism of lithium composite negative electrode during battery cycling;

[0041] 1-metal lithium foil / lithium alloy foil, 1'-powdered lithium in the late stage of reaction (low activity in the reaction), 2-lithium storage supplementary layer, 3-modified graphitized membrane material.

[0042] Figure 2 These are cycle test curves of lithium-ion batteries using the lithium composite negative electrodes of Comparative Example 1, Comparative Example 2, Comparative Example 3, Example 1, Example 2, Example 3, and Example 4.

[0043] Figure 3 A time-voltage data diagram for a button battery assembled with a lithium storage supplementary layer material.

[0044] Figure 4 Time-voltage data plot for a coin cell assembled without lithium storage supplementary layer material. DETAILED DESCRIPTION

[0045] To facilitate understanding of the present application, the present application lists the following examples. Those skilled in the art should understand that the examples are only provided to help understand the present application and should not be considered as specific limitations of the present application.

[0046] Example 1

[0047] Preparation of modified graphitized membrane:

[0048] Flake graphite powder is used, oxidized with concentrated sulfuric acid, and the product is washed with water to neutrality and dried at low temperature to obtain product A. Product A, single-walled carbon nanotubes, and polyvinylidene fluoride resin are mixed in a mass ratio of 97.5:1.5:1, and a trace amount of 1-methyl-2-pyrrolidone solvent is added. The mixture is kneaded evenly, and a graphitized film with a thickness of 20 μm is prepared by means of a roller press with a pressure set to 3 MPa. The film is then rolled up with a release film on one side. The tensile strength of the film is 16.5 MPa.

[0049] Preparation of lithium composite negative electrode:

[0050] The active material used was a rolled lithium foil of 20 μm thickness. A roll of lithium foil and the rolled graphitized film of 20 μm thickness prepared above were unwound. A preliminary single-sided lithium composite negative electrode was obtained by means of a roller press with a pressure set to 2 MPa.

[0051] Another roll of 20 μm thick lithium foil and the preliminary single-sided lithium composite negative electrode was unwound, and a preliminary double-sided lithium composite negative electrode was obtained by means of a roller press with a pressure set to 4 MPa.

[0052] The preliminary double-sided lithium composite negative electrode was subjected to another hot roller pressing process with the pressure set to 2 MPa, the temperature set to 50°C, and the roller speed set to 30 m / min to obtain the lithium composite negative electrode 1 to be used in the battery (the thickness of the lithium storage supplement layer was 5 μm).

[0053] Example 2

[0054] Preparation of modified graphitized membrane:

[0055] A polyimide polymer was first synthesized, carbonized at 1300°C for 1 hour, and then graphitized at 2600°C for 1 hour to obtain a graphitized product (B). Product B was then mixed with multi-walled carbon nanotubes (MWCNTs) and polytetrafluoroethylene (PTFE) (powder, less than 12 μm, Aladdin) in a mass ratio of 97.5:1:1.5. A trace amount of 1-methyl-2-pyrrolidone was added and mixed thoroughly. Using a roller press at a pressure of 5 MPa, a 17 μm thick film was prepared. The film was then rolled up with a thin layer of silicone oil-coated PET plastic film to obtain a rolled graphitized film with a tensile strength of 20.1 MPa.

[0056] Preparation of lithium composite negative electrode:

[0057] The active material used was a rolled lithium foil of 20 μm thickness. A roll of lithium foil and the rolled graphitized film of 17 μm thickness prepared above were unwound. With the help of a roller press, the pressure was set to 1 MPa to obtain a preliminary single-sided lithium composite negative electrode.

[0058] Another roll of 20 μm thick lithium foil and the preliminary single-sided lithium composite negative electrode was unwound, and a preliminary double-sided lithium composite negative electrode was obtained by means of a roller press with a pressure set to 4 MPa.

[0059] The preliminary double-sided lithium composite negative electrode was subjected to another hot roller pressing process with the pressure set to 1 MPa, the temperature set to 50°C, and the roller speed set to 30 m / min to obtain the lithium composite negative electrode 2 to be used in the battery (the thickness of the lithium storage supplement layer was 10 μm).

