A method for micro-nano fine bubble flotation-ultrasonic salt mixing decomposition of fine-grained scheelite
Through the micro-nano bubble flotation of fine-grained scheelite - ultrasonic mixing and salt decomposition method, ultrasonic waves and mechanical stirring are used to enhance bubble mineralization, combined with combined inhibitors and composite decomposers, the separation of fine-grained scheelite and gangue minerals is solved. and efficient decomposition issues, achieving efficient scheelite recovery and sodium tungstate extraction.
Patent Information
- Application Number
- CN202411148384.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The existing fine-grained scheelite beneficiation technology is difficult to efficiently separate fine-grained scheelite and calcium-containing gangue minerals. Moreover, the traditional decomposition and leaching process consumes high energy, serious equipment wear, and difficult recovery of decomposition agents.
The micro-nano bubble flotation-ultrasonic salt decomposition method of micro-grained scheelite is used, which includes three steps of ultrasonic mineralization, micro-nano bubble selection and ultrasonic salt decomposition. Ultrasonic waves and mechanical stirring are used to enhance bubble mineralization, combined with Combining inhibitors and complex decomposition agents to achieve separation and efficient decomposition of scheelite and gangue minerals.
It improves the flotation recovery rate and decomposition efficiency of scheelite, reduces the amount of decomposition agent and energy consumption, avoids the wear and tear of high-pressure equipment, and achieves efficient extraction of sodium tungstate.
Smart Images

Figure CN118649771B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fine-grained scheelite beneficiation, and in particular relates to a micro-nano fine bubble flotation-ultrasonic salt mixing decomposition method for fine-grained scheelite. Background Art
[0002] Tungsten is a rare metal and one of the main raw materials for the production of tungsten metal industry. With the long-term and large-scale development of mineral resources, high-grade, easy-to-handle, coarse-grained rich ore resources are becoming increasingly scarce. Fine-grained scheelite has large reserves and has the characteristics of small mass and large specific surface area. It is difficult to float up into the concentrate during conventional flotation. In addition, scheelite often coexists with calcium-containing gangue minerals. The floatability of such gangue minerals is similar to that of scheelite, making flotation separation difficult. Therefore, it is of great value to develop new and efficient separation technologies for fine-grained scheelite minerals to achieve efficient recovery of the fine-grained minerals.
[0003] The decomposition and leaching of scheelite mainly adopts the Na2CO3 high-pressure decomposition and leaching process, and there is also the NaOH high-pressure decomposition and leaching process. The amount of Na2CO3 used in the Na2CO3 high-pressure decomposition and leaching process reaches 2.5~4.5 times the theoretical amount. For low-grade fine-grained scheelite concentrate, it even requires more than 5 times. In addition, high temperature and high pressure are required to strengthen the leaching. The operating temperature is as high as 225℃ and the pressure that the equipment must be able to withstand must be greater than 2MPa. There will be problems such as serious wear of high-pressure equipment, and the excess sodium carbonate is difficult to recover economically. Based on this, it is of great strategic and practical significance to develop scheelite flotation and decomposition leaching technology with low additive dosage, low reaction temperature and high decomposition efficiency. Summary of the invention
[0004] Aiming at the problems existing in the existing fine-grained scheelite beneficiation technology, the present invention provides a method for micro-nano fine bubble flotation-ultrasonic salt decomposition of fine-grained scheelite. The invention mainly includes three steps of ultrasonic mineralization flotation, micro-nano fine bubble selection, and ultrasonic salt decomposition to achieve effective flotation separation of useful minerals and gangue minerals in scheelite and efficient decomposition of scheelite.
[0005] The micro-nano fine bubble flotation-ultrasonic salt mixing decomposition method of fine-grained scheelite of the present invention comprises the following steps:
[0006] Step 1: Ultrasonic mineralization process: Add the combined inhibitor PA and the collector to the scheelite slurry, enter the ultrasonic mineralization process of the flotation process, stir and float under an ultrasonic environment, so that the bubbles and fine scheelite generated during the operation are fully mineralized to obtain ultrasonic mineralized slurry.
