An optimized repair method for surface cracks of positive electrode material precursor
By adopting two surface crack repair methods in the precursor of high nickel positive electrode material, the sphere cracking problem is solved, and the product pass rate and performance stability are improved.
Patent Information
- Application Number
- CN202411146602.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The precursors of high-nickel positive electrode materials often experience spherical cracking during sintering, resulting in a decline in the performance of lithium-ion batteries. The existing technology surface crack repair methods are not thorough enough, which affects the product qualification rate.
在正极材料前驱体成长至目标粒径后,降低搅拌转速,升高温度,加入碱性溶液和抗氧化剂的混合修复液进行一次表面裂纹修复,再次使用氨水和硫酸铵溶液的混合溶液进行二次修复,确保裂纹的彻底修复。
Through the two surface crack repair processes, the pass rate of the positive electrode material precursor is significantly improved, the negative impact of spherical cracks on performance is avoided, and the high quality and stability of the material are ensured.
Smart Images

Figure CN118651901B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high-nickel positive electrode material precursors, and in particular relates to an optimized repair method for surface cracks of a positive electrode material precursor. Background Art
[0002] With the development of society and the change of lifestyle, the requirements for lithium-ion batteries are getting higher and higher. In order to meet the growing demand for portable electronic products, electric vehicles and large-scale energy storage devices, it is urgent to develop positive electrode materials with high energy density, long cycle life and high safety. High nickel positive electrode materials have become one of the most promising positive electrode materials due to their higher specific capacity.
[0003] Since the nickel content of the high-nickel positive electrode material precursor is high, the surface primary particles are finer and have better sphericity than the low-nickel precursor, and cracks often appear on the surface of the sphere. When the high-nickel positive electrode material is sintered, the sphere often cracks, affecting the performance of the positive electrode material, and thus causing the performance of the lithium-ion battery to decline. The present invention aims to develop an optimized repair method for surface cracks of a positive electrode material precursor, so as to achieve the goal of sintering high-nickel positive electrode materials without cracking by repairing the surface cracks of the positive electrode material precursor, thereby optimizing the performance of the positive electrode material.
[0004] For example, the patent document CN 116789190A discloses a method for repairing cracks in a positive electrode material precursor, which includes the following steps: in the process of preparing a positive electrode material precursor by coprecipitation reaction, when the particle size of the positive electrode material precursor reaches the target particle size, the reaction system is allowed to stand, and then the upper clear liquid after standing and stratification is removed to obtain a slurry to be repaired; an alkaline solution is mixed with the slurry to be repaired, and a thickener is continued to be mixed, wherein the alkaline substance in the alkaline solution includes any one or a combination of at least two of sodium hydroxide, sodium carbonate or sodium bicarbonate, and the thickener includes any one or a combination of at least two of sodium hydroxymethyl cellulose, sodium polyacrylate or sodium alginate; the temperature is raised to repair the cracks. The repair method provided in the patent document can repair cracks on the surface of large-particle precursors and high-nickel precursors, effectively improving the product qualification rate. However, the method for repairing surface cracks of positive electrode materials reported in the patent document only repairs surface cracks in the alkali addition process once, and a part of the positive electrode material precursor material after the repair is completed will still have surface crack defects, and the repair is not perfect and thorough. Therefore, it is necessary to optimize and improve the repair method of the patent document to better improve the product qualification rate. Summary of the invention
[0005] The technical problem solved by the present invention is to provide a method for optimizing and repairing surface cracks of a positive electrode material precursor, wherein the method stops the reaction when the positive electrode material precursor grows to a target D50, reduces the stirring speed, increases the temperature, adds a repair liquid and a mixed solution of an ammonia solution and an ammonium sulfate solution, and optimizes and repairs the cracks for 24 to 48 hours. The crack optimization and repair method of the present invention can achieve thorough repair of surface cracks of a positive electrode material precursor through two surface crack repair processes, thereby improving the qualified rate of the positive electrode material precursor, and can effectively avoid the influence of the ball cracking of the positive electrode material precursor on the performance of the positive electrode material.
