A kind of anti-scratch polyurethane paint surface protective film and preparation method thereof
By using cross-linking and dynamic covalent bonds of linear and branched prepolymers in the scratch-resistant polyurethane paint protective film, the problem of difficult to take into account both mechanical properties and self-repair properties in the prior art is solved, and high Protective film with mechanical properties and excellent self-healing ability.
Patent Information
- Application Number
- CN202411150918.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The existing scratch-resistant polyurethane painted protective film is difficult to maintain good self-repair performance while improving mechanical properties, and it is difficult to take into account both.
Self-healing polyurethane slurry is used to cross-link the linear prepolymer and branched prepolymer to form dynamic covalent bonds and ionic interactions, improving mechanical properties and self-healing capabilities. Specific methods include using hydrazide-capped hyperbranched polyurethane prepolymer to react with raw materials such as isophorone diisocyanate, polytetrahydrofuran glycol, 2-hydroxymethylpropionic acid, and emulsification of N-methyldiethanolamine and deionized water. , an aqueous polyurethane prepolymer dispersion was prepared, and mixed with adipic acid dihydrazide, defoaming agent, wetting agent, etc., and then applied to the surface of the plate and dried to form a protective film.
It has achieved high mechanical properties and excellent self-repairing ability of anti-scratch polyurethane paint protective film. The pencil has a hardness of 6H, an adhesion of 4B, and the lowest wear of mass. It can effectively protect the paint surface of the car body and repair itself when damaged.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of protective films, and in particular to an anti-scratch polyurethane paint surface protective film and a preparation method thereof. Background Art
[0002] Car paint protection film is commonly known as car cover film. When used, it is attached to the paint surface of the car body to protect the car paint, and it has the functions of anti-scratch, stain resistance, environmental corrosion resistance, and decorative beauty. The surface of the car cover film on the market is generally coated with self-repairing paint. When the car body encounters scratches or minor collisions, as long as the car cover base film itself is not damaged, the small scratches can be automatically eliminated in a short time, or eliminated under heating conditions; when a serious collision damages the base film, the car cover film can also be partially replaced. Therefore, the application of self-repairing paint on the car cover film can effectively protect the car paint, reduce the trouble of repairing the car paint, avoid environmental pollution caused by repairing the car paint, and make the car body more beautiful, improve the car's value retention rate, meet people's personalized needs, and is very popular in the market.
[0003] Patent technology document CN116854865B discloses a self-repairing, scratch-resistant paint protective film, which uses isotribenzyl alcohol as a chain extender, polytetrahydrofuran diol and polyisocyanate to polymerize into a hyperbranched polyurethane prepolymer, and then introduces an acrylic resin segment containing an indole ring into the hyperbranched polyurethane prepolymer. A large number of carboxyl, carbonyl, amide and other groups in the acrylic resin of the invention can form hydrogen bonds with nitrogen and oxygen atoms of polyurethane. When the polyurethane is scratched under the impact of external force, the effect of hydrogen bonds can enable the material to quickly self-repair.
[0004] Patent technical document CN117264550B discloses a paint protection film and a self-repairing coating thereof, wherein the self-repairing coating adopts a water-based polyurethane self-repairing coating, and the coating is prepared from a self-repairing water-based polyurethane emulsion, water and a water-based additive; the self-repairing water-based polyurethane emulsion is mainly formed by the reaction of isophorone diisocyanate, polyether diol, ferric chloride hexahydrate and a modified monomer, and the modified monomer is prepared by the reaction of amino carbon quantum dots and a catechol derivative with a monoepoxy group and a silane-protected phenolic hydroxyl group. The invention utilizes iron-catechol coordination bonds and hydrogen bonds to synergistically enhance the self-repairing performance.
[0005] Patent technical document CN113088176A discloses a self-healing scratch-resistant polyurethane coating, which is prepared from the following raw materials: polymer polyol resin, diisocyanate, dihydrazide chain extender, silicone functional additive, other additives, catalyst and diluent solvent. It further discloses the use of dihydrazide chain extender (such as succinic acid dihydrazide, azelaic acid dihydrazide, etc.) that can form dynamic urea-type hydrogen bonds. The dynamic urea-type hydrogen bonds can not only undergo dynamic exchange at room temperature, but also give the polyurethane coating rapid self-healing properties.
