A kind of nano paper hydrogel and preparation method thereof

By introducing the dual network structure of PVA, TOCNF, Mxene and borate into the hydrogel, the stability of the hydrogel in high temperature and high humidity environment is solved, and high sensitivity and long-term reliable sensing performance are achieved. In a variety of medical and health monitoring applications.

CN118652448BActive Publication Date: 2024-11-22XIAN JIAOTONG LIVERPOOL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411133181.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-22
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

Existing hydrogel sensors perform poorly in high temperature and high humidity environments, making it difficult to maintain environmental stability in harsh climatic conditions and variable environments, which limits their wide application, especially when monitoring human movement activities.

Method used

Using the preparation method of nanopaper hydrogel, PVA, TOCNF, Mxene and borate are mixed in a specific proportion to form a polymer dual network structure, combining ultrasonic treatment and dynamic reversible borate bonds to improve its mechanical properties and environment. stability.

Benefits of technology

The designed nanopaper hydrogel has excellent environmental stability, strain sensitivity, temperature tolerance and thermal and humidity stability. It is suitable for wearable human detection equipment, which can effectively monitor human movement and health, and has antibacterial properties and biological phases. Capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118652448B_ABST
    Figure CN118652448B_ABST
Patent Text Reader

Abstract

The present invention relates to a nanopaper hydrogel, comprising: PVA, TOCNF, MXene, borate and deionized water; wherein the mass ratio of PVA to TOCNF is 1:8, the mass ratio of PVA to MXene is 50:1-10:1, and the mass ratio of PVA to borate is 20:1; PVA, TOCNF and MXene are cross-linked to form a polymer network to form a first network structure, and the borate forms a dynamic reversible borate ester bond with PVA and TOCNF to form a second network structure. The present invention also relates to a method for preparing the nanopaper hydrogel and a sensor prepared from the nanopaper hydrogel. The nanopaper hydrogel designed in the present application has the characteristics of excellent environmental stability, excellent strain sensitivity, excellent temperature tolerance, excellent thermal and wet stability, excellent antibacterial properties, excellent biocompatibility and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrogel materials, in particular to a nano paper hydrogel and a preparation method thereof. Background Art

[0002] Wearable sensor technology is revolutionizing healthcare through continuous, non-invasive monitoring of physiological parameters. An ideal strain sensor should have good stretchability (Young's modulus or strain factor), high sensitivity, fast response and recovery, linearity, low hysteresis, and good dynamic durability to fully monitor human movement activities. Hydrogel sensors have proven to be a promising solution due to their physiological and mechanical properties similar to human skin (high water content and tunable physicochemical properties) and their potential to monitor human health in real-time, accurately, comfortably, and at low cost.

[0003] In the prior art, most hydrogel sensors can sense physical deformation in a stable environment, but they usually perform poorly in terms of temperature tolerance and resistance to moisture and high temperature, which greatly limits the widespread application of hydrogel-based sensors in harsh climatic conditions and environments with variable temperature and humidity. However, practical application scenarios require sensors to have environmental stability, such as the high temperature and high humidity environment during athletes' exercise, the environment of newborns in infant incubators, etc. Therefore, the design and development of hydrogels with multiple environmental tolerance has become an urgent need and a major challenge. Furthermore, the environmental stability of strain sensors should be high enough to minimize the impact of daily human activities (such as temperature and humidity changes). Human skin is a complex physiological system that continuously radiates heat to the outside world and continuously produces sweat. These metabolites in the body change the temperature and humidity of the microenvironment. Although significant progress has been made in this regard in the past decade, there is still a challenge to manufacture strain sensors with both excellent environmental stability and the ability to sense human motion over a full range. Summary of the invention

[0004] The purpose of the present invention is to solve the deficiencies of the prior art and provide a hydrogel with good environmental stability, tolerance to high temperature and high humidity, and the ability to sense human body movements in a full range.