[0006] The present invention adopts the following technical solution to solve the above technical problems, a method for optimizing and repairing surface cracks of a positive electrode material precursor, and the specific steps are as follows:
[0007] Step S1, in the process of preparing the positive electrode material precursor by coprecipitation reaction, when the particle size of the positive electrode material precursor reaches the target particle size, the reaction is finished, and the material in the reactor is the material to be repaired;
[0008] Step S2, introducing an inert protective gas into the reactor so that the oxygen content in the reactor is less than 1.5%;
[0009] Step S3, reducing the speed of the reactor and increasing the temperature of the reactor to 55-85° C.;
[0010] Step S4, adding a repair liquid into the reactor to repair the surface cracks of the material to be repaired, wherein the repair liquid is a mixed solution of an alkaline solution and an antioxidant solution, the alkaline solution is one or more of a sodium hydroxide solution, a potassium hydroxide solution, a sodium carbonate solution or a sodium bicarbonate solution, and the antioxidant solution is one or more of a sodium thiosulfate solution, a vitamin C solution, a sodium D-isoascorbate solution, an oxalic acid solution, a potassium borohydride solution, a sodium borohydride solution or an ethanol solution;
[0011] Step S5, adding a mixed solution of an ammonia solution and an ammonium sulfate solution into the reactor to perform secondary surface crack repair on the material to be repaired.
[0012] Furthermore, the chemical formula of the positive electrode material precursor in step S1 is Ni x Co y Mn 1-x-y M z (OH)2, wherein M is a doping element, M is selected from one or more of Ca, Mg, Zn, Co, Cu, Ti, Al, Sn, Zr, Mn, B, Sr, V, Cr, La, Yb, Ce or Ac, 0<x≤0.9, 0<y≤0.9, 0≤z≤0.9.
[0013] Furthermore, the inert protective gas in step S2 is one or more of nitrogen, helium or argon.
[0014] Furthermore, in step S3, the rotation speed of the reactor is reduced to 80-150 rpm based on the original rotation speed of the reactor.
[0015] Furthermore, in step S4, the feeding ratio of the repair liquid to the material to be repaired is 1~4mL:1L; the concentration of the alkaline solution in the repair liquid is 8~10mol / L; the concentration of the antioxidant in the repair liquid is 3~5mol / L; the volume percentage of the alkaline solution in the repair liquid is 20%~80%, and the remainder is the antioxidant.
[0016] Furthermore, in step S5, the volume percentage of the ammonia solution in the mixed solution of the ammonia solution and the ammonium sulfate solution is 10% to 30%, and the remainder is the ammonium sulfate solution; the concentration of the ammonia solution is 8 to 12 mol / L, and the concentration of the ammonium sulfate solution is 1 to 3 mol / L.
[0017] Furthermore, the cathode material precursor for the secondary surface crack repair in step S5 has a D50 of 4-20 μm, a particle size distribution of (D90-D10) / D50<0.70, and a tap density of >1.80 g / cm 3 , with a specific surface area of 5-15m 2 / g, porosity is 10%-60%.
[0018] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0019] 1. During the reaction of the cathode material precursor of the present invention, when ball cracking is found, there is no need to adjust the process conditions to improve the ball cracking. Instead, the feed is stopped after the reaction reaches the target particle size, and then nitrogen protection, lowering the speed of the reactor, increasing the temperature of the reactor, adding a repair liquid and a mixed solution of an ammonia solution and an ammonium sulfate solution, etc. are adopted to thoroughly repair the cracks on the surface of the cathode material precursor sphere.
[0020] 2. The addition of repair liquid in the process of surface crack repair of the present invention can make the hydroxide ions in the repair liquid enter the gap between the positive electrode material precursor spheres, and combine with the residual metal ions attached to the surface of the positive electrode material precursor spheres, so that the surface of the positive electrode material precursor spheres is tightly combined, thereby achieving the purpose of repairing the surface cracks of the positive electrode material precursor. The addition of antioxidant solution can effectively avoid the oxidation of the positive electrode material precursor and the change of performance indicators due to long-term aging, and at the same time can effectively avoid the collapse of the positive electrode material precursor sphere cracking, destroying the original spherical particle morphology of the precursor material, so as to affect the performance of the positive electrode material.
[0021] 3. The addition of a mixed solution of an ammonia solution and an ammonium sulfate solution in the secondary surface crack repair process of the present invention can better complex the residual metal ions and hydroxides in the mother liquor, make the surface of the positive electrode material precursor sphere tighter, better beautify and thoroughly repair the surface cracks of the positive electrode material precursor, and after the secondary surface crack repair process, the surface cracks of the positive electrode material precursor are repaired more thoroughly and perfectly, thereby effectively improving the qualified rate of the positive electrode material precursor.