[0006] Although the protective films in the above patents all have self-healing properties, their mechanical properties are generally low and it is difficult to play a protective role. Moreover, if their mechanical properties are to be improved, the self-healing properties of the protective film will inevitably be affected. It is difficult to take both into account at the same time. Summary of the invention
[0007] In view of this, the purpose of the present invention is to provide an anti-scratch polyurethane paint protective film and a preparation method thereof, aiming to give the protective film better self-repairing properties on the basis of ensuring higher mechanical properties of the protective film.
[0008] Based on the above purpose, the present invention provides an anti-scratch polyurethane paint protective film, which is obtained by coating a self-repairing polyurethane slurry on a flat plate; the self-repairing polyurethane slurry comprises the following raw materials in parts by weight: 100-150 parts of an aqueous polyurethane prepolymer dispersion, 3-5 parts of adipic acid dihydrazide, 1-5 parts of a defoamer, 1-5 parts of a wetting agent, 1-5 parts of a leveling agent and 20-30 parts of deionized water;
[0009] The solid content of the aqueous polyurethane prepolymer dispersion is 30-40%;
[0010] The aqueous polyurethane prepolymer dispersion is prepared by reacting a hydrazide-terminated hyperbranched polyurethane prepolymer with isophorone diisocyanate, polycarbonate diol and 1.3-dihydroxymethylacetone after neutralization with N-methyldiethanolamine, and then adding deionized water for emulsification after the reaction is completed.
[0011] The hydrazide-terminated hyperbranched polyurethane prepolymer is obtained by reacting isophorone diisocyanate, polytetrahydrofuran diol, and dimethylol propionic acid, and then reacting with mesityl alcohol to form a branched polyurethane prepolymer, and then using hydroxyacetohydrazide to terminate the prepolymer.
[0012] Preferably, the preparation method of the hydrazide-terminated hyperbranched polyurethane prepolymer is as follows: isophorone diisocyanate, polytetrahydrofuran diol, dihydroxymethyl propionic acid, and dibutyltin dilaurate are mixed, the temperature is raised to 70-80° C., and the mixture is stirred for reaction for 2-3 hours, and then isotribenzyl alcohol is added, the temperature is raised to 90-100° C., and the mixture is stirred for reaction for 1-2 hours, and finally hydroxyacetohydrazide is added, the temperature is lowered to 60-70° C., and the mixture is stirred for reaction for 30-40 minutes to obtain the hydrazide-terminated hyperbranched polyurethane prepolymer.
[0013] Preferably, the weight ratio of isophorone diisocyanate, polytetramethylene glycol, dimethylol propionic acid, mesitylene glycol and hydroxyacetohydrazide is 100-120:40-50:10-15:20-30:5-10.
[0014] Preferably, the preparation method of the aqueous polyurethane prepolymer dispersion is as follows: dissolving the hydrazide-terminated hyperbranched polyurethane prepolymer in acetone, adding N-methyldiethanolamine, heating to 40-50° C., stirring and reacting for 30-40 minutes, then adding isophorone diisocyanate, polycarbonate diol, 1.3-dihydroxymethylacetone, and dibutyltin dilaurate, heating to 70-80° C., stirring and reacting for 1-2 hours, removing acetone by rotary evaporation, adding deionized water for emulsification, and obtaining an aqueous polyurethane prepolymer dispersion with a solid content of 30-40%.
[0015] Preferably, the weight ratio of the hydrazide-terminated hyperbranched polyurethane prepolymer, N-methyldiethanolamine, isophorone diisocyanate, polycarbonate diol and 1.3-dihydroxymethylacetone is 100-120:8-10:50-60:18-24:15-20.
[0016] Preferably, the molecular weight of the polycarbonate diol is 500-1000; the molecular weight of the polytetrahydrofuran diol is 500-1000.
[0017] Preferably, the defoaming agent is one of BYK028, BYK-W961 and SI-2292.
[0018] Preferably, the wetting agent is one of BYK333 and BYK-3480.
[0019] Preferably, the leveling agent is a silicone or acrylate leveling agent.
[0020] More preferably, the leveling agent is BYK-302.
