A surface modification method for high temperature resistant silicon carbon rod
By spraying multi-layer structural coating, the problem of oxidation and corrosion of silicon carbon rods in high-temperature environments is solved, and its oxidation resistance, corrosion resistance and high-temperature resistance are improved, and its combination with other materials is enhanced, which extends the service life. and improve heat conduction efficiency.
Patent Information
- Application Number
- CN202411112706.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-14
AI Technical Summary
Silicon carbon rods are susceptible to oxidation and corrosion in high temperature environments, resulting in reduced performance and shortened lifetime. Their surface chemical activity and physical structure have weak binding ability with other materials, affecting the heat conduction efficiency.
Antioxidant coatings are prepared by spray guns evenly spraying hexamethylene diisocyanate, myrtetradecanol, organopolysilazane and molybdenum disilide powder, and high-temperature resistant materials are obtained by sintering hafnium carbide, hafnium nitride and graphite-like carbon nitride , a multi-layer structural coating is formed, coated on the surface of the silicon carbon rod and cross-linked curing treatment.
It significantly improves the oxidation, corrosion and high temperature resistance of silicon carbon rods, forms a dense protective film and an oxygen-insulating layer, extends the service life of silicon carbon rods and improves the heat conduction efficiency.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of silicon carbon rod modification, and particularly relates to a surface modification method of a high temperature resistant silicon carbon rod. Background Art
[0002] As a high-performance heating element, silicon carbon rods are widely used in many fields such as electric heating industry, chemical industry, steel, etc. However, with the development of modern industrial technology, the performance requirements for silicon carbon rods are increasing, especially in terms of stability and durability in high temperature environments.
[0003] First, silicon carbon rods work in high temperature environments for a long time, and their surfaces are easily affected by oxidation and corrosion, resulting in performance degradation and shortened life. Especially in high temperature acidic medium working environments, the oxidation resistance and corrosion resistance of silicon carbon rods become key factors restricting their application. Therefore, studying the surface modification method of high temperature resistant silicon carbon rods and improving their oxidation resistance and corrosion resistance are of great significance for extending the service life of silicon carbon rods and improving industrial production efficiency. Secondly, the surface properties of silicon carbon rods directly affect their bonding ability with other materials and thermal conductivity efficiency. In industrial production, silicon carbon rods often need to be combined with metals, ceramics and other materials to achieve the transfer and conversion of thermal energy. However, due to the chemical activity and physical structure characteristics of the surface of silicon carbon rods, the bonding ability with other materials is weak, and the thermal conductivity efficiency is also affected. Therefore, improving the chemical activity and physical structure of the surface of silicon carbon rods through surface modification technology, improving their bonding ability with other materials and thermal conductivity efficiency is an effective way to improve the performance of silicon carbon rods.
[0004] Patent CN 106220245 B discloses a method for preparing a high-temperature anti-oxidation coating on the surface of a recrystallized silicon carbon rod, which mainly includes the following steps: step (1): cleaning, decontaminating and drying the surface of the silicon carbon rod; step (2): using high-content silicone oil as a dispersant, adding a crosslinking agent and a catalyst to MoSi2 and Si3N4 powders with a volume ratio of 5:1 and a powder particle size of 1-6μm, and dispersing them into a uniform slurry; step (3): using the slurry obtained in step (2) to evenly coat the surface of the silicon carbon rod obtained in step (1), and putting it into an oven for crosslinking and curing; step (4): putting the silicon carbon rod obtained in step (3) into a high-temperature furnace, heating it to 800-1000℃ under a protective gas atmosphere, then keeping it warm for 1-2h, cooling it to room temperature and taking out the sample. The high silicon carbon rod prepared by this method has high-temperature anti-oxidation performance, but the high temperature resistance, anti-oxidation performance and corrosion resistance of the silicon carbon rod prepared by this method still have room for improvement. Summary of the invention
[0005] The object of the present invention is to provide a surface modification method of a high temperature resistant silicon carbon rod, which is used to solve the technical problem that the silicon carbon rod in the prior art has poor high temperature resistance, oxidation resistance and corrosion resistance.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The present invention provides a surface modification method for a high temperature resistant silicon carbon rod, comprising the following steps:
[0008] Step (1): cleaning the surface of the silicon carbon rod to remove dust and oil on the surface, and then drying it to obtain a clean silicon carbon rod;
[0009] Step (2): uniformly coating the obtained anti-oxidation coating on the surface of a clean silicon carbon rod, and obtaining an oxidation-resistant silicon carbon rod after drying;
[0010] Step (3): Use a spray gun to evenly spray the high temperature resistant material onto the surface of the oxidation resistant silicon carbon rod, then perform a cross-linking and curing treatment, and then place the rod in a high temperature furnace for heating treatment. After the treatment is completed, a high temperature resistant silicon carbon rod is obtained.
[0011] Preferably, the anti-oxidation coating in step (2) comprises silicon powder anti-oxidation coating and molybdenum disilicide anti-oxidation coating.