[0060] Example 3

[0061] The modified graphitized film material of Example 3 is consistent with that of Example 2.

[0062] The 20 μm thick lithium foil in Example 2 was replaced with a 20 μm thick lithium-magnesium alloy foil (magnesium content of 5%). A roll of lithium-magnesium alloy foil and the 17 μm thick graphitized film prepared above were unwound. With the help of a roller press, the pressure was set to 2 MPa to obtain a preliminary single-sided lithium composite negative electrode.

[0063] Another roll of 20 μm thick lithium-magnesium alloy foil and the preliminary single-sided lithium composite negative electrode was unwound, and a preliminary double-sided lithium composite negative electrode was obtained by means of a roller press with a pressure set to 4 MPa.

[0064] The preliminary double-sided lithium composite negative electrode was subjected to a hot roller press with a pressure of 1 MPa, a temperature of 45°C and a roller speed of 30 m / min to obtain a lithium composite negative electrode 3 (lithium storage supplement layer thickness of 10 μm) to be used in batteries.

[0065] Example 4

[0066] Preparation of modified graphitized membrane: Use 5% solid content of graphene oxide oily slurry, then add 0.4% solid content of single-walled carbon nanotube slurry, and finally add 0.5% content of polyvinylidene fluoride to mix into a new slurry. The three are mixed evenly, and the mass ratio of graphene: single-walled carbon nanotube: polyvinylidene fluoride is 98:1:1. Use a 250μm doctor blade to apply the above new slurry on a PET plastic film coated with a thin silicone oil layer, and then dry it at 45 degrees for 10 hours to form a preliminary dried graphene oxide film. Remove the graphene oxide film from the PE The T plastic film is peeled off to obtain a self-supporting graphene oxide film. The graphene oxide film is then placed in a vitamin C solution (0.5 mol / L) for reduction. The temperature is controlled at 80°C and the reduction is carried out for 24 hours to obtain a reduced graphene film. The reduced graphene film is further compacted by the protection of the upper and lower film materials to obtain a formed graphene film. The rolled graphene film is then subjected to a high temperature treatment of 2500°C for 30 minutes to obtain a graphitized film. The graphitized film has a thickness of 12 μm and a tensile strength of 23.5 MPa.

[0067] Preparation of lithium composite negative electrode:

[0068] The active material used was a rolled lithium foil of 20 μm thickness. A roll of lithium foil and the rolled graphitized film of 12 μm thickness prepared above were unwound. With the help of a roller press, the pressure was set to 1.5 MPa to obtain a preliminary single-sided lithium composite negative electrode.

[0069] Another roll of 20 μm thick lithium foil and the preliminary single-sided lithium composite negative electrode was unwound, and a preliminary double-sided lithium composite negative electrode was obtained by means of a roller press with a pressure set to 4 MPa.

[0070] The preliminary double-sided lithium composite negative electrode was subjected to a hot roller press with a pressure of 1 MPa, a temperature of 45°C and a roller speed of 40 m / min to obtain a lithium composite negative electrode 4 to be used in batteries (the thickness of the lithium storage supplement layer was 7.5 μm).

[0071] Comparative Example 1:

[0072] The active material used was a rolled lithium foil of 20 μm thickness. Two rolls of lithium foil and 6 μm thick copper foil were unwound. A roller press was used with a pressure of 3 MPa to obtain a lithium composite negative electrode 5.

[0073] Comparative Example 2:

[0074] Preparation of ungraphitized membrane: First, a polyimide polymer was synthesized and carbonized at 1300°C for 1 hour to obtain an ungraphitized product (B). Product B, multi-walled carbon nanotubes, and polytetrafluoroethylene (powder, particle size less than 12 μm, Aladdin) were mixed in a mass ratio of 97.5:1:1.5. A trace amount of 1-methyl-2-pyrrolidone was added and mixed thoroughly. Using a roller press at a pressure of 5 MPa, a 17 μm thick membrane was prepared. The membrane was then rolled up with a thin layer of silicone oil-coated PET plastic film to obtain a rolled membrane with a tensile strength of 18.6 MPa.