[0022] 4. The finished product of the cathode material precursor prepared after the final surface crack repair of the present invention: D50 is 4-20 μm, particle size distribution (D90-D10) / D50<0.70, and tap density is>1.80 g / cm 3 , with a specific surface area of 5-15m 2 / g, porosity is 10%-60%. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is the SEM image of the surface of the positive electrode material precursor in Example 1 before repair.
[0024] Figure 2 This is the SEM image of the positive electrode material precursor after surface repair in Example 1.
[0025] Figure 3 This is the SEM image of the positive electrode material precursor before surface repair in Example 2.
[0026] Figure 4 This is the SEM image of the positive electrode material precursor after surface repair in Example 2.
[0027] Figure 5 This is the SEM image of the positive electrode material precursor after surface repair in Comparative Example 1.
[0028] Figure 6 This is the SEM image of the positive electrode material precursor after surface repair in Comparative Example 2.
[0029] Figure 7 This is the SEM image of the positive electrode material precursor after surface repair in Comparative Example 3. DETAILED DESCRIPTION
[0030] The above contents of the present invention are further described in detail below through examples, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples, and all technologies implemented based on the above contents of the present invention belong to the scope of the present invention. Example 1
[0031] This embodiment provides an optimized repair method for cracks in a positive electrode material precursor, wherein the positive electrode material precursor is a nickel-cobalt-manganese hydroxide precursor, wherein the molar ratio of Ni, Co, and Mn is 92:5:3, and the repair method comprises the following steps:
[0032] (1) When the particle size of the cathode material precursor in the reactor reaches D50 of 13 μm (the SEM image of the cathode material precursor before repair is as follows Figure 1 As shown), stop feeding and turn off stirring, turn on nitrogen protection, reduce the stirring speed of the reactor to 120 rpm, and heat the reactor to 65°C;
[0033] (2) adding a repair solution, i.e., a mixed solution of a sodium hydroxide solution and an ascorbic acid solution, into the reactor, wherein the volume ratio of the sodium hydroxide solution to the ascorbic acid solution is 4:1, so that the concentration of hydroxide ions in the mixed system is 0.5 g / L;
[0034] (3) adding 9 mol / L ammonia solution and 3 mol / L ammonium sulfate solution to the reactor, wherein the volume ratio of the ammonia solution to the ammonium sulfate solution is 3:7, so that the concentration of ammonium ions in the mixed system is maintained at an ammonia concentration of 5 g / L under the reaction conditions;
[0035] (4) Crack optimization repair was performed for 32 h at a temperature of 65 °C and a stirring rate of 120 rpm. The repair was stopped after the surface cracks of the cathode material precursor disappeared (the SEM image of the cathode material precursor after repair is shown in Figure 2 as shown).
[0036] Depend on Figure 1 and Figure 2 From the comparison, it can be seen that the surface cracks of the repaired positive electrode material precursor completely disappeared and still maintained a good spherical particle morphology, indicating that the repair method provided in this embodiment has a good crack optimization and repair effect. Example 2
[0037] This embodiment provides an optimized repair method for cracks in a positive electrode material precursor, wherein the positive electrode material precursor is a nickel-cobalt-manganese hydroxide precursor, wherein the molar ratio of Ni, Co, and Mn is 83:5:12, and the repair method comprises the following steps:
[0038] (1) When the particle size of the cathode material precursor in the reactor reaches D50 of 15 μm (the SEM image of the cathode material precursor before repair is as follows Figure 3 As shown), stop feeding and turn off stirring, turn on nitrogen protection, reduce the stirring speed of the reactor to 120 rpm, and heat the reactor to 65°C;
[0039] (2) adding a repair solution, i.e., a mixed solution of a sodium hydroxide solution and an ascorbic acid solution, into the reactor, wherein the volume ratio of the sodium hydroxide solution to the ascorbic acid solution is 4:1, so that the concentration of hydroxide ions in the mixed system is 0.5 g / L;
[0040] (3) adding 9 mol / L ammonia solution and 3 mol / L ammonium sulfate solution to the reactor, wherein the volume ratio of the ammonia solution to the ammonium sulfate solution is 3:7, so that the concentration of ammonium ions in the mixed system is maintained at an ammonia concentration of 5 g / L under the reaction conditions;
[0041] (4) Crack optimization repair was performed for 32 h at a temperature of 65 °C and a stirring rate of 120 rpm. The repair was stopped after the surface cracks of the cathode material precursor disappeared (the SEM image of the cathode material precursor after repair is shown in Figure 4 as shown).
