A production protection method, production system and application thereof suitable for large-diameter glass tubes

By coating large-diameter glass tubes with polytetrafluoroethylene and vinyl trichlorosilane solutions and silica sol, and immersing them in silicone polymers to form a protective film, the problems of large volatilization of the spray liquid and insufficient high-temperature stability are solved. problem, achieving a combination of high light transmittance and wear resistance, reducing environmental pollution.

CN118652047BActive Publication Date: 2024-10-18HUNAN KIBING PHARMACEUTICAL MATERIAL TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411120767.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-10-18
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

The temperature in the spraying area of ​​large-diameter glass tubes is high, and the spray liquid volatilizes greatly, resulting in insufficient high-temperature stability. It is necessary to increase the concentration of the spray liquid to ensure the adhesion rate, but this leads to environmental pollution and a decrease in transmittance.

Method used

Use polytetrafluoroethylene and vinyl trichlorosilane to dissolve in carbon tetrachloride to form a solution, apply it evenly on the substrate, and dry it at 150 degrees Celsius. After coating the silica sol, it is immersed in the silicone polymer and dried. Dry to form a finished protective film and wrap it around the glass tube, using a mass ratio of polysiloxane and polysilazane of 1:1 to improve wear resistance and high temperature stability.

Benefits of technology

The prepared protective film has good light transmittance and wear resistance, can stably adhere to the glass surface at high temperatures, reduce diffuse reflection, increase light transmittance, and effectively make up for the lack of wear resistance of polysilazane. At the same time Ensure high temperature stability and transmittance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the field of glass manufacturing, and in particular to a production protection method, production system and application thereof suitable for large-diameter glass tubes, in order to solve the problems in the prior art that the spraying area temperature of large-diameter glass tubes is high, the volatilization amount of the spraying liquid is large, and the high-temperature stability is insufficient. In order to ensure the adhesion rate, the concentration of the spraying liquid is usually increased, resulting in environmental pollution problems. The method comprises the following steps: dissolving polytetrafluoroethylene and vinyl trichlorosilane in carbon tetrachloride, uniformly coating the prepared solution on the surface of the substrate, and drying it at 150 degrees Celsius; coating the substrate with silica sol; immersing the substrate coated with silica sol into an organosilicon polymer, drying and drying to form a finished protective film; and winding the finished protective film online on the outside of the glass tube. This scheme can avoid production environmental pollution and ensure high-temperature stability, wear resistance and transmittance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of glass manufacturing, and in particular to a production protection method and a production system suitable for large-diameter glass tubes and applications thereof. Background Art

[0002] The glass tube needs to be sprayed before rough cutting. Since the diameter of the glass tube is relatively large (6mm-50mm), the temperature of the rough cutting position of the small diameter glass tube is relatively high and relatively low. Correspondingly, before rough cutting, the temperature of the spraying position of the large diameter glass tube is relatively high than that of the small diameter glass tube. The existing spraying method is to use Tween 80 and water to prepare a solution for spraying. After the spraying liquid is sprayed, the water is dried to form a Tween 80 protective layer on the surface of the glass tube to reduce scratches on the surface of the glass tube during transportation.

[0003] Tween 80 is a surfactant with certain chemical activity, which has adverse effects on human health and the environment. The existing spraying method, because it is an online spraying method, still has the problem of uneven spraying, and the uneven spraying leads to the risk of wear in the unsprayed areas. In addition, the existing method of using water evaporation to leave Tween 80 to form a protective film, because the evaporation of water will cause many pores, and in order to increase the distribution area of ​​Tween 80, it can only be achieved by increasing the concentration of Tween 80, but the concentration of Tween 80 is too high, which will not only affect the production environment, but also affect the transmittance of the glass.

[0004] As mentioned above, the temperature in the spraying area of ​​a large-diameter glass tube is relatively high, the volatilization of the spraying liquid is large, and the high-temperature stability is insufficient. In order to ensure the adhesion rate, the concentration of the spraying liquid is usually increased, which leads to more environmental pollution problems. Summary of the invention

[0005] The present invention discloses a production protection method, a production system and an application thereof suitable for large-diameter glass tubes, in order to solve the problems mentioned in the background technology, that is, the temperature in the spraying area of ​​the large-diameter glass tube is relatively high, the volatilization amount of the spraying liquid is relatively large, the high-temperature stability is insufficient, and in order to ensure the adhesion rate, the concentration of the spraying liquid is usually increased, which leads to more environmental pollution problems.

[0006] The solution of the present invention is:

[0007] A production protection method suitable for large-diameter glass tubes comprises the following steps:

[0008] Dissolving polytetrafluoroethylene and vinyl trichlorosilane in carbon tetrachloride, coating the prepared solution evenly on the surface of the substrate, and drying at 150 degrees Celsius;

[0009] coating a silica sol on a substrate;

[0010] The substrate coated with silica sol is immersed in the organic silicon polymer, and dried to form a finished protective film;

[0011] The finished protective film is wound online around the glass tube.

[0012] Furthermore,

[0013] The mass ratio of the polytetrafluoroethylene to vinyltrichlorosilane is 1:1.