[0075] The active material used was a rolled lithium foil of 20 μm thickness. A roll of lithium foil and the rolled 17 μm thick non-graphitized film prepared above were unwound. With the help of a roller press, the pressure was set to 1.5 MPa to obtain a preliminary single-sided lithium composite negative electrode.

[0076] Another roll of 20 μm thick lithium foil and the preliminary single-sided lithium composite negative electrode was unwound, and a preliminary double-sided lithium composite negative electrode was obtained by means of a roller press with a pressure set to 4 MPa.

[0077] The preliminary double-sided lithium composite negative electrode was subjected to a hot roller press with a pressure of 1 MPa, a temperature of 50° C., and a roller speed of 30 m / min to obtain a lithium composite negative electrode 6 to be used in batteries.

[0078] Comparative Example 3:

[0079] Preparation of graphitized membrane: First, a polyimide polymer was synthesized, and the polyimide was carbonized at 1300°C for 1 hour, and then graphitized at 2600°C for 1 hour to obtain a graphitized product (B). Product B and polytetrafluoroethylene (powder, particle size less than 12 μm, Aladdin) were mixed in a mass ratio of 98.5:1.5, and a trace amount of 1-methyl-2-pyrrolidone was added and mixed evenly. With the help of a roller press, the pressure was set to 5 MPa to prepare a membrane with a thickness of 17 μm. The membrane had a tensile strength of 17.8 MPa.

[0080] The active material used was a rolled lithium foil of 20 μm thickness. A roll of lithium foil and the rolled film of 17 μm thickness prepared above were unwound. A preliminary single-sided lithium composite negative electrode was obtained by means of a roller press with a pressure set to 1 MPa.

[0081] Another roll of 20 μm thick lithium foil and the preliminary single-sided lithium composite negative electrode was unwound, and a preliminary double-sided lithium composite negative electrode was obtained by means of a roller press with a pressure set to 4 MPa.

[0082] The preliminary double-sided lithium composite negative electrode was subjected to a hot roller press with a pressure of 1 MPa, a temperature of 50°C and a roller speed of 30 m / min to obtain a lithium composite negative electrode 7 to be used in batteries (the thickness of the lithium storage supplement layer was 1.5 μm).

[0083] The lithium composite negative electrode 1 of Example 1, the lithium composite negative electrode 2 of Example 2, the lithium composite negative electrode 3 of Example 3, the lithium composite negative electrode 4 of Example 4, the lithium composite negative electrode 5 of Comparative Example 1, the lithium composite negative electrode 6 of Comparative Example 2, and the lithium composite negative electrode 7 of Comparative Example 3 were used as negative electrodes, and the positive electrode was a lithium nickel cobalt manganese oxide positive electrode (positive electrode surface density of 38.5 mg / cm 2 ), the diaphragm uses a single-sided ceramic PE diaphragm with a thickness of 14μm, and the soft-pack battery is assembled. The electrolyte uses a liquid ether electrolyte. The charge and discharge rate is 0.2C, and the test voltage range is: 2.7-4.35V. The electrochemical performance of the seven groups is as follows Figure 1 shown.

[0084] Through the electrochemical cycle diagram ( Figure 2 ) It can be seen that the cycle performance of lithium composite negative electrodes 1, 2, 3, and 4 in Examples 1, 2, 3, and 4 is superior to that of lithium composite negative electrodes 5, 6, and 7 in Comparative Examples 1, 2, and 3. The capacity of the lithium composite negative electrodes in Examples 1, 2, 3, and 4 rapidly decays between 100 and 150 cycles, at which point the lithium storage supplementary layer begins to function. Between 150 and 200 cycles, the battery capacity increases, extending the cycle life of the four battery cells in the examples by more than 50 cycles. However, the lithium composite negative electrode 5 in Comparative Example 1 lacks a lithium storage layer due to its central copper layer. The lithium composite negative electrode 6 in Comparative Example 2 lacks a lithium storage layer due to its central non-graphitized membrane material. Consequently, its capacity linearly decays after approximately 150 cycles. In Comparative Example 3, the lithium storage supplementary layer is too thin (1.5 μm thick), failing to replenish the battery capacity in the later stages of the battery cycle, resulting in rapid capacity decay after 140 cycles.