[0007] Step 2: Scheelite roughing process: The ultrasonic mineralized slurry of step 1 enters the roughing process of the flotation process, which includes a roughing operation and a scavenging operation. After the roughing process is completed, a roughing tungsten concentrate slurry is obtained.
[0008] Step 3: Micro-nano fine bubble selection process: Add the combined inhibitor PA to the rough tungsten concentrate pulp in step 2, and then add the collector to enter the micro-nano fine bubble selection process of the flotation process. This selection process includes 2 to 4 stages of micro-nano fine bubble selection operations. The micro-nano fine bubbles refer to the micro-nano fine bubbles that are transported to the pulp during the selection process. The micro-nano fine bubbles are evenly dispersed in the pulp. After the selection process is completed, the flotation tungsten concentrate pulp is obtained. The tungsten grade of the scheelite flotation tungsten concentrate is higher than 23%, and the recovery rate is higher than 40%.
[0009] Step 4 solid-liquid separation process: The flotation tungsten concentrate slurry of step 3 enters the solid-liquid separation process to obtain scheelite concentrate and filtrate, and the filtrate is circulated to the ultrasonic mineralization process of step 1 to form a water circuit circulation.
[0010] Step 5: Ultrasonic salt mixing decomposition process: Add water and a composite decomposition agent to the scheelite concentrate in step 4 to form a decomposition system, enter the ultrasonic salt mixing decomposition process, stir under an ultrasonic environment to decompose the scheelite concentrate to generate sodium tungstate, and obtain a mineral containing sodium tungstate. At this time, a small amount of sodium tungstate will be dissolved in the water, but the water content is low at this time, and most of the sodium tungstate is in a precipitated state and mixed with the slag.
[0011] Step 6: Water leaching separation process: The minerals containing sodium tungstate in step 5 enter the water leaching separation process, so that the sodium tungstate is effectively dissolved, and other substances are contained in the slag, so as to achieve the separation of sodium tungstate.
[0012] The micro-grained scheelite is a scheelite ore material with a particle size of -15 μm and a content of more than 70%.
[0013] The ultrasonic frequency in step 1 is 0.3 MHz to 0.8 MHz; the pulp concentration during flotation is 35% to 45%, and the pH value is 8 to 10.
[0014] The micro-nano bubbles described in step 3 refer to bubbles with a Sauter diameter of ≤400µm when bubbles occur, and the superficial gas velocity is controlled at 1.0cm / s~1.5cm / s; the flotation temperature is 20℃~35℃, and the pulp pH=7~10.
[0015] The combined inhibitor PA in step 1 and step 3 is composed of PSS (sodium polystyrene sulfonate) and ATMP (aminotrimethylene phosphonic acid) in a mass ratio of (8-4):1, and the collector is sodium oleate.
[0016] In step 1, the corresponding dosage of combined inhibitor PA for each ton of scheelite slurry is 90g~160g, and the corresponding dosage of collector is 45g~90g; in step 3, the corresponding dosage of collector for each ton of rough tungsten concentrate slurry is 25g~40g, and the corresponding dosage of combined inhibitor PA is 40g~80g.
[0017] The water content of the scheelite concentrate obtained by filtration in step 4 is less than 13%.
[0018] The ultrasonic frequency in step 5 is 19.7KHz~22.3KHz; the composite decomposition agent includes sodium phosphate and sodium hydroxide, and the mass ratio of sodium phosphate to sodium hydroxide is 2:1; the dosage of the composite decomposition agent is 3%~10% of the mass of the scheelite concentrate; the liquid-solid mass ratio of the decomposition system is 8:1~3:1, the decomposition temperature is 140℃~200℃, and the decomposition time is 2h~4h.
[0019] In step 6, the liquid-to-solid mass ratio of water leaching separation is 15:1~25:1, stirring is 1h~3h, and the tungsten leaching rate is higher than 90%.
