A wear-resistant boron nitride / silicon nitride self-lubricating composite material and preparation method thereof

A three-dimensional continuous boron nitride/silicon nitride composite with spherical boron nitride particles addresses wear resistance issues, providing improved tribological properties for extreme conditions.

CN118652124BActive Publication Date: 2024-12-03NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411154661.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-12-03
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

Boron nitride addition to silicon nitride composites reduces wear resistance, limiting their application in harsh environments due to high temperature, high pressure, and high-speed conditions.

Method used

A three-dimensional continuous structure is designed by adding spherical boron nitride particles to silicon nitride, forming a boron nitride/silicon nitride composite with improved tribological properties through a specific preparation method involving wet ball milling, granulation, and hot pressing sintering.

Benefits of technology

The composite material exhibits enhanced wear resistance and lubricity at high temperatures, making it suitable for structural and wear-resistant parts in extreme conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118652124B_ABST
    Figure CN118652124B_ABST
Patent Text Reader

Abstract

The present invention discloses a wear-resistant boron nitride / silicon nitride self-lubricating composite material and a preparation method thereof, and belongs to the technical field of self-lubricating ceramic-based composite materials. The present invention is based on the structural / functional integrated design principle of composite materials, and by adding spherical boron nitride into a silicon nitride matrix, a boron nitride / silicon nitride self-lubricating composite material with a three-dimensional continuous structure is designed and constructed. Compared with general boron nitride / silicon nitride self-lubricating composite materials, the wear resistance of the material at different temperatures is significantly improved, which helps boron nitride / silicon nitride self-lubricating composite materials become important candidate materials for structural parts and wear-resistant functional parts, and provides technical support for exploring the industrial application of solid self-lubricating materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of self-lubricating ceramic-based composite materials, and relates to a wear-resistant boron nitride / silicon nitride self-lubricating composite material and a preparation method thereof. Background Art

[0002] Tribology includes three parts: friction, wear and lubrication. According to statistics, the energy consumed by wear in the world accounts for about 30% of the total energy each year, and the equipment damage caused by friction failure not only reduces production efficiency but also causes large asset losses. In addition, the working conditions of bearings and bushings of space satellites, sliding seal components of hypersonic aircraft, and key sliding bushings used to adjust the working mode in power systems are more severe, involving high temperature, high pressure, high speed, vibration shock, special gases and other harsh environments. Boron nitride / silicon nitride composites, as a classic self-lubricating composite material, are widely used in sealing components, engine components and high-speed cutting tools because silicon nitride ceramics themselves have the advantages of high hardness, low thermal expansion and excellent chemical stability in a wide temperature range. In addition, adding solid lubricant materials, especially boron nitride materials, to silicon nitride ceramics is an effective way to achieve high-temperature self-lubrication, because hexagonal boron nitride (h-BN) has a hexagonal lamellar structure with good lubricity, as well as a high thermal decomposition temperature and thermal shock resistance. However, the introduction of boron nitride will significantly reduce the wear resistance of silicon nitride materials, restricting the production and application of this material. Summary of the invention

[0003] In order to address the deficiencies of the above-mentioned prior art, the present invention provides a wear-resistant boron nitride / silicon nitride self-lubricating composite material and a preparation method thereof. A three-dimensional continuous structure is designed based on the structural and functional integration design concept of the composite material. Nano-boron nitride is granulated to form spherical boron nitride particles, and the spherical boron nitride is added to the silicon nitride material to form a boron nitride / silicon nitride composite material with a three-dimensional continuous structure, thereby significantly improving the high-temperature tribological properties of the material and providing technical support for exploring the industrial application of solid self-lubricating materials.

[0004] The preparation method of the wear-resistant boron nitride / silicon nitride self-lubricating composite material of the present invention comprises the following steps:

[0005] (1) Nano silicon nitride (α-Si3N4) powder, nano yttrium oxide and aluminum oxide powder are mixed uniformly by wet ball milling to obtain mixed silicon nitride powder. Nano α-Si3N4 powder, nano yttrium oxide and aluminum oxide powder are mixed uniformly by wet ball milling at a mass ratio of 90:6:4.

[0006] The purity of nano-α-Si3N4 powder, nano-yttrium oxide, aluminum oxide powder and nano-boron nitride powder is ≥99%, and the particle size is 0.2~1 μm.