[0012] Preferably, the preparation method of the silicon powder anti-oxidation coating and the molybdenum disilicide anti-oxidation coating comprises the following steps:
[0013] Q1: Under an argon atmosphere, hexamethylene diisocyanate and tetrahydrofuran solution were added to a container, stirred evenly, and then tetradecanol and dibutyltin dilaurate were added. The temperature was raised to react. After the reaction was completed, rotary evaporation was performed to obtain an intermediate product 1.
[0014] Q2: Under an argon atmosphere, add organic polysilazane and tetrahydrofuran to a container, stir evenly, add intermediate product 1, heat to react, and after the reaction is completed, perform rotary evaporation to obtain intermediate product 2;
[0015] Q3: The intermediate product 2 is added to ethyl acetate, and ultrasonically dispersed to obtain a solution containing the intermediate product 2. Then, silicon powder and molybdenum disilicide powder are respectively added to the solution containing the intermediate product 2, and mixed to obtain silicon powder antioxidant coating and molybdenum disilicide antioxidant coating.
[0016] In the above process, hexamethylene diisocyanate and tetradecanol undergo a condensation reaction under the catalysis of dibutyltin dilaurate to obtain an intermediate product 1, and then the intermediate product 1 reacts with an organic polysilazane to obtain an intermediate product 2. Then, the intermediate product 2 is used as a precursor, and silicon powder and molybdenum disilicide powder are used as fillers to obtain an antioxidant coating.
[0017] Preferably, in Q1, the molar ratio of hexamethylene diisocyanate to tetradecanol is (0.8-1.2): (0.9-1.1), the stirring speed is 600-800 rpm, the heating reaction temperature is 40-50°C, and the reaction time is 3-6h; in Q2, the molar ratio of the organopolysilazane to the intermediate 1 is (0.9-1.1): (0.8-1.2), the stirring speed is 600-700 rpm, and the heating reaction temperature is The temperature is 30-34°C and the reaction time is 6-12h. In Q3, the dosage ratio of the intermediate product 2, ethyl acetate and silicon powder is (0.2-0.4) g: (4-10) mL: (0.1-0.2) g, the dosage ratio of the intermediate product 2, ethyl acetate and molybdenum disilicide is (0.2-0.4) g: (4-10) mL: (0.1-0.2) g, the ultrasonic dispersion time is 5-10 min, and the mixing time is 30-50 min.
[0018] Preferably, in step (2), the coating and drying process is as follows: placing the silicon carbon rod coated with the silicon powder anti-oxidation coating in a vacuum furnace, heating it to 1500°C at a rate of 3-5°C / min, keeping it warm for 30 minutes and then slowly cooling it at the same rate, then coating the surface with molybdenum disilicide anti-oxidation coating, then placing it in a vacuum furnace, heating it to 1200°C at a rate of 3-5°C / min, keeping it warm for 30 minutes and then slowly cooling it at the same rate, then repeating the coating with molybdenum disilicide anti-oxidation coating and high temperature treatment once.
[0019] Preferably, in step (3), the method for preparing the high temperature resistant material comprises the following steps:
[0020] S1: adding hafnium carbide, hafnium nitride and graphite-like carbon nitride into a ball mill, and drying them in an oven after ball milling to obtain pretreated powder;
[0021] S2: placing the pretreated powder in a mold, putting it into a spark plasma sintering furnace for sintering, and then cooling it to room temperature to obtain a high temperature resistant material.
[0022] In the above process, during the sintering process, chemical bonds between hafnium carbide, hafnium nitride and graphite-like carbon nitride are broken and reorganized to form a high temperature resistant material.
[0023] Preferably, in S1, the purity of hafnium carbide is 99.7wt% and the average particle size is 1μm, the purity of hafnium nitride is 99.8wt% and the average particle size is 1μm, the purity of graphite-like carbon nitride is 99.5wt% and the average particle size is 1-2μm, and the mass ratio of hafnium carbide, hafnium nitride and graphite-like carbon nitride is (75-90):(10-25):(10-14). During the ball milling process, the dispersion medium is ethanol, the ball milling time is 6-8h, the oven temperature is 80-85°C, and the drying time is 10-12h.
[0024] Preferably, in S2, before sintering, the vacuum degree in the sintering furnace is reduced to 0.1 mbar, and then filled with argon for protection, and then the temperature is increased to 2000°C at a rate of 10°C / min, and a pressure of 20 MPa is applied for 20 minutes.
[0025] Preferably, in step (3), the cross-linking curing temperature is 180-220°C, the time is 1-3h, and the heating treatment process is: under argon protection, the temperature is increased at a rate of 10°C / min to 1200-1400°C, the temperature is kept at a temperature for 2-4h, and then the temperature is cooled at a rate of 20°C / min.
[0026] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0027] 1. The present invention first uses hexamethylene diisocyanate, tetradecanol, organic polysilazane, silicon powder and molybdenum disilicide powder as raw materials to prepare an antioxidant coating, then uses hafnium carbide, hafnium nitride and graphite-like carbon nitride as raw materials, and obtains a high-temperature resistant material after sintering. The antioxidant coating and the high-temperature resistant material are coated on the surface of the silicon rod, and after treatment, a surface-modified silicon carbon rod with excellent antioxidant performance, corrosion resistance and high-temperature resistance is obtained.