[0020] The present invention first carries out an ultrasonic mineralization process before the roughing process of the flotation process, and combines mechanical stirring and collectors in an ultrasonic environment to enhance bubble mineralization, and strengthen the collision and adhesion effect between the flotation bubbles and the pulp particles; in the concentrating stage of the flotation process, micro-nano fine bubbles are uniformly dispersed in the pulp, and combined with the collector, the scheelite particles are brought into the foam layer by the micro-nano fine bubbles, and the calcium-containing gangue minerals are selectively suppressed, thereby strengthening the separation of fine scheelite and gangue minerals during the flotation process. Ultrasonic mineralization flotation, roughing, micro-nano fine bubble concentrating and other processes are closely linked to form a micro-nano fine bubble multi-stage mineralization flotation combination, realizing the enhancement of bubble mineralization by ultrasonic and mechanical force coupling, the enhancement of fine scheelite separation by micro-nano fine bubbles, and the enhancement of concentrate quality separation by combined inhibitors, thereby realizing the efficient flotation of fine scheelite. The scheelite concentrate obtained after the flotation is subjected to ultrasonic salt decomposition, and the scheelite concentrate is decomposed and converted into water-soluble sodium tungstate in an ultrasonic environment in combination with mechanical stirring and a composite decomposition agent; and then separated by water leaching to obtain a sodium tungstate product. The present invention completes two major processes of raw ore from ore dressing to decomposition at one time. By adopting the method of the present invention, the flotation tungsten concentrate has a high grade and a high decomposition conversion rate of the tungsten concentrate, and a sodium tungstate product that is easy to use can be directly obtained from the ore raw material in an efficient manner.
[0021] Compared with the conventional technology, the micro-nano fine bubble flotation-ultrasonic salt mixing decomposition method of fine scheelite of the present invention has the following beneficial effects:
[0022] 1. Ultrasonic mineralization is used for flotation of fine-grained scheelite. On the one hand, the external ultrasonic vibration field can greatly increase the contact probability between mineral particles and reagent molecules, and on the other hand, it can also promote the generation and diffusion of micro-nano bubbles, so that the mineralization of ore particles and bubbles in the slurry is effectively improved.
[0023] 2. Micro-nano fine bubble selection effectively captures fine-grained scheelite and inhibits gangue minerals. Fine-grained scheelite has poor interaction with ordinary bubbles, and micro-nano bubbles can greatly improve the interaction with fine-grained scheelite. At the same time, the self-developed combined inhibitor PA can effectively inhibit calcium-containing gangue minerals. By changing the surface charge properties, the gangue minerals that are originally similar to the surface charge of scheelite are effectively inhibited, and the dosage of the inhibitor (130g / t~240g / t) is much less than the dosage of conventional inhibitor water glass (1000g / t~4000g / t).
[0024] 3. The composite decomposer composed of sodium phosphate and other materials is more environmentally friendly than traditional decomposers such as Na2CO3 and NaOH, and does not require a high-pressure environment. The reaction can be completed under normal pressure, and the amount of decomposer used is effectively reduced, which is only 2%~10% of the traditional decomposer.
[0025] 4. The salt-mixing decomposition process of the present invention adopts ultrasonic salt-mixing decomposition, because the precipitation material (Ca5(PO4)3OH) produced in the decomposition process of scheelite by sodium phosphate (Na3PO4) will wrap on the surface of ore particles to cover the particles, affecting liquid-solid contact and diffusion, thereby affecting the decomposition rate. Ultrasonic waves can act on the precipitation on the surface of particles, avoid the covering of particles by the product layer, weaken the influence of diffusion control on the reaction, promote the continuous reaction, and thus improve the reaction efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a process schematic diagram of the micro-nano fine bubble flotation-ultrasonic salt mixing decomposition method of fine-grained scheelite described in the present invention. DETAILED DESCRIPTION
[0027] The technical scheme of the present invention is clearly and completely described below in conjunction with the embodiments and the accompanying drawings. It should be pointed out that the embodiments described in the present invention are only used to further explain and illustrate, rather than to limit the scope of application. Based on the present invention, all other embodiments obtained by those skilled in the art without making creative work belong to the protection scope of the present invention.
[0028] The process flow of each embodiment is as follows Figure 1 shown.