[0007] (2) Granulating the nano-boron nitride powder to form spherical boron nitride powder, dripping polyvinyl alcohol solution into the spherical boron nitride powder, adding α-Si3N4 powder, so that the surface of the spherical boron nitride powder is coated with a layer of nano-silicon nitride powder; adding the spherical boron nitride powder coated with nano-silicon nitride powder to the mixed silicon nitride powder after drying and sieving, wet ball milling and mixing to make it uniform, and drying and sieving the mixed powder.

[0008] The particle size of the spherical boron nitride powder is in the range of 10 to 130 μm, which is denoted as xSBN (x is the average particle size). The volume fraction of the spherical boron nitride powder coated with silicon nitride powder is 20 to 40% of the mixed silicon nitride powder.

[0009] During the drying process of the mixed powder, the air pressure is preferably reduced to 90 mbar at 40 °C and 30 r / min for rotary evaporation, and then the powder is transferred to a vacuum drying oven and thoroughly dried at a constant temperature of 60 °C for 24 hours. The sieving process is to gently grind the dried powder with a mortar and sieve it with a 100-200 mesh sieve to obtain loose powder. A layer of hexagonal boron nitride powder is coated on the inner surface of the graphite mold, and graphite paper is placed between the blank and the graphite pad to facilitate demoulding.

[0010] In steps (1) and (2), the wet ball milling uses anhydrous ethanol as a dispersant, and the mass ratio of the total mass of the powder raw material to the dispersant is 1:1 to 1:3; the ball mill speed during wet ball milling is 100 to 200 r / min, and the ball milling time is 24 to 48 hours. The ball milling time is preferably 30 minutes forward, 30 minutes reverse, 5 minutes down, and a total time of 48 hours. The grinding balls used in wet ball milling are alumina balls, and the mass ratio of the total mass of the powder raw material to the grinding balls is 1:1; the ball mill jar used is made of polytetrafluoroethylene.

[0011] (3) The dried and sieved mixed powder is cold pressed into a green body, which is transferred to a graphite mold and sintered in a hot pressing furnace at 1700-1750°C and 10-15 MPa for 50-60 minutes in a nitrogen atmosphere to obtain a spherical boron nitride / silicon nitride (SBN / Si3N4) self-lubricating composite material.

[0012] During the sintering process, the heating rate below 1550°C is 10°C / min, and the heating rate between 1550°C and 1750°C is 5°C / min. The temperature is kept at this temperature for 50 to 60 minutes. When the temperature rises to 600°C, nitrogen is filled into the hot pressing furnace.

[0013] In the boron nitride / silicon nitride self-lubricating composite material, hexagonal boron nitride is evenly distributed in the silicon nitride matrix in a spherical structure. The self-lubricating composite material exhibits excellent high-temperature tribological properties. The friction coefficient of the 60-micron-sized spherical boron nitride / silicon nitride (60SBN / Si3N4) composite material at 800 ℃ is 0.59, and the wear rate is 0.72×10 -3 mm 3 / (N·m); the friction coefficient at 1200 ℃ is 0.54, and the wear rate is 1.58×10 -3 mm 3 / (N·m).

[0014] In summary, the present invention is based on the structural / functional integrated design principle of composite materials. By adding spherical boron nitride into a silicon nitride matrix, a boron nitride / silicon nitride self-lubricating composite material with a three-dimensional continuous structure is designed and constructed. Compared with general boron nitride / silicon nitride self-lubricating composite materials, the wear resistance of the material at different temperatures is significantly improved, which helps boron nitride / silicon nitride self-lubricating composite materials become an important candidate material for structural parts and wear-resistant functional parts. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The XRD spectra of spherical boron nitride powders of four particle sizes prepared in Example 1, Example 2, Example 3 and Comparative Example 1 of the present invention are shown.

[0016] Figure 2 It is the XRD spectrum of the powders of Example 1, Example 2, Example 3 and Comparative Example 1 of the present invention after being uniformly mixed by ball milling.

[0017] Figure 3 It is the X-ray diffraction (XRD) spectrum of the boron nitride / silicon nitride (BN / Si3N4) self-lubricating composite material prepared in Example 1, Example 2, Example 3 and Comparative Example 1 of the present invention.

[0018] Figure 4 1 is a SEM image (a) and an energy spectrum diagram (a1) of the BN / Si3N4 self-lubricating composite material prepared in Example 1 of the present invention.