[0028] 2. The present invention utilizes hexamethylene diisocyanate and tetradecanol to react to obtain an intermediate product 1, and then the intermediate product 1 is reacted with an organic polysilazane to obtain an intermediate product 2, and then silicon powder and molybdenum disilicide powder are used as fillers respectively to prepare silicon powder antioxidant coatings and molybdenum disilicide antioxidant coatings, and a transition layer / oxygen barrier layer multilayer structure antioxidant coating system is designed to effectively increase the antioxidant and corrosion resistance of the silicon carbon rod. The intermediate product 2 is converted into a ceramic material with high temperature resistance, corrosion resistance and antioxidant properties at high temperature. Silicon and molybdenum disilicide are used as fillers to further improve the heat resistance and stability of the antioxidant coating. Silicon powder reacts with oxygen at high temperature to form a dense protective film to prevent further penetration of oxygen, and molybdenum disilicide can also form a protective layer that can isolate oxygen under high temperature conditions, thereby making the silicon carbon rod have excellent antioxidant and corrosion resistance.
[0029] 3. The present invention obtains a high temperature resistant material by sintering hafnium oxide, hafnium nitride and graphite-like carbon nitride, and sprays the high temperature resistant material onto the surface of the silicon carbon rod, so that the silicon carbon rod has excellent high temperature resistance. Hafnium oxide and hafnium nitride have high melting points and good thermal stability, can maintain a stable structure and performance under high temperature conditions, and effectively prevent the silicon carbon rod from oxidation, thermal decomposition and other reactions under high temperature conditions. The layered structure of graphite-like carbon nitride has good lubricity and wear resistance, can reduce the friction and wear of the silicon carbon rod at high temperature, and extend the service life. The protective layer formed by the high temperature resistant material effectively isolates the direct contact between the silicon carbon rod and the external environment, further improving the high temperature resistance of the silicon carbon rod. DETAILED DESCRIPTION
[0030] The following will be combined with the technical solutions in the embodiments of the present invention to clearly and completely describe. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] The following embodiments of the present invention are used:
[0032] Hexamethylene diisocyanate was purchased from Shanghai MacLean Biochemical Technology Co., Ltd., CAS number: 822-06-0;
[0033] Tetrahydrofuran was purchased from Jinan Jinhao Chemical Co., Ltd., CAS No.: 109-99-9;
[0034] Tetradecanol was purchased from Shanghai Tuyi International Trading Co., Ltd., CAS number: 112-72-1;
[0035] Dibutyltin dilaurate was purchased from Shanghai MacLean Biochemical Technology Co., Ltd., CAS No.: 77-58-7;
[0036] Organopolysilazane was purchased from Guangdong Wengjiang Chemical Reagent Co., Ltd., CAS No.: 475645-84-2;
[0037] Ethyl acetate was purchased from Qianyan Chemical Technology (Wuhan) Co., Ltd., CAS No.: 141-78-6;
[0038] Silica powder was purchased from Jiangsu Runfeng Synthetic Technology Co., Ltd., CAS No.: 69012-64-2;
[0039] Molybdenum disilicide powder was purchased from Beijing Solebow Technology Co., Ltd., CAS number: 12136-78-6;
[0040] Hafnium carbide was purchased from Shanghai Jizhi Biochemical Technology Co., Ltd., CAS number: 12069-85-1;
[0041] Hafnium nitride was purchased from Shanghai MacLean Biochemical Technology Co., Ltd., CAS number: 25817-87-2;
[0042] Graphite-like carbon nitride was purchased from Shanghai MacLean Biochemical Technology Co., Ltd., CAS No.: 143334-20-7;
[0043] Ethanol was purchased from Jiangsu Pulex Biotechnology Co., Ltd., CAS No.: 64-17-5.
[0044] Example 1
[0045] This embodiment discloses a method for preparing a silicon powder anti-oxidation coating and a molybdenum disilicide anti-oxidation coating, comprising the following steps:
[0046] Q1: Under argon atmosphere, add 1.25 mL of hexamethylene diisocyanate and tetrahydrofuran solution into the container, stir evenly at 800 rpm, then add 1.61 g of tetradecanol and dibutyltin dilaurate, heat to 50 °C for 4 h, and after the reaction is completed, rotary evaporate to obtain intermediate 1;
[0047] Q2: Under argon atmosphere, add 2.62g of organopolysilazane and tetrahydrofuran into the container, stir evenly at 700rpm, add 1.25g of intermediate product 1, heat at 34°C for 12h, and after the reaction, rotary evaporate to obtain intermediate product 2;
[0048] Q3: Add 0.3 g of intermediate product 2 to 7 mL of ethyl acetate and ultrasonically disperse for 8 min to obtain a solution containing intermediate product 2. Then add 0.15 g of silicon powder and 0.15 g of molybdenum disilicide powder to the solution containing intermediate product 2 respectively and mix for 30 min to obtain silicon powder antioxidant coating and molybdenum disilicide antioxidant coating.