[0021] Furthermore, the present invention also provides a method for preparing a scratch-resistant polyurethane paint protective film, comprising the following steps:
[0022] S1: mixing an aqueous polyurethane prepolymer dispersion, adipic acid dihydrazide, a defoamer, a thickener, a leveling agent and deionized water to obtain a self-healing polyurethane slurry;
[0023] S2: The self-repairing polyurethane slurry is coated on the surface of the flat plate, first dried at room temperature for 3-5 hours, and then dried at 60-65°C for 34-36 hours to obtain a scratch-resistant polyurethane paint protective film.
[0024] Beneficial effects of the present invention:
[0025] The anti-scratch polyurethane paint protective film of the present invention is cross-linked by a linear prepolymer and a branched prepolymer, and the linear polyurethane prepolymer is interspersed in the branched polyurethane prepolymer as a bridge, so that the mechanical properties and self-repairing ability of the anti-scratch polyurethane paint protective film are improved.
[0026] The anti-scratch polyurethane paint surface protective film of the present invention can form dynamic covalent bonds through the ketone groups in the linear prepolymer and the hydrazide groups in the branched prepolymer, thereby improving the curing efficiency, mechanical properties and self-repairing ability.
[0027] The anti-scratch polyurethane paint protection film of the present invention improves water solubility through neutralization reaction of tertiary amine in linear prepolymer and dimethylol propionic acid in branched prepolymer, and also has ion interaction, further enhancing self-repairing ability and mechanical properties. DETAILED DESCRIPTION
[0028] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.
[0029] The sources and / or properties of the raw materials used in the embodiments and comparative examples of the present invention are as follows: polytetrahydrofuran diol was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. with a product number of P141386 and an average molecular weight of 850; polycarbonate diol was purchased from Guangzhou Haoyi New Materials Technology Co., Ltd. with a model of Asahi Kasei T5650J and an average molecular weight of 800.
[0030] Example 1: A scratch-resistant polyurethane paint protective film, the specific preparation steps are as follows:
[0031] (1) 100 g of isophorone diisocyanate, 40 g of polytetrahydrofuran diol, 10 g of dimethylol propionic acid, and 0.1 g of dibutyltin dilaurate were mixed, the temperature was raised to 70° C., and the mixture was stirred for reaction for 2 h. Then 20 g of isotribenzyl alcohol was added, the temperature was raised to 90° C., and the mixture was stirred for reaction for 1 h. Finally, 5 g of hydroxyacetohydrazide was added, the temperature was lowered to 60° C., and the mixture was stirred for reaction for 30-40 min to obtain a hydrazide-terminated hyperbranched polyurethane prepolymer.
[0032] (2) Dissolve 100 g of hydrazide-terminated hyperbranched polyurethane prepolymer in 200 g of acetone, add 8 g of N-methyldiethanolamine, heat to 40°C, stir and react for 30 min, then add 50 g of isophorone diisocyanate, 18 g of polycarbonate diol, 15 g of 1.3-dihydroxymethylacetone, and 0.1 g of dibutyltin dilaurate, heat to 70°C, stir and react for 1 h, remove acetone by rotary evaporation, add deionized water for emulsification, and obtain an aqueous polyurethane prepolymer dispersion with a solid content of 33%;
[0033] (3) 100 g of aqueous polyurethane prepolymer dispersion, 3 g of adipic acid dihydrazide, 1 g of BYK028, 1 g of BYK333, 1 g of BYK-302 and 20 g of deionized water were mixed according to the raw material ratio to obtain a self-healing polyurethane slurry;
[0034] (4) The self-healing polyurethane slurry was coated on the surface of the flat plate, first dried at room temperature for 3 h, and then dried at 60 °C for 34 h to obtain a scratch-resistant polyurethane paint protective film.
[0035] Example 2: A scratch-resistant polyurethane paint protective film, the specific preparation steps are as follows:
[0036] (1) 110 g of isophorone diisocyanate, 45 g of polytetrahydrofuran diol, 13 g of dimethylol propionic acid, and 0.3 g of dibutyltin dilaurate were mixed, the temperature was raised to 75° C., and the mixture was stirred for reaction for 2.5 h. Then 25 g of isotribenzyl alcohol was added, the temperature was raised to 95° C., and the mixture was stirred for reaction for 1.5 h. Finally, 7.5 g of hydroxyacetohydrazide was added, the temperature was lowered to 65° C., and the mixture was stirred for reaction for 35 min to obtain a hydrazide-terminated hyperbranched polyurethane prepolymer.