[0019] Figure 5 1 and 2 are the SEM image (a) and energy spectrum (a1) of the BN / Si3N4 self-lubricating composite material prepared in Example 2 of the present invention.

[0020] Figure 6 1 and 2 are the SEM image (a) and energy spectrum (a1) of the BN / Si3N4 self-lubricating composite material prepared in Example 3 of the present invention.

[0021] Figure 7The SEM image (a) and energy spectrum (a1) of the BN / Si3N4 self-lubricating composite material prepared in Comparative Example 1 of the present invention.

[0022] Figure 8 It is a microstructure diagram of the SBN / Si3N4 self-lubricating composite material prepared in Example 1 (a), Example 2 (b), and Example 3 (c) of the present invention.

[0023] Fig. 9 This is a graph showing the variation of the friction coefficient of the BN / Si3N4 self-lubricating composite material prepared by the present invention at room temperature with the experimental time.

[0024] Fig.10 This is a graph showing the variation of the friction coefficient of the BN / Si3N4 self-lubricating composite material prepared by the present invention at 400°C with the experimental time.

[0025] Fig.11 This is a graph showing the variation of the friction coefficient of the BN / Si3N4 self-lubricating composite material prepared by the present invention at 800°C with the experimental time.

[0026] Fig.12 The figure is a graph showing the variation of the friction coefficient of the BN / Si3N4 self-lubricating composite material prepared by the present invention at 1200°C with the experimental time.

[0027] Fig.13 It is the wear rate of the BN / Si3N4 self-lubricating composite material prepared by the present invention at room temperature.

[0028] Fig.14 is the wear rate of the BN / Si3N4 self-lubricating composite material prepared by the present invention at 400°C.

[0029] Fig.15 is the wear rate of the BN / Si3N4 self-lubricating composite material prepared by the present invention at 800°C.

[0030] Fig.16 is the wear rate of the BN / Si3N4 self-lubricating composite material prepared by the present invention at 1200°C. DETAILED DESCRIPTION

[0031] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention. Example 1

[0033] A method for preparing a 20-micron-diameter spherical boron nitride / silicon nitride (20SBN / Si3N4) self-lubricating composite material comprises the following steps:

[0034] S1: Spherical boron nitride powder treatment: The nano boron nitride powder is granulated to form a spherical boron nitride powder with a diameter of 20±10μm, 3wt% polyvinyl alcohol solution is dripped into the spherical boron nitride powder, and nano α-Si3N4 powder is added to make the surface of the spherical boron nitride powder covered with a layer of nano silicon nitride powder.

[0035] S2: Preparation of mixed powder: Nano-α-Si3N4 powder, nano-yttrium oxide and alumina powder were placed in a polytetrafluoroethylene ball mill at a mass ratio of 90:6:4, and anhydrous ethanol was used as the dispersion medium. The mass ratio of the original powder (the total mass of nano-α-Si3N4 powder, nano-yttrium oxide and alumina powder), grinding balls and dispersion medium was 1:1:2. The ball mill was placed in a planetary ball mill and milled at a speed of 200 r / min for 24 hours to obtain mixed silicon nitride powder.

[0036] 30 vol% of spherical boron nitride powder coated with nano silicon nitride powder was added to the dried and sieved mixed silicon nitride powder. The mass ratio of the powder (the total mass of the mixed silicon nitride powder and the spherical boron nitride powder coated with nano silicon nitride powder) to the dispersion medium anhydrous ethanol was 1:3. The powder was placed in a ball mill and milled at a speed of 100 r / min for 48 hours to obtain a uniformly mixed powder.

[0037] S3: Hot pressing sintering: The ball-milled slurry was subjected to rotary drying at 40 °C and 30 r / min with the pressure reduced to 90 mbar. The powder was transferred to a vacuum drying oven and dried thoroughly at a constant temperature of 60 °C for 24 h. The loose mixed powder was sieved with a 200-mesh sieve.