[0049] This embodiment discloses a method for preparing a high temperature resistant material, comprising the following steps:
[0050] S1: 83g of hafnium carbide with a purity of 99.7wt% and an average particle size of 1μm, 17.5g of hafnium nitride with a purity of 99.8wt% and an average particle size of 1μm, and 12g of graphite-like carbon nitride with a purity of 99.5wt% and an average particle size of 1-2μm were added to a ball mill. During the ball milling process, the dispersion medium was ethanol, the ball milling time was 6h, and after ball milling, it was placed in an oven at 85°C for 12h to obtain a pretreated powder;
[0051] S2: The pretreated powder is placed in a mold and put into a spark plasma sintering furnace. Before sintering, the vacuum degree in the sintering furnace is reduced to 0.1 mbar, and then argon is filled in for protection. Subsequently, the temperature is increased to 2000°C at a rate of 10°C / min, and a pressure of 20MPa is applied for insulation for 20 minutes. Subsequently, the material is cooled to room temperature to obtain a high temperature resistant material.
[0052] This embodiment discloses a surface modification method of a high temperature resistant silicon carbon rod, comprising the following steps:
[0053] Step (1): cleaning the surface of the silicon carbon rod to remove dust and oil on the surface, and then drying it to obtain a clean silicon carbon rod;
[0054] Step (2): placing the silicon carbon rod coated with silicon powder anti-oxidation coating in a vacuum furnace, heating it to 1500°C at a rate of 5°C / min, keeping it warm for 30 minutes and then slowly cooling it at the same rate, then coating the surface with molybdenum disilicide anti-oxidation coating, then placing it in a vacuum furnace, heating it to 1200°C at a rate of 5°C / min, keeping it warm for 30 minutes and then slowly cooling it at the same rate, then repeating the coating with molybdenum disilicide anti-oxidation coating and high temperature treatment once to obtain an oxidation-resistant silicon carbon rod;
[0055] Step (3): Use a spray gun to evenly spray the high temperature resistant material on the surface of the oxidation resistant silicon carbon rod, then perform a cross-linking and curing treatment at 220°C for 3 hours, then place it in a high temperature furnace for heating treatment, and heat it under argon protection at a heating rate of 10°C / min to 1400°C, keep it at this temperature for 2 hours, then cool it at a rate of 20°C / min. After the treatment, a high temperature resistant silicon carbon rod is obtained.
[0056] Example 2
[0057] This embodiment discloses a method for preparing a silicon powder anti-oxidation coating and a molybdenum disilicide anti-oxidation coating, comprising the following steps:
[0058] Q1: Under argon atmosphere, add 1.00 mL of hexamethylene diisocyanate and tetrahydrofuran solution into the container, stir evenly at 800 rpm, then add 1.45 g of tetradecanol and dibutyltin dilaurate, heat to 50 °C for 4 h, and after the reaction is completed, rotary evaporate to obtain intermediate 1;
[0059] Q2: Under argon atmosphere, add 2.35g of organopolysilazane and tetrahydrofuran into the container, stir evenly at 700rpm, add 1.00g of intermediate product 1, heat at 34°C for 12h, and after the reaction, rotary evaporate to obtain intermediate product 2;
[0060] Q3: Add 0.2 g of intermediate product 2 to 4 mL of ethyl acetate and disperse by ultrasonic for 8 min to obtain a solution containing intermediate product 2. Then add 0.10 g of silicon powder and 0.11 g of molybdenum disilicide powder to the solution containing intermediate product 2 respectively and mix for 30 min to obtain silicon powder antioxidant coating and molybdenum disilicide antioxidant coating.
[0061] This embodiment discloses a method for preparing a high temperature resistant material, comprising the following steps:
[0062] S1: 75g of hafnium carbide with a purity of 99.7wt% and an average particle size of 1μm, 10.0g of hafnium nitride with a purity of 99.8wt% and an average particle size of 1μm, and 10g of graphite-like carbon nitride with a purity of 99.5wt% and an average particle size of 1-2μm were added to a ball mill. During the ball milling process, the dispersion medium was ethanol, the ball milling time was 6h, and after ball milling, it was placed in an oven at 85°C for 12h to obtain a pretreated powder;
[0063] S2: The pretreated powder is placed in a mold and put into a spark plasma sintering furnace. Before sintering, the vacuum degree in the sintering furnace is reduced to 0.1 mbar, and then argon is filled in for protection. Subsequently, the temperature is increased to 2000°C at a rate of 10°C / min, and a pressure of 20MPa is applied for insulation for 20 minutes. Subsequently, the material is cooled to room temperature to obtain a high temperature resistant material.
[0064] This embodiment discloses a surface modification method of a high temperature resistant silicon carbon rod, comprising the following steps:
[0065] Step (1): cleaning the surface of the silicon carbon rod to remove dust and oil on the surface, and then drying it to obtain a clean silicon carbon rod;
[0066] Step (2): placing the silicon carbon rod coated with silicon powder anti-oxidation coating in a vacuum furnace, heating it to 1500°C at a rate of 5°C / min, keeping it warm for 30 minutes and then slowly cooling it at the same rate, then coating the surface with molybdenum disilicide anti-oxidation coating, then placing it in a vacuum furnace, heating it to 1200°C at a rate of 5°C / min, keeping it warm for 30 minutes and then slowly cooling it at the same rate, then repeating the coating with molybdenum disilicide anti-oxidation coating and high temperature treatment once to obtain an oxidation-resistant silicon carbon rod;
[0067] Step (3): Use a spray gun to evenly spray the high temperature resistant material on the surface of the oxidation resistant silicon carbon rod, then perform a cross-linking and curing treatment at 220°C for 3 hours, then place it in a high temperature furnace for heating treatment, and heat it under argon protection at a heating rate of 10°C / min to 1400°C, keep it at this temperature for 2 hours, then cool it at a rate of 20°C / min. After the treatment, a high temperature resistant silicon carbon rod is obtained.