[0029] Example 1 This example uses a fine-grained scheelite from Jiangxi with a WO3 content of 0.85% as raw material, and the content of the ore particle size -15μm is 82%. The specific steps are as follows:
[0030] Step 1: Ultrasonic mineralization process: add pH adjuster lime to the pulp to make the pulp pH = 10, the corresponding dosage of combined inhibitor PA per ton of pulp is 160g (the mass ratio of PSS to ATMP is 6:1), the dosage of collector sodium oleate is 90g, the pulp concentration is 41%, and the ultrasonic mineralization process of the flotation process is entered. The ultrasonic frequency is 0.8MHz, so that the bubbles and fine scheelite particles generated during the operation are fully mineralized under the coupling effect of ultrasound and mechanical stirring to obtain ultrasonic mineralized pulp.
[0031] Step 2 Scheelite roughing process: The ultrasonic mineralized slurry in step 1 enters the roughing process of the flotation process, which includes a roughing operation and a scavenging operation. After the roughing process is completed, a roughing tungsten concentrate slurry is obtained. The gangue minerals are suppressed by the combined inhibitor, and the scheelite is not affected by the inhibitor, so it is effectively separated from the gangue minerals.
[0032] Step 3: Micro-nano fine bubble selection process: adjust the pH value of the rough tungsten concentrate slurry in step 2 to pH=8, add the combined inhibitor PA (the mass ratio of PSS to ATMP is 6:1) to the slurry to selectively inhibit the gangue minerals, and the application amount is 80g per ton of slurry; then add the collector sodium oleate to make the scheelite adsorb the collector, and the application amount is 40g per ton of slurry; enter the micro-nano fine bubble selection process of the flotation process, which includes 2 stages of micro-nano fine bubble selection operations. During the selection operation, micro-nano fine bubbles are transported into the slurry, the bubble Sauter diameter is ≤400µm, the apparent gas velocity is controlled at 1.0cm / s, the micro-nano fine bubbles are uniformly dispersed in the slurry, the flotation temperature is 20°C, and after the selection process, a flotation tungsten concentrate slurry is obtained, the tungsten grade is 28.4%, and the recovery rate is 70.5%.
[0033] Step 4 solid-liquid separation process: The flotation tungsten concentrate slurry of step 3 enters the solid-liquid separation process to obtain scheelite concentrate and filtrate containing reagents. The water content of the concentrate is 11.5%. The filtrate is circulated to the ultrasonic mineralization process in step 1 to form a water circuit.
[0034] Step 5: Ultrasonic salt decomposition process: add water and a composite decomposition agent (the mass ratio of sodium phosphate and sodium hydroxide is 2:1) to the scheelite concentrate of step 4, enter the ultrasonic salt decomposition process, stir at an ultrasonic frequency of 22.3KHz to decompose the scheelite concentrate, the liquid-solid ratio of the decomposition process is 8:1, the amount of the composite decomposition agent is 10% of the mass of the scheelite concentrate, the salt decomposition temperature is 200°C, the salt decomposition time is 4h, and a mineral containing sodium tungstate is obtained.
[0035] Step 6: Water leaching separation process: The mineral containing sodium tungstate in step 5 enters the water leaching separation process, with a liquid-to-solid ratio of 25:1 and stirred for 3 hours to effectively dissolve the sodium tungstate. Other substances are contained in the slag to achieve the separation of sodium tungstate. The tungsten leaching rate is 96%.
[0036] Example 2 This example uses a Hunan fine-grained scheelite with a WO3 content of 0.95% as raw material, and the content of the ore particle size -15μm is 75%. The specific steps are as follows:
[0037] Step 1: Ultrasonic mineralization process: add pH adjuster lime to the pulp to make the pulp pH = 8, the corresponding dosage of combined inhibitor PA per ton of pulp is 90g (the mass ratio of PSS to ATMP is 7:1), the dosage of collector sodium oleate is 45g, the pulp concentration is 35%, and enters the ultrasonic mineralization process of the flotation process. The ultrasonic frequency is 0.5MHz, so that the bubbles and fine scheelite particles generated during the operation are fully mineralized under the coupling effect of ultrasound and mechanical stirring to obtain ultrasonic mineralized pulp.