[0037] (2) Dissolve 110 g of hydrazide-terminated hyperbranched polyurethane prepolymer in 300 g of acetone, add 9 g of N-methyldiethanolamine, heat to 45°C, stir and react for 35 min, then add 55 g of isophorone diisocyanate, 23 g of polycarbonate diol, 17.5 g of 1.3-dihydroxymethylacetone, and 0.3 g of dibutyltin dilaurate, heat to 75°C, stir and react for 1.5 h, remove acetone by rotary evaporation, add deionized water for emulsification, and obtain an aqueous polyurethane prepolymer dispersion with a solid content of 35%;
[0038] (3) 130 g of aqueous polyurethane prepolymer dispersion, 4 g of adipic acid dihydrazide, 3 g of BYK028, 3 g of BYK333, 3 g of BYK-302 and 25 g of deionized water were mixed according to the raw material ratio to obtain a self-healing polyurethane slurry;
[0039] (4) The self-healing polyurethane slurry was coated on the surface of the flat plate, first dried at room temperature for 4 h, and then dried at 63 °C for 35 h to obtain a scratch-resistant polyurethane paint protective film.
[0040] Example 3: A scratch-resistant polyurethane paint protective film, the specific preparation steps are as follows:
[0041] (1) 117 g of isophorone diisocyanate, 48 g of polytetrahydrofuran diol, 12 g of dimethylol propionic acid, and 0.3 g of dibutyltin dilaurate were mixed, the temperature was raised to 75° C., and the mixture was stirred for reaction for 3 h. Then 27 g of isotribenzyl alcohol was added, the temperature was raised to 97° C., and the mixture was stirred for reaction for 2 h. Finally, 6 g of hydroxyacetohydrazide was added, the temperature was lowered to 68° C., and the mixture was stirred for reaction for 30 min to obtain a hydrazide-terminated hyperbranched polyurethane prepolymer.
[0042] (2) Dissolve 115 g of hydrazide-terminated hyperbranched polyurethane prepolymer in 330 g of acetone, add 9 g of N-methyldiethanolamine, heat to 50 ° C, stir and react for 40 min, then add 53 g of isophorone diisocyanate, 21 g of polycarbonate diol, 18 g of 1.3-dihydroxymethylacetone, and 0.4 g of dibutyltin dilaurate, heat to 70 ° C, stir and react for 1 h, remove acetone by rotary evaporation, add deionized water for emulsification, and obtain an aqueous polyurethane prepolymer dispersion with a solid content of 40%;
[0043] (3) 140 g of aqueous polyurethane prepolymer dispersion, 5 g of adipic acid dihydrazide, 2 g of BYK028, 4 g of BYK333, 3 g of BYK-302 and 30 g of deionized water were mixed according to the raw material ratio to obtain a self-healing polyurethane slurry;
[0044] (4) The self-healing polyurethane slurry was coated on the surface of the flat plate, first dried at room temperature for 5 h, and then dried at 60 °C for 36 h to obtain a scratch-resistant polyurethane paint protective film.
[0045] Example 4: A scratch-resistant polyurethane paint protective film, the specific preparation steps are as follows:
[0046] (1) 120 g of isophorone diisocyanate, 50 g of polytetrahydrofuran diol, 15 g of dimethylol propionic acid, and 0.5 g of dibutyltin dilaurate were mixed, the temperature was raised to 80° C., and the mixture was stirred for reaction for 3 h. Then 30 g of isotribenzyl alcohol was added, the temperature was raised to 100° C., and the mixture was stirred for reaction for 2 h. Finally, 10 g of hydroxyacetohydrazide was added, the temperature was lowered to 70° C., and the mixture was stirred for reaction for 40 min to obtain a hydrazide-terminated hyperbranched polyurethane prepolymer.