[0068] Example 3
[0069] This embodiment discloses a method for preparing a silicon powder anti-oxidation coating and a molybdenum disilicide anti-oxidation coating, comprising the following steps:
[0070] Q1: Under argon atmosphere, add 1.50 mL of hexamethylene diisocyanate and tetrahydrofuran solution into the container, stir evenly at 800 rpm, then add 1.77 g of tetradecanol and dibutyltin dilaurate, heat to 50 °C for 4 h, and after the reaction is completed, rotary evaporate to obtain intermediate 1;
[0071] Q2: Under argon atmosphere, add 2.88g of organopolysilazane and tetrahydrofuran into the container, stir evenly at 700rpm, add 1.50g of intermediate product 1, heat at 34°C for 12h, and after the reaction, rotary evaporate to obtain intermediate product 2;
[0072] Q3: Add 0.4 g of intermediate product 2 to 10 mL of ethyl acetate and ultrasonically disperse for 8 min to obtain a solution containing intermediate product 2. Then add 0.2 g of silicon powder and 0.15 g of molybdenum disilicide powder to the solution containing intermediate product 2 respectively and mix for 30 min to obtain silicon powder antioxidant coating and molybdenum disilicide antioxidant coating.
[0073] This embodiment discloses a method for preparing a high temperature resistant material, comprising the following steps:
[0074] S1: 90g of hafnium carbide with a purity of 99.7wt% and an average particle size of 1μm, 25g of hafnium nitride with a purity of 99.8wt% and an average particle size of 1μm, and 14g of graphite-like carbon nitride with a purity of 99.5wt% and an average particle size of 1-2μm were added to a ball mill. During the ball milling process, the dispersion medium was ethanol, the ball milling time was 6h, and after ball milling, it was placed in an oven at 85°C for 12h to obtain a pretreated powder;
[0075] S2: The pretreated powder is placed in a mold and put into a spark plasma sintering furnace. Before sintering, the vacuum degree in the sintering furnace is reduced to 0.1 mbar, and then argon is filled in for protection. Subsequently, the temperature is increased to 2000°C at a rate of 10°C / min, and a pressure of 20MPa is applied for insulation for 20 minutes. Subsequently, the material is cooled to room temperature to obtain a high temperature resistant material.
[0076] This embodiment discloses a surface modification method of a high temperature resistant silicon carbon rod, comprising the following steps:
[0077] Step (1): cleaning the surface of the silicon carbon rod to remove dust and oil on the surface, and then drying it to obtain a clean silicon carbon rod;
[0078] Step (2): placing the silicon carbon rod coated with silicon powder anti-oxidation coating in a vacuum furnace, heating it to 1500°C at a rate of 5°C / min, keeping it warm for 30 minutes and then slowly cooling it at the same rate, then coating the surface with molybdenum disilicide anti-oxidation coating, then placing it in a vacuum furnace, heating it to 1200°C at a rate of 5°C / min, keeping it warm for 30 minutes and then slowly cooling it at the same rate, then repeating the coating with molybdenum disilicide anti-oxidation coating and high temperature treatment once to obtain an oxidation-resistant silicon carbon rod;
[0079] Step (3): Use a spray gun to evenly spray the high temperature resistant material on the surface of the oxidation resistant silicon carbon rod, then perform a cross-linking and curing treatment at 220°C for 3 hours, then place it in a high temperature furnace for heating treatment, and heat it under argon protection at a heating rate of 10°C / min to 1400°C, keep it at this temperature for 2 hours, then cool it at a rate of 20°C / min. After the treatment, a high temperature resistant silicon carbon rod is obtained.
[0080] Example 4
[0081] This embodiment discloses a method for preparing a silicon powder anti-oxidation coating and a molybdenum disilicide anti-oxidation coating, comprising the following steps:
[0082] Q1: Under argon atmosphere, add 1.1 mL of hexamethylene diisocyanate and tetrahydrofuran solution into the container, stir evenly at 800 rpm, then add 1.53 g of tetradecanol and dibutyltin dilaurate, heat to 50 °C for 4 h, and after the reaction is completed, rotary evaporate to obtain intermediate 1;
[0083] Q2: Under argon atmosphere, add 2.47g of organopolysilazane and tetrahydrofuran into the container, stir evenly at 700rpm, add 1.1g of intermediate product 1, heat at 34°C for 12h, and after the reaction, rotary evaporate to obtain intermediate product 2;
[0084] Q3: Add 0.25 g of intermediate product 2 to 6 mL of ethyl acetate and ultrasonically disperse for 8 min to obtain a solution containing intermediate product 2. Then add 0.11 g of silicon powder and 0.18 g of molybdenum disilicide powder to the solution containing intermediate product 2, respectively, and mix for 30 min to obtain silicon powder antioxidant coating and molybdenum disilicide antioxidant coating.