[0005] In a first aspect, the present application provides a method for preparing a nanopaper hydrogel, comprising the following steps:

[0006] S1. Add PVA to deionized water, heat and stir evenly to fully dissolve it, and obtain a PVA solution;

[0007] S2, adding TOCNF to the PVA solution, stirring and mixing evenly to obtain a mixed solution;

[0008] S3, adding Mxene to the mixed solution, adding deionized water, stirring evenly and then ultrasonically treating to fully mix, to obtain a mixed gel;

[0009] S4, adding borate to the mixed gel, stirring evenly, to obtain nanopaper hydrogel.

[0010] The mass ratio of PVA to TOCNF is 1:8, the mass ratio of PVA to Mxene is 50:1-10:1, and the mass ratio of PVA to borate is 20:1; the PVA, TOCNF and MXene are cross-linked to form a polymer network to form a first network structure, the borate forms a dynamic reversible borate ester bond with PVA and TOCNF to form a second network structure, and the Mxene is Ti3C2T x The borate is borax.

[0011] More specifically, preferably, the mass ratio of PVA to Mxene is 50:3.

[0012] More specifically, in step S1, the heating temperature is 80°C to 90°C.

[0013] More specifically, in step S2, the fiber length of the TOCNF is 0.5~2.0 μm.

[0014] More specifically, in step S3, after the mixture is stirred and mixed evenly, an ultrasonic treatment process is also included.

[0015] More specifically, in step S4, the borate is added as a solution.

[0016] In a second aspect, the present application also provides a nanopaper hydrogel prepared by the above method.

[0017] In a third aspect, the present application also provides a nanopaper hydrogel sensor.

[0018] In a fourth aspect, the present application provides an application of the above-mentioned nanopaper hydrogel sensor in a soft robot.

[0019] In a fifth aspect, the present application provides an application of a nanopaper hydrogel sensor in a wearable human body detection device.

[0020] The beneficial effects of the present invention are:

[0021] 1. The nanopaper hydrogel designed in this application has excellent environmental stability, excellent strain sensitivity, excellent temperature tolerance, excellent thermal and moisture stability and excellent antibacterial properties, and has excellent biocompatibility, is safe and non-toxic, is attached to human skin, is cool and comfortable, and is an excellent sensing material for wearable human detection equipment.

[0022] 2. The nanopaper hydrogel sensor designed in this application has good sensing capabilities and has good detection sensitivity for activities such as fingers, wrists, forehead, chin, pulse, heartbeat, etc. It can sense human movements such as speaking, writing, and breathing. It can be used in neonatal monitoring, physical condition monitoring during exercise, postoperative rehabilitation training, pronunciation recognition and pronunciation training for the deaf and mute, and can also be used for early diagnosis of asthma, heart failure, embolism and other diseases. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is a scanning electron microscope image of the nanopaper hydrogel of the present application;

[0024] Figure 2 This is a graph showing the mechanical strength test of the nanopaper hydrogel of this application;

[0025] Figure 3 This is a test chart of the tensile strength, Young's modulus, and maximum tensile force of the nanopaper hydrogel of the present application;

[0026] Figure 4 This is a sensitivity test diagram of the nano-hydrogel of the present application under different stretching amounts;

[0027] Figure 5 This is a test diagram of the self-healing performance of the nanopaper hydrogel in this application;

[0028] Figure 6 This is a test diagram of the environmental stability of the nanopaper hydrogel of the present application;

[0029] Figure 7 This is a graph of the activity monitoring data of fingers and wrists by the nanopaper hydrogel sensor of the present application;

[0030] Figure 8 This is a data graph of the activity monitoring of the forehead and chin by the nanopaper hydrogel sensor of the present application;

[0031] Fig. 9 This is the data graph of the activity monitoring of the throat speaking by the nanopaper hydrogel sensor of this application;

[0032] Fig.10 This is a graph of the activity monitoring data of finger writing by the nanopaper hydrogel sensor of the present application;

[0033] Fig.11 This is a pulse monitoring data diagram of the nanopaper hydrogel sensor of the present application;

[0034] Fig.12 This is a data graph of heart rate monitoring by the nanopaper hydrogel sensor of the present application;