[0038] The mixed powder after drying and sieving is loaded into a steel mold and dry pressed at 200 MPa for 3 minutes to form a green body. A layer of boron nitride is coated on the inner wall of the graphite mold to facilitate demoulding. The green body is transferred to the graphite mold. The green body and the graphite pad are separated by graphite paper, and then placed in a hot pressing sintering furnace for sintering. Hot pressing sintering process conditions: The hot pressing furnace is vacuumized, and the vacuum value is <10 1Pa, the axial pressure was 10 MPa, the temperature was increased to 600 ℃ at a heating rate of 10 ℃ / min, the heating was paused and filled with nitrogen atmosphere, then the temperature was increased to 1550 ℃ at a heating rate of 10 ℃ / min, and then to 1750 ℃ ​​at a heating rate of 5 ℃ / min, and kept warm for 60 min. After cooling to room temperature with the furnace, the 20SBN / Si3N4 self-lubricating composite material was obtained.

[0039] Friction performance test method: First, the sintered sample was wire-cut into blocks with a size of 12.5 mm × 10 mm × 4 mm. The sample was polished to a smooth surface with a roughness of 1 μm using diamond sandpaper and ultrasonically cleaned with acetone for 10 min. The tribological properties of the boron nitride / silicon nitride self-lubricating composite material under atmospheric environment at room temperature, 400°C, 800°C and 1200°C were studied using a high-temperature friction and wear tester. The friction test conditions were a frequency of 5 Hz, a stroke of 1 mm, a pressure of 0.5 MPa, and the wear partner was a silicon nitride pin. During the test, the friction coefficient was recorded in real time by the data acquisition software.

[0040] Tribological properties of 20SBN / Si3N4: The wear rate at room temperature is 1.9×10 -4 mm 3 / (N·m), and the wear rate at 400 ℃ is 0.34×10 -3 mm 3 / (N·m), and the wear rate at 800 ℃ is 0.66×10 -3 mm 3 / (N·m), and the wear rate at 1200 ℃ is 2.26×10 -3 mm 3 / (N·m). Example 2

[0041] A method for preparing a 60 micron particle size spherical boron nitride / silicon nitride (60SBN / Si3N4) self-lubricating composite material comprises the following steps:

[0042] S1: Spherical boron nitride powder treatment: The nano boron nitride powder is granulated to form a spherical boron nitride powder with a diameter of 60±10 μm, 3 wt% polyvinyl alcohol solution is dripped into the spherical boron nitride powder, and a layer of nano silicon nitride powder is coated on the surface.

[0043] S2: Preparation of mixed powder: Take nano-α-Si3N4 powder, nano-yttrium oxide and alumina powder, and place them in a polytetrafluoroethylene ball mill at a mass ratio of 90:6:4. The dispersion medium is anhydrous ethanol. The mass ratio of the original powder, grinding ball and dispersion medium is 1:1:2. Place the ball mill in a planetary ball mill and mill at a speed of 200 r / min for 24 hours to obtain a mixed silicon nitride powder. Add 30 vol% of spherical boron nitride powder coated with nano-α-Si3N4 powder to the dried and sieved mixed silicon nitride powder. The mass ratio of the powder and the dispersion medium anhydrous ethanol is 1:3. Put it in a ball mill and mill at a speed of 100 r / min for 48 hours to obtain a uniformly mixed powder.

[0044] S3: Hot pressing sintering: The ball-milled slurry was subjected to rotary drying at 40 °C and 30 r / min with the pressure reduced to 90 mbar. The powder was transferred to a vacuum drying oven and dried thoroughly at a constant temperature of 60 °C for 24 h. The loose mixed powder was sieved with a 200-mesh sieve.

[0045] The mixed powder after drying and sieving is loaded into a steel mold and dry pressed at 200 MPa for 3 minutes to form a green body. A layer of boron nitride is coated on the inner wall of the graphite mold to facilitate demoulding. The green body is transferred to the graphite mold. The green body and the graphite pad are separated by graphite paper, and then placed in a hot pressing sintering furnace for sintering. Hot pressing sintering process conditions: The hot pressing furnace is vacuumized, and the vacuum value is <10 1 Pa, the axial pressure was 10 MPa, the temperature was increased to 600 ℃ at a heating rate of 10 ℃ / min, the heating was paused and filled with nitrogen atmosphere, then the temperature was increased to 1550 ℃ at a heating rate of 10 ℃ / min, and then to 1750 ℃ ​​at a heating rate of 5 ℃ / min, and kept warm for 60 min. After cooling to room temperature with the furnace, a 60SBN / Si3N4 self-lubricating composite material was obtained.

[0046] The friction performance test method is the same as that in Example 1.