[0038] Step 2: Scheelite roughing process: The ultrasonic mineralized slurry of step 1 enters the roughing process of the flotation process, which includes a roughing operation and a scavenging operation. After the roughing process is completed, a roughing tungsten concentrate slurry is obtained.
[0039] Step 3: Micro-nano fine bubble selection process: adjust the pH value of the roughing tungsten concentrate slurry in step 2 to pH=9, add the combined inhibitor PA (the mass ratio of PSS to ATMP is 7:1) to the slurry, and the application amount is 40g per ton of slurry; then add the collector sodium oleate, and the application amount is 25g per ton of slurry; enter the micro-nano fine bubble selection process of the flotation process, which includes 3 stages of micro-nano fine bubble selection operations. During the selection operation, micro-nano fine bubbles are transported into the slurry, the bubble Sauter diameter is ≤400µm, the apparent gas velocity is controlled at 1.3cm / s, the micro-nano fine bubbles are uniformly dispersed in the slurry, the flotation temperature is 25°C, and after the selection process, a flotation tungsten concentrate slurry is obtained, the tungsten grade is 30%, and the recovery rate is 72.4%.
[0040] Step 4 solid-liquid separation process: The flotation tungsten concentrate slurry of step 3 enters the solid-liquid separation process to obtain scheelite concentrate and filtrate containing reagents. The water content of the concentrate is 12.5%. The filtrate is circulated to the ultrasonic mineralization process in step 1 to form a water circuit.
[0041] Step 5: Ultrasonic salt decomposition process: add water and a composite decomposition agent (the mass ratio of sodium phosphate and sodium hydroxide is 2:1) to the scheelite concentrate of step 4, enter the ultrasonic salt decomposition process, stir at an ultrasonic frequency of 22.2KHz to decompose the scheelite concentrate, the liquid-solid ratio of the decomposition process is 3:1, the amount of the composite decomposition agent is 3% of the mass of the scheelite concentrate, the salt decomposition temperature is 140°C, the salt decomposition time is 2h, and a mineral containing sodium tungstate is obtained.
[0042] Step 6: Water leaching separation process: The mineral containing sodium tungstate in step 5 enters the water leaching separation process, with a liquid-solid ratio of 15:1 and stirred for 1 hour to effectively dissolve the sodium tungstate. Other substances are contained in the slag to achieve the separation of sodium tungstate. The tungsten leaching rate is 90.20%.
[0043] Example 3 This example uses a fine-grained scheelite from Yunnan with a WO3 content of 0.7% as raw material, and the content of the ore particle size -15μm is 73%. The specific steps are as follows:
[0044] Step 1: Ultrasonic mineralization process: add pH adjuster lime to the pulp to make the pulp pH = 9, the corresponding dosage of combined inhibitor PA per ton of pulp is 125g (the mass ratio of PSS to ATMP is 8:1), the dosage of collector sodium oleate is 75g, the pulp concentration is 45%, and enters the ultrasonic mineralization process of the flotation process. The ultrasonic power is 0.3MHz, so that the bubbles and fine scheelite particles generated during the operation are fully mineralized under the coupling effect of ultrasound and mechanical stirring to obtain ultrasonic mineralized pulp.
[0045] Step 2: Scheelite roughing process: The ultrasonic mineralized slurry of step 1 enters the roughing process of the flotation process, which includes a roughing operation and a scavenging operation. After the roughing process is completed, a roughing tungsten concentrate slurry is obtained.
[0046] Step 3: Micro-nano fine bubble selection process: adjust the pH value of the roughing tungsten concentrate slurry in step 2 to pH=10, add the combined inhibitor PA (the mass ratio of PSS to ATMP is 8:1) to the slurry, and the application amount is 60g per ton of slurry; then add the collector sodium oleate, and the application amount is 36g per ton of slurry; enter the micro-nano fine bubble selection process of the flotation process, which includes 4 stages of micro-nano fine bubble selection operations. During the selection operation, micro-nano fine bubbles are transported into the slurry, the bubble Sauter diameter is ≤400µm, the apparent gas velocity is controlled at 1.5cm / s, the micro-nano fine bubbles are uniformly dispersed in the slurry, the flotation temperature is 30°C, and after the selection process, a flotation tungsten concentrate slurry is obtained, the tungsten grade is 29.5%, and the recovery rate is 71.3%.