[0035] Fig.13This is a data chart of the monitoring of human breathing by the nanopaper hydrogel sensor of this application. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical scheme and advantages of the implementation of the present invention clearer, the specific implementation methods of the present invention are clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] The nanopaper hydrogel designed in this application includes: PVA, TOCNF, Mxene, borate and deionized water; wherein the mass ratio of PVA to TOCNF is 1:8, the mass ratio of PVA to Mxene is 50:1~10:1, and the mass ratio of PVA to borate is 20:1. The nanopaper hydrogel is a polymer double network structure, which is formed based on (2,2,6,6-tetramethylpiperidin-1-oxy) oxidized cellulose nanofibers TOCNF and polyvinyl alcohol (PVA). The PVA elastic material has high crystallinity and a dense network, and serves as a supporting skeleton in the hydrogel. The plant-derived TEMPO oxidized cellulose nanofibers (TOCNF) have uniform microscopic size (0.5-2.0μm), excellent mechanical properties, good modifiability and abundant functional groups (cellulose C6 primary hydroxyl groups can be selectively oxidized to carboxyl groups), and are effective reinforcing materials as interlayer crosslinkers in the hydrogel. The double network structure includes a polymer network formed by cross-linking PVA, TOCNF and MXene, i.e. the first network structure, and a dynamically reversible borate bond formed by PVA, TOCNF and borate, i.e. the second network structure. The double network structure gives the hydrogel excellent mechanical properties and high strength, can withstand high levels of tensile and compressive deformation, and has characteristics such as shear thinning and multiple responsiveness.

[0038] This application adds MXene materials to the formula. MXene materials exhibit high metal-like conductivity due to the presence of their transition metal carbide or nitride layered structure. At the same time, MXene has rich surface functional groups and a large specific surface area, showing excellent electrochemical properties. MXene two-dimensional materials are very suitable as conductive fillers in hydrogel systems due to their excellent water dispersibility, interaction with hydrogel precursors and sensitive conductivity. In particular, the high conductivity of MXene is very beneficial for constructing efficient conductive paths in polymer-based hydrogels. Hydrogels containing MXene nanosheet fillers have been significantly improved in electrical, mechanical and stress / strain sensing properties.

[0039] This application selects the prepared MXene nanosheets as the building blocks, and utilizes its rich surface functional groups (such as -OH, -F, -O, etc.), large specific surface area and high conductivity, and uses the electrostatic repulsion between the MXene nanosheets to make them uniformly dispersed in the colloid. The MXene nanosheets are uniformly dispersed in the double network structure, and are bonded to the PVA support skeleton through hydrogen bonds to form an elastic layer, simulating the "calcite sheets" arranged in parallel in the alternating layered structure. The highly conductive MXene effectively improves the conductivity of the hydrogel; the rich surface functional groups of MXene interact with the polymer network to enhance the sensitivity of the hydrogel. Preferably, the MXene material uses homemade Ti3C2T x Solution. Ti3C2T x Solution preparation method: 2 g LiF was dissolved in 40 mL 9 mol / L HCl, stirred in a polytetrafluoroethylene (PTFE) container for 30 min, and then 2 g Ti3AlC2 powder was slowly added to the solution, stirred and reacted at 35 °C for 24 h. After sufficient reaction, the solution was centrifuged at 3500 rpm to pH 5. At pH 5, Ti3C2T x The Ti3C2T4 was obtained by re-dispersing the precipitate in deionized water (DI) and ultrasonically treating it for 10 min. The precipitate was then centrifuged at 3500 rpm for 5 min, and the supernatant was collected to obtain the Ti3C2T4 x Solution.

[0040] Borates are added to the formula. The boric acid groups in the borate form dynamic reversible borate ester bonds with PVA and TOCNF. Specifically, borate can provide boric acid groups (B(OH)3 or B(OH)4 — ), these groups can form reversible borate ester bonds with the hydroxyl groups (OH) on the surface of PVA and TOCNF, thus giving the nanopaper hydrogel strong self-healing ability and good recyclability.