[0085] Comparison of the data of Example 2 and Example 3 shows that the active material of the lithium composite negative electrode 3 of Example 3 uses lithium-magnesium alloy foil. Due to the presence of magnesium, it is beneficial to the uniform deposition of metallic lithium, and the electrochemical performance is slightly better.

[0086] The test method for the thickness of the lithium storage supplement layer is as follows: When the battery cell is cycled to 140 cycles, in an argon glove box, disassemble the discharged battery cell, remove the negative electrode sheet, peel off the powdered lithium and dead lithium on the surface of the negative electrode sheet, and rinse the surface of the electrode sheet with electrolyte, leaving only the graphitized film material and the lithium storage supplement layer. Then buckle it into a disc with an inner diameter of 14mm, place the lithium storage supplement layer side facing the diaphragm, and use the metal lithium disc as the counter electrode. Inject electrolyte and assemble it into a buckle battery for testing. The test process is as follows:

[0087] Set aside for 12 hours

[0088] Constant current charging current 3.08mA voltage 2V

[0089] Finish.

[0090] The cells of Example 1, Example 2, Example 3, Example 4, Comparative Example 2 and Comparative Example 3 were all tested according to the above-mentioned test method for the lithium storage supplement layer. The charging data of Example 1, Example 2, Example 3, Example 4 and Comparative Example 3 are shown in FIG. Figure 3 After standing for 12 hours, the battery was charged at a constant current of 3.08 mA, and the voltage of the battery was charged from 0.008 V to 2 V. All the lithium in the lithium storage supplement layer was transferred to the negative electrode. The capacity of the lithium storage supplement layer of the corresponding embodiment is shown in Table 1 below. The charging data of Comparative Example 2 is shown in Table 1 below. Figure 4 In Comparative Example 2, since there is no lithium storage supplement layer, the battery voltage remains at around 1.56V after 12 hours of storage. When charged at a constant current of 3.08mA, the battery voltage suddenly changes from 1.56V to nearly 4V, and the released capacity is 0, indicating that the membrane material in Comparative Example 2 has not been graphitized and no lithium storage supplement layer has been formed.

[0091] In Comparative Example 3, since there is no transmission channel of carbon nanotubes or carbon fibers, metallic lithium is not easy to enter the graphitized interlayer, so the thickness of the formed lithium storage supplement layer is only 1.5 μm, which is relatively thin.

[0092] Note: The capacity of the lithium storage supplement layer = 3.08mA (set current size) × Figure 3 / Figure 4 The time on the horizontal axis is used to obtain the capacity of the lithium storage supplement layer in Table 1;

[0093] The area of ​​the electrode is 1.54cm 2 In this way, the surface capacity of Example 1 / Example 2 / Example 3 / Example 4 / Comparative Example 2 / Comparative Example 3 can be calculated, and the approximate thickness of the lithium storage supplementary layer can be deduced.

[0094] Table 1. Charge capacity of the lithium storage supplementary layer in the assembled battery test

[0095]

[0096] The applicant declares that while the above-mentioned embodiments are used to illustrate the detailed structural features of the present application, the present application is not limited to the above-mentioned detailed structural features, which does not mean that the present application must rely on the above-mentioned detailed structural features in order to be implemented. Those skilled in the art should understand that any improvements to the present application, equivalent replacements for selected components, additions of auxiliary components, and selection of specific methods, etc., fall within the scope of protection and disclosure of the present application.