[0047] The tribological properties of 60SBN / Si3N4 are as follows: the friction coefficient is 0.61 at room temperature and the wear rate is 0.31×10 -4 mm 3 / (N·m), the friction coefficient at 400 ℃ is 0.56, and the wear rate is 0.66×10 -3 mm 3 / (N·m), the friction coefficient at 800 ℃ is 0.59, and the wear rate is 0.72×10 -3 mm 3 / (N·m), the friction coefficient at 1200 ℃ is 0.54, and the wear rate is 1.58×10 -3 mm 3 / (N·m). Example 3

[0048] A method for preparing a 120 micron particle size spherical boron nitride / silicon nitride (120SBN / Si3N4) self-lubricating composite material comprises the following steps:

[0049] S1: Spherical boron nitride powder treatment: First, the nano boron nitride powder is granulated to form a spherical boron nitride powder with a diameter of 120±10μm, and a 3wt% polyvinyl alcohol solution is dripped into the spherical boron nitride powder to coat a layer of nano silicon nitride powder on the surface.

[0050] S2: Preparation of mixed powder: Take nano-α-Si3N4 powder, nano-yttrium oxide and alumina powder, and place them in a polytetrafluoroethylene ball mill at a mass ratio of 90:6:4. The dispersion medium is anhydrous ethanol. The mass ratio of the original powder, grinding ball and dispersion medium is 1:1:2. Place the ball mill in a planetary ball mill and mill at a speed of 200 r / min for 24 hours to obtain a mixed silicon nitride powder. Add 30 vol% of spherical boron nitride powder coated with nano-α-Si3N4 powder to the dried and sieved silicon nitride powder. The mass ratio of the powder and the dispersion medium anhydrous ethanol is 1:3. Put it in a ball mill and mill at a speed of 100 r / min for 48 hours to obtain a uniformly mixed powder.

[0051] S3: Hot pressing sintering: The ball-milled slurry was subjected to rotary drying at 40 °C and 30 r / min with the pressure reduced to 90 mbar. The powder was transferred to a vacuum drying oven and dried thoroughly at a constant temperature of 60 °C for 24 h. The loose mixed powder was sieved with a 200-mesh sieve.

[0052] The mixed powder after drying and sieving is loaded into a steel mold and dry pressed at 200 MPa for 3 minutes to form a green body. A layer of boron nitride is coated on the inner wall of the graphite mold to facilitate demoulding. The green body is transferred to the graphite mold. The green body and the graphite pad are separated by graphite paper, and then placed in a hot pressing sintering furnace for sintering. Hot pressing sintering process conditions: The hot pressing furnace is vacuumized, and the vacuum value is <10 1 Pa, the axial pressure was 10 MPa, the temperature was increased to 600 ℃ at a heating rate of 10 ℃ / min, the heating was paused and filled with nitrogen atmosphere, then the temperature was increased to 1550 ℃ at a heating rate of 10 ℃ / min, and then to 1750 ℃ ​​at a heating rate of 5 ℃ / min, and kept warm for 60 min. After cooling to room temperature with the furnace, a 120SBN / Si3N4 self-lubricating composite material was obtained.

[0053] The friction performance test method is the same as that in Example 1.

[0054] Tribological properties of 120SBN / Si3N4: The wear rate at room temperature is 1.3×10 -4 mm3 / (N·m), the wear rate at 400 ℃ is 0.53×10 -3 mm 3 / (N·m), and the wear rate at 800 ℃ is 1.17×10 -3 mm 3 / (N·m), the wear rate at 1200℃ is 1.86×10 -3 mm 3 / (N·m).

[0055] Comparative Example 1

[0056] A method for preparing a nano boron nitride / silicon nitride (nBN / Si3N4) self-lubricating composite material comprises the following steps:

[0057] S1: Preparation of mixed powder: Nano-α-Si3N4 powder, nano-yttrium oxide and alumina powder were placed in a polytetrafluoroethylene ball mill at a mass ratio of 90:6:4. The dispersion medium was anhydrous ethanol. The mass ratio of the original powder, grinding ball and dispersion medium was 1:1:2. The ball mill was placed in a planetary ball mill and milled at a speed of 200 r / min for 24 hours to obtain a mixed silicon nitride powder. 30 vol% of nano-boron nitride powder was added to the dried and sieved silicon nitride powder. The mass ratio of the powder to the dispersion medium was 1:3. The powder was placed in a ball mill and milled at a speed of 100 r / min for 48 hours to obtain a uniformly mixed powder.