[0041] In the hydrogel formula designed in this application, PVA and TOCNF are the skeleton of the hydrogel, and the ratio between the materials is strictly set. When the ratio between PVA and TOCNF is too large, the hydrogel will be too hard to show flexibility and difficult to stably fit on the skin. When the ratio between PVA and TOCNF is too small, the hydrogel cannot be formed, cannot form a film, will be in a solution state, and cannot be used. When the borate content is too much, the formed hydrogel becomes brittle, and when the borate content is too little, the number of borate ester bonds is small, and the hydrogel self-healing performance is poor.

[0042] In the following specific examples, the nano-hydrogel formula is selected from: 4 g TOCNF (Tianjin Wood Elf Biotechnology Co., Ltd., fiber length 0.5-1 um), 0.5 g PVA particles (Rohn's reagent, PVA 1799), Ti3C2T x (Ti3C2T is prepared according to the above method) x solution, with a concentration of 10 mg / ml) and 0.5 mL of borax solution with a concentration of 50 mg / mL. The hydrogels were prepared by adding different amounts of Ti3C2T x The hydrogels were named PBTM-X, where PBTM-1 means that 1 ml Ti3C2T x Solution; PBTM-2, means 2 ml Ti3C2T was added x Solution, and PBTM-3, PBTM-4 and PBTM-5 are prepared by analogy.

[0043] The preparation method of the nanopaper hydrogel designed in this application (taking PBTM-1 as an example):

[0044] S1. Add 0.5 g of PVA particles into 5 ml of deionized water, stir evenly with a magnetic stirrer, and then heat to 90° C. and continue to stir vigorously until the PVA is completely dissolved to obtain a PVA solution;

[0045] S2, adding 4 g of TOCNF to the PVA solution, and continuing to stir for 60 minutes to fully mix, to obtain a mixed solution;

[0046] S3, 1 ml Ti3C2T x Add to the mixed solution, add 4 ml of deionized water, stir for 30 minutes and then ultrasonicate for 30 minutes to mix thoroughly to obtain a mixed gel;

[0047] S4. Add 0.5 ml of borax solution into the mixed gel and stir evenly to obtain nanopaper hydrogel.

[0048] The present application also provides a nanopaper hydrogel sensor, wherein the prepared nanopaper hydrogel is led out with a positive and negative electrode using a wire to obtain a nanopaper hydrogel sensor.

[0049] The above method was used to prepare Examples PBTM-1 to PBTM-5 and Comparative Example PBTM-0. The specific amounts of materials used are shown in the following table:

[0050]

[0051] The following are the performance test processes and results of the embodiments and comparative examples:

[0052] Physical characterization and mechanical properties testing:

[0053] Physical Characterization: Scanning electron microscopy (SEM) tests were performed on a ZEISS Gemini SEM 300. Figure 1 shown.

[0054] Mechanical properties testing: Tensile mechanical properties testing was performed on an Intron universal mechanical testing system equipped with a 50N load cell (Instron 5967 universal material testing machine). To ensure that the hydrogels were highly cross-linked to obtain strong mechanical properties, all samples were incubated for 24 hours before further mechanical properties testing. The hydrogels measured 30 mm × 15 mm × 2 mm, and the tensile speed was 10 mm / min during the test.

[0055] Mechanical properties of PBTM-0 to PBTM-5 were tested respectively, and the tensile stress-strain curves are shown in Figure 2 The test results of tensile strength, Young's modulus and maximum tensile force are shown in Figure 3 As shown; the sensitivity of the material when the stretch value is 1cm, 3cm, 5cm, and 8cm was also tested. The test results are shown in Figure 4 Ti3C2T x The content of MXene will affect the mechanical properties of the hydrogel. With the increase of MXene content, the tensile strength, Young's modulus and fmax of the hydrogel tend to increase, but the tensile properties are reduced due to the accumulation of MXene. Different MXene contents also affect the GF of the hydrogel. With the increase of MXene content, the sensing performance of the hydrogel is significantly improved, among which PBTM-3 has the highest GF (7.79, stretching 800%). However, further increasing the MXene content (PBTM-4 and PBTM-5) will reduce the GF of the hydrogel, which is related to the accumulation of MXene. Excessive MXene is easy to gather together, hindering the flow of electrons, thereby reducing the conductivity of the hydrogel. Therefore, the mass ratio of PVA and MXene in the nanopaper hydrogel formula designed in this application is 50:1~10:1. Preferably, when the mass ratio is 50:3, the mechanical properties are the best, that is, PBTM-3 hydrogel is the best choice for strain sensors.