[0085] This embodiment discloses a method for preparing a high temperature resistant material, comprising the following steps:
[0086] S1: 78g of hafnium carbide with a purity of 99.7wt% and an average particle size of 1μm, 12g of hafnium nitride with a purity of 99.8wt% and an average particle size of 1μm, and 11g of graphite-like carbon nitride with a purity of 99.5wt% and an average particle size of 1-2μm were added to a ball mill. During the ball milling process, the dispersion medium was ethanol, the ball milling time was 6h, and after ball milling, it was placed in an oven at 85°C for 12h to obtain a pretreated powder;
[0087] S2: The pretreated powder is placed in a mold and put into a spark plasma sintering furnace. Before sintering, the vacuum degree in the sintering furnace is reduced to 0.1 mbar, and then argon is filled in for protection. Subsequently, the temperature is increased to 2000°C at a rate of 10°C / min, and a pressure of 20MPa is applied for insulation for 20 minutes. Subsequently, the material is cooled to room temperature to obtain a high temperature resistant material.
[0088] This embodiment discloses a surface modification method of a high temperature resistant silicon carbon rod, comprising the following steps:
[0089] Step (1): cleaning the surface of the silicon carbon rod to remove dust and oil on the surface, and then drying it to obtain a clean silicon carbon rod;
[0090] Step (2): placing the silicon carbon rod coated with silicon powder anti-oxidation coating in a vacuum furnace, heating it to 1500°C at a rate of 5°C / min, keeping it warm for 30 minutes and then slowly cooling it at the same rate, then coating the surface with molybdenum disilicide anti-oxidation coating, then placing it in a vacuum furnace, heating it to 1200°C at a rate of 5°C / min, keeping it warm for 30 minutes and then slowly cooling it at the same rate, then repeating the coating with molybdenum disilicide anti-oxidation coating and high temperature treatment once to obtain an oxidation-resistant silicon carbon rod;
[0091] Step (3): Use a spray gun to evenly spray the high temperature resistant material on the surface of the oxidation resistant silicon carbon rod, then perform a cross-linking and curing treatment at 220°C for 3 hours, then place it in a high temperature furnace for heating treatment, and heat it under argon protection at a heating rate of 10°C / min to 1600°C, keep it at this temperature for 2 hours, then cool it at a rate of 20°C / min. After the treatment, a high temperature resistant silicon carbon rod is obtained.
[0092] Example 5
[0093] This embodiment discloses a method for preparing a silicon powder anti-oxidation coating and a molybdenum disilicide anti-oxidation coating, comprising the following steps:
[0094] Q1: Under argon atmosphere, add 1.4 mL of hexamethylene diisocyanate and tetrahydrofuran solution into the container, stir evenly at 800 rpm, then add 1.68 g of tetradecanol and dibutyltin dilaurate, heat to 50 °C for 4 h, and after the reaction is completed, rotary evaporate to obtain intermediate 1;
[0095] Q2: Under argon atmosphere, add 2.75 g of organopolysilazane and tetrahydrofuran into the container, stir evenly at 700 rpm, add 1.4 g of intermediate 1, heat at 34 °C for 12 h, and after the reaction, rotary evaporate to obtain intermediate 2;
[0096] Q3: Add 0.35 g of intermediate product 2 to 8 mL of ethyl acetate and disperse by ultrasonic for 8 min to obtain a solution containing intermediate product 2. Then add 0.18 g of silicon powder and 0.18 g of molybdenum disilicide powder to the solution containing intermediate product 2 respectively and mix for 30 min to obtain silicon powder antioxidant coating and molybdenum disilicide antioxidant coating.
[0097] This embodiment discloses a method for preparing a high temperature resistant material, comprising the following steps:
[0098] S1: 85g of hafnium carbide with a purity of 99.7wt% and an average particle size of 1μm, 23g of hafnium nitride with a purity of 99.8wt% and an average particle size of 1μm, and 13g of graphite-like carbon nitride with a purity of 99.5wt% and an average particle size of 1-2μm were added to a ball mill. During the ball milling process, the dispersion medium was ethanol, the ball milling time was 6h, and after ball milling, it was placed in an oven at 85°C for 12h to obtain a pretreated powder;
[0099] S2: The pretreated powder is placed in a mold and put into a spark plasma sintering furnace. Before sintering, the vacuum degree in the sintering furnace is reduced to 0.1 mbar, and then argon is filled in for protection. Subsequently, the temperature is increased to 2000°C at a rate of 10°C / min, and a pressure of 20MPa is applied for insulation for 20 minutes. Subsequently, the material is cooled to room temperature to obtain a high temperature resistant material.