[0058] S2: Hot pressing sintering: The ball-milled mixed slurry is subjected to rotary drying at 40 °C and 30 r / min and the air pressure is reduced to 90 mbar. The powder is transferred to a vacuum drying oven and thoroughly dried at a constant temperature of 60 °C for 24 h. Use a 200-mesh sieve to obtain a loose mixed powder. Take a certain mass of powder and put it into a steel mold, and dry-press it at 200 MPa for 3 minutes to form a green body. Coat a layer of boron nitride on the inner wall of the graphite mold to facilitate demolding, transfer the green body to the graphite mold, and isolate the green body and the graphite pad with graphite paper, and then put it into a hot pressing sintering furnace for sintering. Hot pressing sintering process conditions: Vacuum the hot pressing furnace, and the vacuum value is <10 1 Pa, the axial pressure was 10 MPa, the temperature was increased to 600 ℃ at a heating rate of 10 ℃ / min, the heating was paused and filled with nitrogen atmosphere, then the temperature was increased to 1550 ℃ at a heating rate of 10 ℃ / min, and then to 1750 ℃ ​​at a heating rate of 5 ℃ / min, and kept warm for 60 min. After cooling to room temperature with the furnace, the nBN / Si3N4 self-lubricating composite material was obtained.

[0059] The friction performance test method is the same as that in Example 1.

[0060] The tribological properties of nBN / Si3N4 are as follows: the friction coefficient is 0.58 at room temperature and the wear rate is 3.55×10 -4 mm 3 / (N·m), the friction coefficient at 400 ℃ is 0.63, and the wear rate is 6.69×10 -3 mm 3 / (N·m), the average friction coefficient at 800 ℃ is 0.70, and the wear rate is 2.35×10 -3 mm 3 / (N·m), the average friction coefficient at 1200 ℃ is 0.95, and the wear rate is 8.16×10 -3 mm 3 / (N·m).

[0061] Figure 1 The XRD spectra of spherical boron nitride powders of four particle sizes prepared in Example 1, Example 2, Example 3 and Comparative Example 1 of the present invention show that the spherical boron nitride has a hexagonal lamellar structure. Figure 2 It is the XRD spectrum of the powders of Example 1, Example 2, Example 3 and Comparative Example 1 of the present invention after being uniformly mixed by ball milling. Figure 3 The X-ray diffraction (XRD) patterns of the boron nitride / silicon nitride (BN / Si3N4) self-lubricating composite materials prepared in Example 1, Example 2, Example 3 and Comparative Example 1 of the present invention show that silicon nitride (Si3N4) changes from α phase to β phase after sintering. The crystal structure of boron nitride does not change and is still a layered structure with lubricity.

[0062] Figure 4 1 is a SEM image (a) and an energy spectrum diagram (a1) of the BN / Si3N4 self-lubricating composite material prepared in Example 1 of the present invention. Figure 5 1 and 2 are the SEM image (a) and energy spectrum (a1) of the BN / Si3N4 self-lubricating composite material prepared in Example 2 of the present invention. Figure 6 1 and 2 are the SEM image (a) and energy spectrum (a1) of the BN / Si3N4 self-lubricating composite material prepared in Example 3 of the present invention. Figure 7 The SEM image (a) and energy spectrum (a1) of the BN / Si3N4 self-lubricating composite material prepared in Comparative Example 1 of the present invention. Figure 7 (a) shows the uniform distribution of the nano boron nitride flakes in the silicon nitride matrix in the comparative example. The figure shows that the structure of the spherical boron nitride in the example is mostly retained after hot pressing sintering, and the three-dimensional continuous structure is not destroyed after sintering.

[0063] Figure 8The microstructure diagram of the SBN / Si3N4 self-lubricating composite material prepared in Example 1 (a), Example 2 (b), and Example 3 (c) of the present invention shows that the spherical boron nitride spheres are evenly distributed in the silicon nitride matrix, and the relative area is 25-35%.

[0064] Figure 9-12 The figure is a graph showing the variation of the friction coefficient of the BN / Si3N4 self-lubricating composite material prepared by the present invention at room temperature, 400°C, 800°C and 1200°C with the experimental time. The figure shows that during the friction process at room temperature, 400°C and 800°C, the friction coefficients of the four samples are similar and stable. During the friction process at 1200°C, the friction coefficient of the comparative example increases continuously with time to 1.2, while the friction coefficient of the embodiment can still remain stable and is around 0.6.