[0056] Since borax contains boric acid groups, it can form dynamically reversible borate ester bonds with PVA and TOCNF, thereby generating a hydrogel with excellent self-healing properties. Self-healing is crucial for hydrogel sensors because it can extend the life of the sensor and improve the efficiency of the raw materials used. The hydrogel also exhibits good self-healing properties. Specifically, when the hydrogel is cut into two halves and the two halves come into contact, they can heal themselves without any external stimulation. Figure 5As shown in a, the hydrogel is cut into two parts, and then the two parts are allowed to contact for 10 minutes at room temperature. After self-repair, the integrated overall hydrogel can be firmly stretched to a larger extension, and no cracks appear along the contact interface, indicating that the double network structure of the hydrogel and its mechanical properties can be quickly restored without any external stimulation. During the healing process, it is caused by the dynamic borate bonds formed at the cutting site. These reversible crosslinks are easily broken and reorganized. In summary, after the self-repair process, the hydrogel still maintains its original performance properties, which will help it to achieve long-term application. The self-healing hydrogel with sufficient adhesion designed in this application is an excellent material for the preparation of strain sensors. It can be well attached to the skin during long-term measurements without relying on external tapes or bandages that may cause skin irritation. In addition, this hydrogel also exhibits strong tissue adhesion behavior, can be directly attached to human skin, and can withstand stretching or follow the movement of finger joints, such as Figure 5 As shown in b.

[0057] Antibacterial performance test:

[0058] The antibacterial properties of PBTM-3 and PBTM-0 hydrogels were evaluated by plate spread counting test, using Escherichia coli (E. coli) and Bacillus subtilis (B. subtilis) as Gram-negative and Gram-positive bacteria models, respectively. The hydrogels were cut into square pieces with a side length of 10 mm × 10 mm, and the upper and lower surfaces were exposed to ultraviolet light for 30 minutes respectively. 100 μL of 1*10 5 CFU / mL of Escherichia coli or Bacillus subtilis culture fluid was evenly coated on the hydrogel surface and then incubated for 24 hours at 37°C. Afterwards, each bacterial suspension was serially diluted 10 times and added to two nutrient agar media, respectively, and incubated for another 18 hours at 37°C to accurately determine the number of colonies.

[0059] The formula for calculating the antibacterial rate is: Antibacterial rate (%) = (A control – A sample) / A control × 100%, where A control and A sample represent the colony concentrations in the control solution and the corresponding hydrogel sample solution, respectively. The specific test results are shown in the following table:

[0060]

[0061] Here, the antibacterial properties of the hydrogel were evaluated by the plate colony counting method, and the antibacterial rate was obtained by counting the colonies. The colony count refers to the total number of colonies in each group at the corresponding dilution multiple. The counting principle is based on the national standard GB 4789.2-2016, and the colony count between 30 CFU and 300 CFU is selected for colony counting. At the lowest dilution multiple, if there is still no colony growth, it proves that the antibacterial effect of the sample is significant. As shown in the test results, a large number of colonies grew on the plates of the hydrogel (PBTM-0) without MXene. Therefore, the hydrogel without MXene showed poor antibacterial activity against Gram-positive bacteria and Gram-negative bacteria. In contrast, the PBTM-3 hydrogel with added MXene showed obvious inhibitory activity, achieving an antibacterial rate of more than 99.9% against Escherichia coli (E. coli) and Bacillus subtilis (B. subtilis), showing a significant antibacterial effect. According to the national standard GB 4789.2-2016, it can be recognized as having an antibacterial rate of 100%.