[0014] Furthermore,

[0015] Preparation method of silica sol: dissolve sodium silicate in deionized water, and stir to completely dissolve it to form silica sol.

[0016] Furthermore,

[0017] The silicone polymer includes polysiloxane and / or polysilazane.

[0018] Furthermore,

[0019] The mass ratio of polysiloxane to polysilazane is 1:1.

[0020] Furthermore,

[0021] The substrate coated with silica sol was immersed in the organosilicon polymer for 10-20 seconds.

[0022] Furthermore,

[0023] The substrate coated with the silica sol was lifted up and then heat treated at 120° C. for 30 minutes.

[0024] Furthermore,

[0025] After the glass tube is drawn out of the muffle furnace, when the temperature drops to 280-320 degrees Celsius, the finished protective film is wrapped around the outer surface of the glass tube.

[0026] A glass tube production system adopts the above-mentioned glass tube production protection method.

[0027] An application of the above-mentioned glass tube production protection method.

[0028] The effect analysis is as follows:

[0029] This scheme first dissolves polytetrafluoroethylene and vinyl trichlorosilane in carbon tetrachloride, uniformly coats the prepared solution on the surface of the substrate, and dries it at 150 degrees Celsius to form a base layer, then dissolves sodium silicate in deionized water, fully stirs it to form a silica sol, and coats the silica sol on the substrate; immerses the substrate coated with the silica sol into an organosilicon polymer, dries it to form a finished protective film; and winds the finished protective film online around the outside of a glass tube.

[0030] The decomposition temperature of polytetrafluoroethylene is 327-350 degrees Celsius, and the decomposition temperature of vinyltrichlorosilane is 300-350 degrees Celsius. Therefore, polytetrafluoroethylene and vinyltrichlorosilane will not decompose when they are wrapped around the high-temperature glass tube.

[0031] Silica gel is coated on the substrate. The glass surface treated with silica sol has a higher content of silanol and more reaction sites, which leads to good compatibility and better grafting efficiency of the polymer on the silica sol coating. After the silica sol is coated, the nano-defects on the glass are filled and become flat, reducing the diffuse reflection of the glass surface. The fully hydrophobic surface prepared by this method can adhere well to the glass surface and has good light transmittance, while filling the defects on the substrate surface and improving the light transmittance.

[0032] The substrate coated with silica sol is immersed in the organosilicon polymer, and the polysiloxane forms a wear-resistant polysiloxane hydrophobic surface on the surface of the silica sol. The organosilicon polymer and the silica sol are bonded by chemical bonds, and the prepared fully hydrophobic surface has good stability. Polysilazane has high temperature stability, but its wear resistance is usually insufficient. In this scheme, the mass ratio of polysiloxane to polysilazane is 1:1, and it cooperates with the base layer to obtain the best synergistic effect, which not only effectively compensates for the problem of insufficient wear resistance of polysilazane, but also ensures high temperature stability, and can retain the fully hydrophobic surface and ensure transmittance. DETAILED DESCRIPTION

[0033] Testing and Characterization

[0034] The transmittance test was conducted according to GB / T 2410-2008, and the abrasion resistance test was conducted according to ASTM F735. The abrasion resistance test was that the haze increased after 200 strokes of quartz sand. The wettability was tested by microscopic images of its water contact angle.

[0035] Example 1

[0036] Dissolve polytetrafluoroethylene and vinyl trichlorosilane in carbon tetrachloride at a mass ratio of 1:1, evenly coat the prepared solution on the surface of the substrate, and dry it at 150 degrees Celsius; dissolve sodium silicate in deionized water, stir it thoroughly to form silica sol, and coat the substrate with silica sol; immerse the substrate coated with silica sol in polysiloxane, dry it and form a finished protective film; wrap the finished protective film online on the outside of the glass tube. The temperature of the glass tube is between 280-320, and the wear resistance, wettability and transmittance are measured after cooling.

[0037] Example 2

[0038] Dissolve polytetrafluoroethylene and vinyl trichlorosilane in carbon tetrachloride at a mass ratio of 1:1, evenly coat the prepared solution on the surface of the substrate, and dry it at 150 degrees Celsius; dissolve sodium silicate in deionized water, stir it thoroughly to form silica sol, and coat the substrate with silica sol; immerse the substrate coated with silica sol in polysilazane, dry it and form a finished protective film; wrap the finished protective film online on the outside of the glass tube. The temperature of the glass tube is between 280-320, and the wear resistance, wettability and transmittance are measured after cooling.

[0039] Example 3

[0040] Dissolve polytetrafluoroethylene and vinyl trichlorosilane in carbon tetrachloride at a mass ratio of 1:1, evenly coat the prepared solution on the surface of the substrate, and dry it at 150 degrees Celsius; dissolve sodium silicate in deionized water, stir it thoroughly to form silica sol, and coat the substrate with silica sol; immerse the substrate coated with silica sol in a mixture of polysiloxane and polysilazane, wherein the mass ratio of polysiloxane to polysilazane is 1:1. After drying, a finished protective film is formed; the finished protective film is wound online on the outside of the glass tube. The temperature of the glass tube is between 280-320 degrees Celsius, and the wear resistance, wettability and transmittance are measured after cooling.