Claims

1. A lithium composite negative electrode, characterized in that: The lithium composite negative electrode comprises: A modified graphitized film material as a current collector, wherein the modified graphitized film material comprises graphite or a graphitized organic polymer and a modifier and a structural reinforcing agent, or is obtained by graphitizing a film material made of graphene oxide, a modifier and a structural reinforcing agent, wherein the modifier is selected from at least one of single-walled carbon nanotubes, multi-walled carbon nanotubes and nano-carbon fibers, the structural reinforcing agent is selected from at least one of polytetrafluoroethylene, polyvinylidene fluoride, styrene-butadiene rubber, carboxymethyl cellulose sodium and polyacrylic acid, and the organic polymer is selected from polyimide or polyacrylonitrile; An active material layer composited on at least one surface of the modified graphitized film, wherein the active material layer is a continuous or intermittently distributed metallic lithium or lithium alloy foil; and Through hot pressing and compounding, lithium atoms diffuse into the modified graphitized film material, insert into the interlayer gap of graphite or the gap between graphene and graphene to form a lithium storage supplement layer.

2. The lithium composite negative electrode according to claim 1, characterized in that The temperature of the graphitization treatment is 2300-3000° C., and the treatment time is 0.5-2 h.

3. The lithium composite negative electrode according to claim 1, characterized in that In the modified graphitized film material, the mass percentage of the modifier is 0.1%-10%, and the mass percentage of the structural reinforcing agent is 0.1%-10%.

4. The lithium composite negative electrode according to claim 1, characterized in that The thickness of the lithium storage supplement layer is 2-25 μm.

5. The lithium composite negative electrode according to claim 1, characterized in that: The sheet resistance of the modified graphitized film is 0.1-100 mΩ / cm 2 , the film thickness is 5-25μm, and the film density is 1.3-2.0g / cm 3 , the tensile strength of the membrane material is 15-100MPa; The thickness of the metal lithium or lithium alloy foil is 1-100 μm and the width is 50-1400 mm; The lithium alloy foil is a foil material formed by combining metallic lithium with any one or at least two elements of Ag, Au, Sn, Si, Zn, Al, Mg, In, Ga, B, Mn, Sb, Cr, C, V, Cu, Fe or Ti.

6. The lithium composite negative electrode according to any one of claims 1 to 5, characterized in that Both sides of the modified graphitized membrane are compounded with active material layers.

7. A method for preparing the lithium composite negative electrode according to claim 6, characterized in that: The method comprises the following steps: Step 1: Prepare the modified graphitized film material, and roll it up together with the release film on one side; Step 2: unwinding the metal lithium / lithium alloy foil and the modified graphitized film, and subjecting the modified graphitized film to a small pressure composite with the metal lithium / lithium alloy foil facing the side not attached with the release film, the pressure being set to 1-2 MPa, and removing the release film to obtain a single-sided lithium composite negative electrode; Step 3: unwinding another roll of lithium metal / lithium alloy foil, and press-compounding the side of the single-sided lithium composite negative electrode without composite lithium with the unrolled lithium metal / lithium alloy foil, with the pressure set to 3-5 MPa, to obtain a preliminary double-sided lithium composite negative electrode; Step 4: The preliminary double-sided lithium composite negative electrode is rolled by a hot roller, the temperature of the hot roller is 40-60° C., and the pressure is set to 1-2 MPa to obtain the lithium composite negative electrode.

8. The method according to claim 7, characterized in that The release film is a polyethylene terephthalate, polypropylene or polyethylene plastic film with a surface treated with a silicone oil coating.

9. The use of the lithium composite negative electrode according to any one of claims 1 to 6, wherein the lithium composite negative electrode is directly used as the negative electrode of a liquid or solid lithium battery, and the positive electrode of the lithium battery uses lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium-rich manganese-based positive electrode material, lithium iron phosphate, lithium iron manganese phosphate, sulfur-carbon positive electrode, sulfurized polyacrylonitrile or lithium cobalt oxide.