[0062] Sensing performance test:

[0063] The sensor prepared by PBTM-3 hydrogel was selected, and the sensing performance was evaluated by Tonghui's LCR TH2830 under the conditions of AC voltage of 1 volt and sweep frequency of 10 kHz to detect various external mechanical stimuli applied to the sensor device. The size of the hydrogel is 30 mm × 15 mm × 2 mm. The hydrogel is adhered to the skin, and the positive and negative electrodes are led out with wires. The current signal change of the hydrogel during skin movement is recorded by LCR. The relative resistance change calculation formula is: ΔR=(R-R0) / R0 ×100%, where R and R0 are the dynamic resistance under different strain states and the resistance under the initial unstrained state, respectively. Gauge Factor: Gauge Factor is defined as the ratio of the unit change of resistance to the unit change of length. The calculation formula of GF is: GF=(ΔR / R) / (ΔL / L).

[0064] The hydrogel was placed in a confined space, and a hair dryer and a humidifier were used to adjust the temperature and humidity in the confined space to evaluate the sensor performance. The test environment was as follows: Figure 6 As shown in a.

[0065] like Figure 6 As shown in Figure b, a finger with hydrogel attached is inserted into the temperature and humidity control box to detect the change in relative resistance when the finger is bent. When the temperature rises to 38°C and the humidity rises to 52%RH, the signal remains stable with a highly repeatable signal pattern. Figure 6As shown in Figure c, after 6 hours, the sensor showed excellent stability under this condition. Similarly, we also simulated and tested the sensing performance of the hydrogel under 32°C and 70%RH conditions similar to the environment of the infant incubator (NICU). The results showed that in this NICU-like environment, the electrical signal response remained highly stable and repeatable, as shown in Figure 5. Figure 6 All the results show that the hydrogel designed in this application can stably output electrical signals under the conditions of 32℃&RH70% and 38℃&RH52% due to its double network structure, so the sensor is insensitive to high temperature and high humidity. This feature makes the sensor show great potential in neonatal monitoring and athlete physical condition monitoring.

[0066] The MXene hydrogel-based sensor designed in this application can be used to monitor large-scale human activities. Figure 7 As shown in (a), the sensor is fixed on the wrist to detect wrist bending movements. The repeatable and clear signals detected under wrist flexion and extension further confirm the reliable sensing ability of the sensor. Figure 7 As shown in Figure b, the sensor is attached to a human finger to detect the bending of the finger. As the bending angle of the finger increases, the relative resistance change increases significantly, indicating that the sensor can clearly measure different bending angles. Therefore, the sensor shows excellent sensing performance in monitoring different bending angles of the joint to provide important clinical information for postoperative rehabilitation training.

[0067] At the same time, these sensors can also be used to monitor small movements of the human body, including the movement of the forehead when frowning and the movement of the throat when speaking. Figure 8 The middle a shows the signal recording of frowning and stretching forehead circulation movement. Figure 8 Middle b shows the signal recording of the jaw opening and closing cycle. Fig. 9 Figure a shows the change in resistance signal when the human body says "good morning". Fig. 9 Figure b shows the change in resistance signal when the human body says "hello". Fig. 9 Figure c shows the change in resistance signal when a person says "good morning". When the sensor is used, a smooth curve with obvious peaks and valleys and high-intensity signals can be observed, showing the potential application value of the sensor in pronunciation recognition and pronunciation training for deaf-mute people. MXene hydrogel is further used to sense the writing movements of human fingers, such as Fig.10 Figure a shows the change in resistance signal when a hand-drawn “triangle” is drawn. Fig.10 Figure b shows the change in resistance signal when a "circle" is drawn by hand. Fig.10 Figure c shows the change in resistance signal when the English word "hello" is handwritten. Fig.10Figure d shows the change in resistance signal when the Chinese word "hello" is handwritten. When the same letter is written repeatedly, the characteristic signal maintains good repeatability and stability, giving the hydrogel its use in electronic skin sensing. As mentioned above, the sensor designed in this application shows high sensitivity even under low strain.