[0100] This embodiment discloses a surface modification method of a high temperature resistant silicon carbon rod, comprising the following steps:
[0101] Step (1): cleaning the surface of the silicon carbon rod to remove dust and oil on the surface, and then drying it to obtain a clean silicon carbon rod;
[0102] Step (2): placing the silicon carbon rod coated with silicon powder anti-oxidation coating in a vacuum furnace, heating it to 1500°C at a rate of 5°C / min, keeping it warm for 30 minutes and then slowly cooling it at the same rate, then coating the surface with molybdenum disilicide anti-oxidation coating, then placing it in a vacuum furnace, heating it to 1200°C at a rate of 5°C / min, keeping it warm for 30 minutes and then slowly cooling it at the same rate, then repeating the coating with molybdenum disilicide anti-oxidation coating and high temperature treatment once to obtain an oxidation-resistant silicon carbon rod;
[0103] Step (3): Use a spray gun to evenly spray the high temperature resistant material on the surface of the oxidation resistant silicon carbon rod, then perform a cross-linking and curing treatment at 220°C for 3 hours, then place it in a high temperature furnace for heating treatment, and heat it under argon protection at a heating rate of 10°C / min to 1400°C, keep it at this temperature for 2 hours, then cool it at a rate of 20°C / min. After the treatment, a high temperature resistant silicon carbon rod is obtained.
[0104] Comparative Example 1
[0105] Comparative Example 1 Compared with Example 1, in the process of preparing the antioxidant coating in Comparative Example 1, hexamethylene diisocyanate is not added, and other conditions remain unchanged.
[0106] Comparative Example 2
[0107] Comparative Example 2 Compared with Example 1, in the process of preparing the antioxidant coating in Comparative Example 2, no organic polysilazane is added, and other conditions remain unchanged.
[0108] Comparative Example 3
[0109] Comparative Example 3 Compared with Example 1, in the process of preparing the antioxidant coating in Comparative Example 3, no silicon powder is added, and other conditions remain unchanged.
[0110] Comparative Example 4
[0111] Comparative Example 4 Compared with Example 1, in the process of preparing the antioxidant coating in Comparative Example 4, no molybdenum disilicide powder is added, and other conditions remain unchanged.
[0112] Comparative Example 5
[0113] Comparative Example 5 Compared with Example 1, in the process of preparing the high temperature resistant material in Comparative Example 5, no hafnium nitride is added, and other conditions remain unchanged.
[0114] Comparative Example 6
[0115] Compared with Example 1, in Comparative Example 6, during the preparation of the high-temperature resistant material, no graphite-like carbon nitride was added, and other conditions remained unchanged.
[0116] Comparative Example 7
[0117] Comparative Example 7 Compared with Example 1, in the process of surface modification of silicon carbon rods in Comparative Example 7, no antioxidant coating was added, and other conditions remained unchanged.
[0118] Comparative Example 8
[0119] Comparative Example 8 Compared with Example 1, in the process of surface modification of silicon carbon rods in Comparative Example 8, no high temperature resistant material is added, and other conditions remain unchanged.
[0120] The samples prepared in Examples 1-5 and Comparative Examples 1-8 were tested. The high temperature resistance and oxidation resistance of the samples were tested according to JB / T 3890-2017. The corrosion resistance of the samples was tested according to Test Method B in GB / T 28416-2012. The weight of the silicon carbon rods before and after the test was tested. The weight loss rate of corrosion was calculated based on the weight loss rate of corrosion = [(m 腐蚀前 -m 腐蚀后 ) / m 腐蚀前 ]×100% for calculation, the test results are shown in Table 1:
[0121]
[0122] It can be seen from the test results in Table 1 that the silicon carbon rods prepared in Examples 1-5 of the present invention have excellent corrosion resistance, high temperature resistance and oxidation resistance. By comparing Comparative Example 1 with Examples 1-5, it can be seen that the addition of hexamethylene diisocyanate can effectively improve the corrosion resistance and oxidation resistance of silicon carbon rods; by comparing Comparative Example 2 with Examples 1-5, it can be seen that the addition of organic polysilazane can effectively improve the corrosion resistance and oxidation resistance of silicon carbon rods; by comparing Comparative Example 3 with Examples 1-5, it can be seen that the addition of silicon powder can effectively improve the corrosion resistance and oxidation resistance of silicon carbon rods; by comparing Comparative Example 4 with Examples 1-5, it can be seen that the addition of molybdenum disilicide powder can effectively improve the corrosion resistance of silicon carbon rods. The results show that the addition of hafnium nitride can effectively improve the high temperature resistance of silicon carbon rods; the addition of graphite-like carbon nitride can effectively improve the high temperature resistance of silicon carbon rods; the addition of antioxidant coating can effectively improve the corrosion resistance and oxidation resistance of silicon carbon rods; the addition of high temperature resistant material can effectively improve the high temperature resistance of silicon carbon rods.