[0047] Step 4 solid-liquid separation process: The flotation tungsten concentrate slurry of step 3 enters the solid-liquid separation process to obtain scheelite concentrate and filtrate containing reagents. The water content of the concentrate is 12%. The filtrate is circulated to the ultrasonic mineralization process in step 1 to form a water circuit.
[0048] Step 5: Ultrasonic salt decomposition process: add water and a composite decomposition agent (the mass ratio of sodium phosphate and sodium hydroxide is 2:1) to the scheelite concentrate of step 4, enter the ultrasonic salt decomposition process, stir at an ultrasonic frequency of 19.7KHz to decompose the scheelite concentrate, the liquid-solid ratio of the decomposition process is 5:1, the amount of the composite decomposition agent is 6% of the mass of the scheelite concentrate, the salt decomposition temperature is 175°C, the salt decomposition time is 3h, and a mineral containing sodium tungstate is obtained.
[0049] Step 6: Water leaching separation process: The mineral containing sodium tungstate in step 5 enters the water leaching separation process, with a liquid-solid ratio of 20:1 and stirred for 2 hours to effectively dissolve the sodium tungstate. Other substances are contained in the slag to achieve the separation of sodium tungstate. The tungsten leaching rate is 93.8%.
[0050] Example 4 This example uses a Hunan fine-grained scheelite with a WO3 content of 0.84% as raw material, and the content of the ore particle size -15μm is 74%. The specific steps are as follows:
[0051] Step 1: Ultrasonic mineralization process: add pH adjuster lime to the pulp to make the pulp pH = 8, the corresponding dosage of combined inhibitor PA per ton of pulp is 110g (the mass ratio of PSS to ATMP is 4:1), the dosage of collector sodium oleate is 75g, the pulp concentration is 43%, and enters the ultrasonic mineralization process of the flotation process. The ultrasonic power is 0.4MHz, so that the bubbles and fine scheelite particles generated during the operation are fully mineralized under the coupling effect of ultrasound and mechanical stirring to obtain ultrasonic mineralized pulp.
[0052] Step 2: Scheelite roughing process: The ultrasonic mineralized slurry of step 1 enters the roughing process of the flotation process, which includes a roughing operation and a scavenging operation. After the roughing process is completed, a roughing tungsten concentrate slurry is obtained.
[0053] Step 3: Micro-nano fine bubble selection process: adjust the pH value of the roughing tungsten concentrate slurry in step 2 to pH=10, add the combined inhibitor PA (the mass ratio of PSS to ATMP is 4:1) to the slurry, and the application amount is 55g per ton of slurry; add the collector sodium oleate, and the application amount is 35g per ton of slurry; enter the micro-nano fine bubble selection process of the flotation process, which includes 3 stages of micro-nano fine bubble selection operations. During the selection operation, micro-nano fine bubbles are transported into the slurry, the Sauter diameter of the bubbles is ≤400µm, the apparent gas velocity is controlled at 1.2cm / s, the micro-nano fine bubbles are uniformly dispersed in the slurry, the flotation temperature is 35°C, and after the selection process, a flotation tungsten concentrate slurry is obtained, the tungsten grade is 28.5%, and the recovery rate is 72.5%.
[0054] Step 4 solid-liquid separation process: The flotation tungsten concentrate slurry of step 3 enters the solid-liquid separation process to obtain scheelite concentrate and a filtrate containing reagents. The water content of the concentrate is 11%. The filtrate is circulated to the ultrasonic mineralization process in step 1 to form a water circuit.