[0065] Figure 13-16 The wear rates of the BN / Si3N4 self-lubricating composite material prepared by the present invention at room temperature, 400°C, 800°C and 1200°C are shown in the figure. The wear rates of the embodiments at room temperature, 400°C and 800°C are one order of magnitude lower than those of the comparative examples, and the wear rate of the embodiments at 1200°C is also significantly better than that of the comparative examples.

Claims

1. A method for preparing a wear-resistant boron nitride / silicon nitride self-lubricating composite material, It is characterized in that The following steps are involved: (1) Nano-α-Si 3 N 4 The powder, nano yttrium oxide and aluminum oxide powder are mixed uniformly by wet ball milling to obtain mixed silicon nitride powder; (2) Granulate the nano boron nitride powder to form spherical boron nitride powder, drip polyvinyl alcohol solution into the spherical boron nitride powder, and add nano α-Si 3 N 4 Powder, so that the surface of the spherical boron nitride powder is coated with a layer of nano α-Si 3 N 4 Powder; Add coated nano α-Si to the dried and sieved mixed silicon nitride powder 3 N 4 The spherical boron nitride powder is wet-milled and mixed evenly, and the mixed powder is dried and sieved; the particle size of the spherical boron nitride powder is 10-130 μm; (3) cold pressing the dried and sieved mixed powder into a green body, transferring the green body into a graphite mold, and using a hot pressing sintering furnace in a nitrogen atmosphere at 1700-1750°C and 10-15 MPa for 50-60 minutes to obtain a spherical boron nitride / silicon nitride self-lubricating composite material; In the spherical boron nitride / silicon nitride self-lubricating composite material, hexagonal boron nitride is uniformly distributed in a silicon nitride matrix in a spherical structure, and the formed silicon nitride composite material has a three-dimensional continuous structural feature.

2. The method for preparing the wear-resistant boron nitride / silicon nitride self-lubricating composite material according to claim 1, Features: Nano α-Si 3 N 4 The purity of powder, nano yttrium oxide, aluminum oxide powder and nano boron nitride powder is ≥99%, and the particle size is 0.2~1 μm.

3. The method for preparing the wear-resistant boron nitride / silicon nitride self-lubricating composite material according to claim 1, Features: In step (1), nano α-Si 3 N 4 The powder, nano yttrium oxide and aluminum oxide powder are mixed uniformly by wet ball milling in a mass ratio of 90:6:

4.

4. The method for preparing the wear-resistant boron nitride / silicon nitride self-lubricating composite material according to claim 1, Features: In step (2), coating nano α-Si 3 N 4 The volume fraction of the spherical boron nitride powder added to the mixed silicon nitride powder is 20-40%.

5. The method for preparing the wear-resistant boron nitride / silicon nitride self-lubricating composite material according to claim 1, Features: In steps (1) and (2), anhydrous ethanol is used as a dispersant in wet ball milling, and the mass ratio of the total mass of the powder raw material to the dispersant is 1:1 to 1:3; the ball mill speed during wet ball milling is 100 to 200 r / min, and the ball milling time is 24 to 48 h.

6. The method for preparing the wear-resistant boron nitride / silicon nitride self-lubricating composite material according to claim 1, Features: In step (2), the process of drying and sieving the mixed powder is first drying by rotary evaporation at 40°C, 30 r / min and 90 mbar, and then transferring the mixed powder to a vacuum drying oven at a constant temperature of 60°C and thoroughly drying for 24 h; the mesh size of the sieve during sieving is 100-200 mesh.

7. The method for preparing the wear-resistant boron nitride / silicon nitride self-lubricating composite material according to claim 1, Features: In step (3), the hot pressing sintering is firstly to evacuate the hot pressing furnace, and the vacuum value is less than 10 1 Pa, axial pressure of 10 ~ 15MPa, heat to 600 ℃ at a rate of 10 ℃ / min, pause heating and fill with nitrogen atmosphere, then heat to 1550 ℃ at a rate of 10 ℃ / min, heat to 1700 ~ 1750 ℃ ​​at a rate of 5 ℃ / min, keep warm for 50 ~ 60 min, and cool to room temperature with the furnace.