[0123] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
[0124] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A surface modification method for a high temperature resistant silicon carbon rod, characterized in that: The following steps are involved: Step (1): cleaning the surface of the silicon carbon rod to remove dust and oil on the surface, and then drying it to obtain a clean silicon carbon rod; Step (2): uniformly coating the obtained antioxidant coating on the surface of a clean silicon carbon rod, and obtaining an oxidation-resistant silicon carbon rod after drying. The antioxidant coating includes a silicon powder antioxidant coating and a molybdenum disilicide antioxidant coating. The preparation method of the silicon powder antioxidant coating and the molybdenum disilicide antioxidant coating includes the following steps: Q1: Under an argon atmosphere, hexamethylene diisocyanate and tetrahydrofuran solution were added to a container, stirred evenly, and then tetradecanol and dibutyltin dilaurate were added. The temperature was raised to react. After the reaction was completed, rotary evaporation was performed to obtain an intermediate product 1. Q2: Under an argon atmosphere, add organic polysilazane and tetrahydrofuran to a container, stir evenly, add intermediate product 1, heat to react, and after the reaction is completed, perform rotary evaporation to obtain intermediate product 2; Q3: adding the intermediate product 2 to ethyl acetate, ultrasonically dispersing to obtain a solution containing the intermediate product 2, and then adding silicon powder and molybdenum disilicide powder to the solution containing the intermediate product 2, respectively, and mixing to obtain silicon powder antioxidant coating and molybdenum disilicide antioxidant coating; Step (3): Use a spray gun to evenly spray the high temperature resistant material onto the surface of the oxidation resistant silicon carbon rod, then perform a cross-linking and curing treatment, and then place the rod in a high temperature furnace for heating treatment. After the treatment is completed, a high temperature resistant silicon carbon rod is obtained.
2. The surface modification method of a high temperature resistant silicon carbon rod according to claim 1, characterized in that: In the Q1, the molar ratio of hexamethylene diisocyanate to tetradecanol is (0.8-1.2): (0.9-1.1), the stirring speed is 600-800 rpm, the heating reaction temperature is 40-50°C, and the reaction time is 3-6h; in the Q2, the molar ratio of the organopolysilazane to the intermediate 1 is (0.9-1.1): (0.8-1.2), the stirring speed is 600-700 rpm, and the heating reaction temperature is 3 0-34°C, the reaction time is 6-12h; in Q3, the dosage ratio of the intermediate product 2, ethyl acetate and silicon powder is (0.2-0.4) g: (4-10) mL: (0.1-0.2) g, the dosage ratio of the intermediate product 2, ethyl acetate and molybdenum disilicide is (0.2-0.4) g: (4-10) mL: (0.1-0.2) g, the ultrasonic dispersion time is 5-10 min, and the mixing time is 30-50 min.
3. The surface modification method of a high temperature resistant silicon carbon rod according to claim 1, characterized in that: In the step (2), the coating and drying process is as follows: placing the silicon carbon rod coated with the silicon powder anti-oxidation coating in a vacuum furnace, heating it to 1500°C at a rate of 3-5°C / min, keeping it warm for 30 minutes and then slowly cooling it at the same rate, then coating the surface with molybdenum disilicide anti-oxidation coating, then placing it in a vacuum furnace, heating it to 1200°C at a rate of 3-5°C / min, keeping it warm for 30 minutes and then slowly cooling it at the same rate, then repeating the coating with molybdenum disilicide anti-oxidation coating and high temperature treatment once.
4. The surface modification method of a high temperature resistant silicon carbon rod according to claim 1, characterized in that: In step (3), the method for preparing the high temperature resistant material comprises the following steps: S1: adding hafnium carbide, hafnium nitride and graphite-like carbon nitride into a ball mill, and drying them in an oven after ball milling to obtain pretreated powder; S2: placing the pretreated powder in a mold, putting it into a spark plasma sintering furnace for sintering, and then cooling it to room temperature to obtain a high temperature resistant material.
5. The surface modification method of a high temperature resistant silicon carbon rod according to claim 4, characterized in that: In S1, the purity of hafnium carbide is 99.7wt% and the average particle size is 1μm, the purity of hafnium nitride is 99.8wt% and the average particle size is 1μm, the purity of graphite-like carbon nitride is 99.5wt% and the average particle size is 1-2μm, and the mass ratio of hafnium carbide, hafnium nitride and graphite-like carbon nitride is (75-90): (10-25): (10-14). During the ball milling process, the dispersion medium is ethanol, the ball milling time is 6-8h, the oven temperature is 80-85°C, and the drying time is 10-12h.
6. The surface modification method of a high temperature resistant silicon carbon rod according to claim 4, characterized in that: In S2, before sintering, the vacuum degree in the sintering furnace is reduced to 0.1 mbar, and then filled with argon for protection, and then the temperature is increased to 2000° C. at a rate of 10° C. / min, and a pressure of 20 MPa is applied for 20 min.
7. The surface modification method of a high temperature resistant silicon carbon rod according to claim 1, characterized in that: In the step (3), the cross-linking curing temperature is 180-220°C, the time is 1-3h, and the heating treatment process is: under argon protection, the temperature is increased at a rate of 10°C / min to 1200-1400°C, the temperature is kept at a temperature for 2-4h, and then the temperature is cooled at a rate of 20°C / min.
Citation Information
Patent Citations
Preparation method of high-temperature anti-oxidation coating on the surface of recrystallized silicon carbide rods
CN106220245B
Preparing method of high-temperature anti-oxidation coating on surface of recrystal silicon carbide rod
CN106220245A
Glass coating for surface of silicon carbide rod and preparation method of glass coating
CN113800950A
Silicon carbide rod with low oxidation degree under high-temperature condition
CN114736021A
Novel preparation method of ultrahigh-melting-point hafnium carbonitride powder
CN115806277A