[0042] Depend on Figure 3 and Figure 4 From the comparison, it can be seen that the surface cracks of the repaired positive electrode material precursor completely disappear and still maintain a good spherical particle morphology, indicating that the repair method provided in this embodiment has a good crack optimization and repair effect.
[0043] Comparative Example 1
[0044] This embodiment provides an optimized repair method for cracks in a positive electrode material precursor, wherein the positive electrode material precursor is a nickel-cobalt-manganese hydroxide precursor, and the molar ratio of Ni, Co and Mn is 92:5:3. The repair method comprises the following steps:
[0045] (1) When the particle size of the cathode material precursor in the reactor reaches D50 of 13 μm (the SEM image of the cathode material precursor before repair is as follows Figure 1 As shown), stop feeding and turn off stirring, turn on nitrogen protection, reduce the stirring speed of the reactor to 120 rpm, and heat the reactor to 65°C;
[0046] (2) Add 9 mol / L ammonia solution to the reactor to keep the concentration of ammonium ions in the mixed system at 5 g / L, which is the ammonia concentration under the reaction conditions;
[0047] (3) After crack optimization repair for 32 h at a temperature of 65 °C and a stirring rate of 120 rpm, cracks still appeared on the surface of the cathode material precursor (the SEM image of the cathode material precursor after repair is shown in Figure 2). Figure 5 as shown).
[0048] Depend on Figure 1 and Figure 5From the comparison, it can be seen that in the case of no alkaline solution added, the surface crack repair ratio of the positive electrode material precursor decreased and still maintained a good spherical particle morphology, but some particles still had surface cracks and the repair effect was relatively poor, indicating that the surface crack repair method of the positive electrode material precursor in this comparative example is invalid.
[0049] Comparative Example 2
[0050] This embodiment provides an optimized repair method for cracks in a positive electrode material precursor, wherein the positive electrode material precursor is a nickel-cobalt-manganese hydroxide precursor, and the molar ratio of Ni, Co and Mn is 92:5:3. The repair method comprises the following steps:
[0051] (1) When the particle size of the cathode material precursor in the reactor reaches D50 of 13 μm (the SEM image of the cathode material precursor before repair is as follows Figure 1 As shown), stop feeding and turn off stirring, turn on nitrogen protection, reduce the stirring speed of the reactor to 120 rpm, and heat the reactor to 65°C;
[0052] (2) adding a repair solution, i.e., a mixed solution of a sodium hydroxide solution and an ascorbic acid solution, into the reactor, wherein the volume ratio of the sodium hydroxide solution to the ascorbic acid solution is 4:1, so that the concentration of hydroxide ions in the mixed system is 0.5 g / L;
[0053] (3) After crack optimization repair for 32 h at a temperature of 65 °C and a stirring rate of 120 rpm, cracks still appeared on the surface of the cathode material precursor (the SEM image of the cathode material precursor after repair is shown in Figure 2). Figure 6 as shown).
[0054] Depend on Figure 1 and Figure 6 From the comparison, it can be seen that when the mixed solution of ammonia solution and ammonium sulfate solution is not added for secondary surface crack repair, the surface crack repair ratio of the positive electrode material precursor decreases and still maintains a good spherical particle morphology, but some particles still have surface cracks and the repair effect is relatively poor, indicating that the surface crack repair method of the positive electrode material precursor in this comparative example cannot completely achieve the complete repair of the surface cracks of the positive electrode material precursor.
[0055] Comparative Example 3
[0056] This embodiment provides an optimized repair method for cracks in a positive electrode material precursor, wherein the positive electrode material precursor is a nickel-cobalt-manganese hydroxide precursor, and the molar ratio of Ni, Co and Mn is 92:5:3. The repair method comprises the following steps:
[0057] (1) When the particle size of the cathode material precursor in the reactor reaches D50 of 13 μm (the SEM image of the cathode material precursor before repair is as follows Figure 1As shown), stop feeding and turn off stirring, turn on nitrogen protection, reduce the stirring speed of the reactor to 120 rpm, and heat the reactor to 65°C;
[0058] (2) adding sodium hydroxide solution to the reaction kettle so that the concentration of hydroxide ions in the mixed system is 0.5 g / L;
[0059] (3) adding 9 mol / L ammonia solution and 3 mol / L ammonium sulfate solution to the reactor, wherein the volume ratio of the ammonia solution to the ammonium sulfate solution is 3:7, so that the concentration of ammonium ions in the mixed system is maintained at an ammonia concentration of 5 g / L under the reaction conditions;
[0060] (4) Crack optimization repair was performed for 32 hours at a temperature of 65°C and a stirring rate of 120 rpm. The surface of some cathode material precursors collapsed and cracked, and some cathode material precursors still had cracks on their surfaces (the SEM image of the cathode material precursor after repair is shown in Figure 2). Figure 7 as shown).