[0055] Step 5: Ultrasonic salt decomposition process: add water and a composite decomposition agent (the mass ratio of sodium phosphate and sodium hydroxide is 2:1) to the scheelite concentrate of step 4, enter the ultrasonic salt decomposition process, stir at an ultrasonic frequency of 22.1 KHz to decompose the scheelite concentrate, the liquid-solid ratio of the decomposition process is 4:1, the amount of the composite decomposition agent is 8% of the mass of the scheelite concentrate, the salt decomposition temperature is 180°C, the salt decomposition time is 3 hours, and a mineral containing sodium tungstate is obtained.
[0056] Step 6: Water leaching separation process: The mineral containing sodium tungstate in step 5 enters the water leaching separation process, with a liquid-to-solid ratio of 15:1 and stirred for 3 hours to effectively dissolve the sodium tungstate. Other substances are contained in the slag to achieve the separation of sodium tungstate. The tungsten leaching rate is 92%.
[0057] Comparative Example 1
[0058] In this comparative example, the mineralization process of step 1 is not ultrasonicated, and the concentrating process of step 3 is not fed into the pulp, and the remaining steps are the same as those of Example 1. At this time, the recovery rate of tungsten in the flotation tungsten concentrate in step 3 is only 35.1%, which is significantly lower than the recovery rate of 70.5% of the flotation tungsten concentrate in step 3 of Example 1. This is because in the absence of ultrasound and micro-nano bubbles, the fine scheelite particles in the original ore cannot be fully combined with the reagents (collectors and inhibitors) and bubbles, so the recovery rate is greatly reduced.
[0059] Comparative Example 2
[0060] In this comparative example, conventional depressant water glass is used in step 1 and step 3, and combined depressant PA is not used. The amount of water glass used and the remaining steps are the same as those in Example 2. At this time, the grade of tungsten in the flotation tungsten concentrate in step 3 is 15%, which is significantly lower than the tungsten grade of 30% in the flotation tungsten concentrate in step 3 of Example 2. This is because conventional depressant water glass has poor inhibitory effect on gangue minerals at the same dosage, and gangue minerals enter the concentrate in large quantities, and qualified concentrate cannot be obtained, resulting in the inability to separate the concentrate and tail.
[0061] Comparative Example 3
[0062] In this comparative example, the decomposition process of step 5 does not use ultrasound, and the remaining steps are the same as those of Example 2. At this time, the tungsten leaching rate of step 6 is only 82.1%, which is significantly lower than the tungsten leaching rate of 90.20% in step 6 of Example 2. This is because the products produced by the decomposition reaction in step 5 cover the surface of the mineral particles to hinder the reaction diffusion. In the absence of ultrasound, these covers cannot be disintegrated, thereby hindering the dissociation and release of tungsten.
Claims
1. A method for micro-nano fine bubble flotation-ultrasonic salt mixing decomposition of fine-grained scheelite, characterized by: The following steps are involved: Step 1: Ultrasonic mineralization process: Add the combined inhibitor PA and the collector to the scheelite slurry, enter the ultrasonic mineralization process of the flotation process, stir and flotate under an ultrasonic environment, so that the bubbles and fine scheelite generated during the operation are fully mineralized to obtain an ultrasonic mineralized slurry; Step 2: Scheelite roughing process: The ultrasonic mineralized slurry in step 1 enters the roughing process of the flotation process, which includes a roughing operation and a scavenging operation. After the roughing operation is completed, a roughing tungsten concentrate slurry is obtained; Step 3: Micro-nano fine bubble selection process: add the combined depressant PA to the roughing tungsten concentrate pulp of step 2, and then add the collector to enter the micro-nano fine bubble selection process of the flotation process, which includes 2 to 4 stages of micro-nano fine bubble selection operations; the micro-nano fine bubbles refer to the micro-nano fine bubbles transported into the pulp during the selection operation, and the micro-nano fine bubbles are evenly dispersed in the pulp. After the selection process is completed, the flotation tungsten concentrate pulp is obtained; Step 4 solid-liquid separation process: The flotation tungsten concentrate slurry of step 3 enters the solid-liquid separation process to obtain scheelite concentrate and filtrate; Step 5: Ultrasonic salt mixing decomposition process: water and a composite decomposition agent are added to the scheelite concentrate in step 4 to form a decomposition system, and then the scheelite concentrate is stirred under an ultrasonic environment to decompose the scheelite concentrate to generate sodium tungstate, thereby obtaining a mineral containing sodium tungstate components; Step 6: Water leaching and separation process: The minerals containing sodium tungstate in step 5 enter the water leaching and separation process, so that the sodium tungstate is effectively dissolved, and other substances are contained in the slag, so as to achieve the separation of sodium tungstate; The combined inhibitor PA in step 1 and step 3 comprises sodium polystyrene sulfonate and aminotrimethylenephosphonic acid.