[0041] Comparative Example 1

[0042] Tween 80 and water are mixed in a ratio of 1:10 to form a mixture, which is evenly coated on the surface of the substrate and dried at 150 degrees Celsius; sodium silicate is dissolved in deionized water, stirred thoroughly to form silica sol, and the silica sol is coated on the substrate; the substrate coated with silica sol is immersed in a mixture of polysiloxane and polysilazane, wherein the mass ratio of polysiloxane to polysilazane is 1:1. After drying, a finished protective film is formed; the finished protective film is wound online on the outside of the glass tube. The temperature of the glass tube is between 280-320 degrees Celsius, and the wear resistance, wettability and transmittance are measured after cooling.

[0043] Comparative Example 2

[0044] Tween 80 and water were mixed in a ratio of 1:10 to form a mixture, which was sprayed on the outside of a glass tube at 280-320 degrees Celsius. The glass tube, which was then cooled to room temperature, was then tested for wear resistance, wettability and transmittance.

[0045] Results and Discussion:

[0046]

[0047] This scheme first dissolves polytetrafluoroethylene and vinyl trichlorosilane in carbon tetrachloride, uniformly coats the prepared solution on the surface of the substrate, and dries it at 150 degrees Celsius to form a base layer, then dissolves sodium silicate in deionized water, fully stirs it to form a silica sol, and coats the silica sol on the substrate; immerses the substrate coated with the silica sol into an organosilicon polymer, dries it to form a finished protective film; and winds the finished protective film online around the outside of a glass tube.

[0048] The decomposition temperature of polytetrafluoroethylene is 327-350 degrees Celsius, and the decomposition temperature of vinyl trichlorosilane is 300-350 degrees Celsius. Therefore, polytetrafluoroethylene and vinyl trichlorosilane will not decompose when they are wrapped around the outside of the high-temperature glass tube. Silica gel is coated on the substrate. The glass surface treated with silica sol has a higher content of silanol and more reaction sites, resulting in good compatibility and better grafting efficiency of the polymer on the silica sol coating. After coating with silica sol, the nano-defects on the glass are filled and become flat, reducing the diffuse reflection of the glass surface. The fully hydrophobic surface prepared by this method can adhere well to the glass surface and has good light transmittance, while filling the defects on the surface of the substrate and improving the light transmittance.

[0049] The substrate coated with silica sol is immersed in the organosilicon polymer, and the polysiloxane forms a wear-resistant polysiloxane hydrophobic surface on the surface of the silica sol. The organosilicon polymer and the silica sol are bonded by chemical bonds, and the prepared fully hydrophobic surface has good stability. Polysilazane has high temperature stability, but its wear resistance is usually insufficient. In this scheme, the mass ratio of polysiloxane to polysilazane is 1:1, and it cooperates with the polytetrafluoroethylene and vinyl trichlorosilane of the base layer to obtain the best synergistic effect, which not only effectively compensates for the problem of insufficient wear resistance of polysilazane, but also ensures high temperature stability, and can retain the fully hydrophobic surface and ensure transmittance.

[0050] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A production protection method suitable for large diameter glass tubes, characterized in that: The steps include: Dissolving polytetrafluoroethylene and vinyl trichlorosilane in carbon tetrachloride, coating the prepared solution evenly on the surface of the substrate, and drying at 150 degrees Celsius; Coating silica sol on the substrate; Preparation method of silica sol: dissolving sodium silicate in deionized water, stirring to completely dissolve it to form silica sol; The substrate coated with silica sol is immersed in an organic silicon polymer, and dried to form a finished protective film; the organic silicon polymer includes: polysiloxane and / or polysilazane; The finished protective film is wound online around the glass tube.

2. The production protection method for large diameter glass tubes according to claim 1, characterized in that: The mass ratio of the polytetrafluoroethylene to vinyltrichlorosilane is 1:

1.

3. The production protection method for large diameter glass tubes according to claim 2, characterized in that: The mass ratio of polysiloxane to polysilazane is 1:

1.

4. The production protection method for large diameter glass tubes according to claim 1, characterized in that: The substrate coated with silica sol was immersed in the organosilicon polymer for 10-20 seconds.

5. The production protection method for large diameter glass tubes according to claim 1, characterized in that: The substrate coated with the silica sol was lifted up and then heat treated at 120° C. for 30 minutes.

6. The production protection method for large diameter glass tubes according to claim 1, characterized in that: After the glass tube is drawn out of the muffle furnace, when the temperature drops to 280-320 degrees Celsius, the finished protective film is wrapped around the outer surface of the glass tube.

7. A glass tube production system, characterized in that: The production protection method suitable for large-diameter glass tubes as described in any one of claims 1 to 6 is adopted.

8. An application of the production protection method for large-diameter glass tubes as claimed in any one of claims 1 to 6.

Citation Information

Patent Citations

  • Strengthening treatment method for glass tube in on-line production process

    CN102219392A

  • Preparation method of SiO2 / polytetrafluoroethylene hybridized super-hydrophobic coating