[0061] Depend on Figure 1 and Figure 7 It can be seen from the comparison that when no antioxidant solution is added during the first surface crack repair process, the surface crack repair ratio of the cathode material precursor decreases, some particles still have surface cracks, and the surface of some cathode material precursor particles collapses and cracks, losing their original spherical particle morphology.
[0062] The above embodiments describe the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for illustrating the principles of the present invention. Without departing from the scope of the principles of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of protection of the present invention.
Claims
1. An optimized repair method for surface cracks of a cathode material precursor, characterized in that The specific steps are: Step S1, in the process of preparing the positive electrode material precursor by coprecipitation reaction, when the particle size of the positive electrode material precursor reaches the target particle size, the reaction is finished, and the material in the reactor is the material to be repaired; Step S2, introducing an inert protective gas into the reactor so that the oxygen content in the reactor is less than 1.5%; Step S3, reducing the speed of the reactor and increasing the temperature of the reactor to 55-85° C.; Step S4, adding a repair liquid into the reactor to repair the surface cracks of the material to be repaired, wherein the repair liquid is a mixed solution of an alkaline solution and an antioxidant solution, the alkaline solution is one or more of a sodium hydroxide solution, a potassium hydroxide solution, a sodium carbonate solution or a sodium bicarbonate solution, and the antioxidant solution is one or more of a sodium thiosulfate solution, a vitamin C solution, a sodium D-isoascorbate solution, an oxalic acid solution, a potassium borohydride solution, a sodium borohydride solution or an ethanol solution; Step S5, adding a mixed solution of an ammonia solution and an ammonium sulfate solution into the reactor to perform secondary surface crack repair on the material to be repaired.
2. The method for optimizing and repairing surface cracks of a cathode material precursor according to claim 1, characterized in that: The chemical formula of the positive electrode material precursor in step S1 is Ni x Co y Mn 1-x-y M z (OH)2, wherein M is a doping element, M is selected from one or more of Ca, Mg, Zn, Co, Cu, Ti, Al, Sn, Zr, Mn, B, Sr, V, Cr, La, Yb, Ce or Ac, 0<x≤0.9, 0<y≤0.9, 0≤z≤0.
9.
3. The method for optimizing and repairing surface cracks of a cathode material precursor according to claim 1, characterized in that: The inert protective gas in step S2 is one or more of nitrogen, helium or argon.
4. The method for optimizing and repairing surface cracks of a cathode material precursor according to claim 1, characterized in that: In step S3, the rotation speed of the reactor is reduced to 80-150 rpm based on the original rotation speed of the reactor.
5. The method for optimizing and repairing surface cracks of a cathode material precursor according to claim 1, characterized in that: In step S4, the feeding ratio of the repair liquid to the material to be repaired is 1~4mL:1L; the concentration of the alkaline solution in the repair liquid is 8~10mol / L; the concentration of the antioxidant in the repair liquid is 3~5mol / L; the volume percentage of the alkaline solution in the repair liquid is 20%~80%, and the remainder is the antioxidant.
6. The method for optimizing and repairing surface cracks of a cathode material precursor according to claim 1, characterized in that: In step S5, the volume percentage of the ammonia solution in the mixed solution of the ammonia solution and the ammonium sulfate solution is 10% to 30%, and the remainder is the ammonium sulfate solution; the concentration of the ammonia solution is 8 to 12 mol / L, and the concentration of the ammonium sulfate solution is 1 to 3 mol / L.
7. The method for optimizing and repairing surface cracks of a cathode material precursor according to claim 1, characterized in that: The cathode material precursor for secondary surface crack repair in step S5 has a D50 of 4-20 μm, a particle size distribution of (D90-D10) / D50<0.70, and a tap density of >1.80 g / cm 3 , with a specific surface area of 5-15m 2 / g, porosity is 10%-60%.
Citation Information
Patent Citations
Method for repairing cracks of positive electrode material precursor
CN116789190A
Ternary positive electrode material precursor and preparation method thereof
CN116062803A
Regeneration and repair method of waste lithium cobalt oxide positive electrode material
CN116364909A