2. The micro-nano fine bubble flotation-ultrasonic salt mixing decomposition method of fine-grained scheelite according to claim 1 is characterized by: The micro-grained scheelite is a scheelite ore material with a particle size of -15 μm and a content of more than 70%.
3. The method for micro-nano fine bubble flotation-ultrasonic salt mixing decomposition of fine-grained scheelite according to claim 1 is characterized in that: The ultrasonic frequency in step 1 is 0.3 MHz to 0.8 MHz; the ultrasonic frequency in step 5 is 19.7 KHz to 22.3 KHz.
4. The method for micro-nano fine bubble flotation-ultrasonic salt mixing decomposition of fine-grained scheelite according to claim 1 is characterized in that: The micro-nano bubbles in step 3 are bubbles with a Sauter diameter of ≤400 μm when bubbles occur, and the superficial gas velocity is controlled at 1.0 cm / s to 1.5 cm / s.
5. The method for micro-nano fine bubble flotation-ultrasonic salt mixing decomposition of fine-grained scheelite according to claim 1 is characterized in that: The combined inhibitor PA in step 1 and step 3 comprises sodium polystyrene sulfonate and aminotrimethylenephosphonic acid, and the mass ratio of the two is (8-4):
1.
6. The method for micro-nano fine bubble flotation-ultrasonic salt mixing decomposition of fine-grained scheelite according to claim 5 is characterized in that: In step 1, the corresponding dosage of combined inhibitor PA for each ton of scheelite slurry is 90g-160g, and the corresponding dosage of collector is 45g-90g; in step 3, the corresponding dosage of collector for each ton of rough tungsten concentrate slurry is 25g-40g, and the corresponding dosage of combined inhibitor PA is 40g-80g.
7. The method for micro-nano fine bubble flotation-ultrasonic salt mixing decomposition of fine-grained scheelite according to claim 1 is characterized in that: In step 1, the slurry concentration during flotation is 35% to 45%, and the pH value is 8 to 10; in step 3, the flotation temperature is 20° C. to 35° C., and the slurry pH value is 7 to 10.
8. The micro-nano fine bubble flotation-ultrasonic salt mixing decomposition method of fine-grained scheelite according to claim 1 is characterized by: The composite decomposition agent in step 5 includes sodium phosphate and sodium hydroxide in a mass ratio of 2:
1. The amount of the composite decomposition agent used is 3% to 10% of the mass of the scheelite concentrate.
9. The micro-nano fine bubble flotation-ultrasonic salt mixing decomposition method of fine-grained scheelite according to claim 1 is characterized by: The liquid-to-solid mass ratio of the decomposition system in step 5 is 8:1 to 3:1, the decomposition temperature is 140° C. to 200° C., and the decomposition time is 2 h to 4 h.
10. The micro-nano fine bubble flotation-ultrasonic salt mixing decomposition method of fine-grained scheelite according to claim 1, characterized in that: The liquid-to-solid mass ratio of the water immersion separation in step 6 is 15:1 to 25:1, and the stirring is performed for 1 hour to 3 hours.
Citation Information
Patent Citations
Method for separating scheelite and calcite through ultrasonic flash-asynchronous flotation
CN111822152A
Flotation method and system for ilmenite
CN113941453A
Novel micro-nano bubble reinforced micro-fine particle mineral flotation recovery system and method
CN114769006A
Method for recovery of high-grade scheelite concentrate and facility for recovery of scheelite concentrate