[0068] Pulse is considered an important physiological signal that provides key medical information such as heart rate and vascular status, highlighting the importance of real-time pulse monitoring. Fig.11 The sensor based on MXene hydrogel in this application is attached to the right carotid artery for real-time pulse monitoring, showing a regular normal pulse waveform of about 80 beats / minute. After the tester ran, the pulse waveform frequency increased to about 110 beats / minute. The pulse waveform is a key parameter for diagnosing arteriosclerosis and vascular aging. Fig.12 The data collected signals of normal human breathing and breathing while running, showing obvious breathing frequency and depth in two different situations. Fig.12 The sensor response is shown when a volunteer wears the sensor on the chest area for respiratory monitoring. The peak and valley values ​​represent the signal changes caused by loading and unloading of the strain sensor when the chest area expands and contracts during breathing. The strain sensor can distinguish the breathing pattern and frequency in running and deep breathing mode, and has obvious signal differences. During deep breathing, the sensor signal increases due to the greater strain acting on the sensor. Real-time detection of abnormal breathing frequency and time pattern can help in the early diagnosis of various diseases such as asthma, heart failure, embolism, etc.

[0069] like Fig.13 As shown in the figure, a flexible sensor (1cm*3cm) is pasted inside a medical mask to make a smart mask. When an adult wears it and breathes, the exhaled and inhaled air first contacts the strain sensor, causing the sensor resistance to increase. Fig.13 As shown, different signals reflect the normal breathing and shortness of breath of the human body, giving the sensor the ability to predict early diseases of the human body. Therefore, the sensor designed in this application can also be used to detect the respiratory rate related to exercise and health.

[0070] The above test experiments highlight the potential of the MXene hydrogel-based strain sensor designed in this application in the application fields of wearable devices and soft robots.

[0071] The nanopaper hydrogel designed in this application also has excellent environmental stability (stored for 35 days at 4°C), strain sensitivity (GF 7.79, 800% strain), excellent temperature tolerance (-80°C) and good thermal and moisture stability (at 32°C with a relative humidity of 70% and at 38°C with a relative humidity of 52%).

[0072] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.

Claims

1. A method for preparing a nanopaper hydrogel, characterized in that: The following steps are involved: S1. Add PVA to deionized water, heat and stir to obtain a fully dissolved PVA solution; S2, adding TOCNF to the PVA solution, stirring and mixing evenly to obtain a mixed solution; S3, adding Mxene to the mixed solution, adding deionized water, stirring and mixing evenly to obtain a mixed gel; S4, adding borate to the mixed gel, stirring and mixing evenly to obtain a nanopaper hydrogel; The mass ratio of PVA to TOCNF is 1:8, the mass ratio of PVA to Mxene is 50:1-10:1, and the mass ratio of PVA to borate is 20:1; the PVA, TOCNF and MXene are cross-linked to form a polymer network to form a first network structure, and the borate forms a dynamic reversible borate ester bond with PVA and TOCNF to form a second network structure; the Mxene is Ti3C2T x The borate is borax.

2. The preparation method according to claim 1, characterized in that: The mass ratio of the PVA to Mxene is 50:

3.

3. The preparation method according to claim 1, characterized in that: In step S1, the heating temperature is 80°C to 90°C.

4. The preparation method according to claim 1, characterized in that: In step S2, the fiber length of the TOCNF is 0.5~2.0 μm.

5. The preparation method according to claim 1, characterized in that: In step S3, after stirring and mixing evenly, an ultrasonic treatment process is also included.

6. The preparation method according to claim 1, characterized in that: In step S4, the borate is added as a solution.

7. A nanopaper hydrogel, characterized in that: Prepared by the preparation method according to any one of claims 1 to 6.

8. A nanopaper hydrogel sensor prepared based on the nanopaper hydrogel according to claim 7.

9. An application of the nanopaper hydrogel sensor according to claim 8 in a soft robot.