[0047] (2) Dissolve 120 g of hydrazide-terminated hyperbranched polyurethane prepolymer in 400 g of acetone, add 10 g of N-methyldiethanolamine, heat to 50° C., stir and react for 40 min, then add 60 g of isophorone diisocyanate, 24 g of polycarbonate diol, 20 g of 1.3-dihydroxymethylacetone, and 0.5 g of dibutyltin dilaurate, heat to 80° C., stir and react for 2 h, remove acetone by rotary evaporation, add deionized water for emulsification, and obtain an aqueous polyurethane prepolymer dispersion with a solid content of 30%;
[0048] (3) 150 g of aqueous polyurethane prepolymer dispersion, 5 g of adipic acid dihydrazide, 5 g of BYK028, 5 g of BYK333, 5 g of BYK-302 and 30 g of deionized water were mixed according to the raw material ratio to obtain a self-healing polyurethane slurry;
[0049] (4) The self-healing polyurethane slurry was coated on the surface of the flat plate, first dried at room temperature for 5 h, and then dried at 65 °C for 36 h to obtain a scratch-resistant polyurethane paint protective film.
[0050] Comparative Example 1: A polyurethane paint protective film, the specific preparation steps are as follows:
[0051] (1) 110 g of isophorone diisocyanate, 45 g of polytetrahydrofuran diol, 13 g of dimethylol propionic acid, and 0.3 g of dibutyltin dilaurate were mixed, the temperature was raised to 75° C., and the mixture was stirred for reaction for 2.5 h. Then 25 g of isotribenzyl alcohol was added, the temperature was raised to 95° C., and the mixture was stirred for reaction for 1.5 h. Finally, 7.5 g of hydroxyacetohydrazide was added, the temperature was lowered to 65° C., and the mixture was stirred for reaction for 35 min to obtain a hydrazide-terminated hyperbranched polyurethane prepolymer.
[0052] (2) 9 g of N-methyldiethanolamine, 55 g of isophorone diisocyanate, 23 g of polycarbonate diol, 17.5 g of 1.3-dihydroxymethylacetone, and 0.3 g of dibutyltin dilaurate were heated to 75°C and stirred for reaction for 1.5 h to obtain a polyurethane prepolymer. 110 g of hydrazide-terminated hyperbranched polyurethane prepolymer was dissolved in 300 g of acetone and added to the polyurethane prepolymer. After mixing evenly, the acetone was removed by rotary evaporation, and deionized water was added for emulsification to obtain an aqueous polyurethane prepolymer dispersion with a solid content of 35%;
[0053] (3) 130 g of aqueous polyurethane prepolymer dispersion, 4 g of adipic acid dihydrazide, 3 g of BYK028, 3 g of BYK333, 3 g of BYK-302 and 25 g of deionized water were mixed according to the raw material ratio to obtain a self-healing polyurethane slurry;
[0054] (4) The self-healing polyurethane slurry was coated on the surface of the flat plate, first dried at room temperature for 4 h, and then dried at 63 °C for 35 h to obtain a scratch-resistant polyurethane paint protective film.
[0055] Comparative Example 2: A polyurethane paint protective film, the specific preparation steps are as follows:
[0056] (1) 110 g of isophorone diisocyanate, 45 g of polytetrahydrofuran diol, 13 g of dimethylol propionic acid, and 0.3 g of dibutyltin dilaurate were mixed, the temperature was raised to 75° C., and the mixture was stirred for reaction for 2.5 h. Then, 25 g of isotribenzyl alcohol was added, the temperature was raised to 95° C., and the mixture was stirred for reaction for 1.5 h to obtain a hyperbranched polyurethane prepolymer;
[0057] (2) Dissolve 110 g of hyperbranched polyurethane prepolymer in 300 g of acetone, add 9 g of N-methyldiethanolamine, heat to 45° C., stir and react for 35 min, then add 55 g of isophorone diisocyanate, 23 g of polycarbonate diol, 17.5 g of 1.3-dihydroxymethylacetone, and 0.3 g of dibutyltin dilaurate, heat to 75° C., stir and react for 1.5 h, remove acetone by rotary evaporation, add deionized water for emulsification, and obtain an aqueous polyurethane prepolymer dispersion with a solid content of 35%;
[0058] (3) 130 g of aqueous polyurethane prepolymer dispersion, 4 g of adipic acid dihydrazide, 3 g of BYK028, 3 g of BYK333, 3 g of BYK-302 and 25 g of deionized water were mixed according to the raw material ratio to obtain a self-healing polyurethane slurry;
[0059] (4) The self-healing polyurethane slurry was coated on the surface of the flat plate, first dried at room temperature for 4 h, and then dried at 63 °C for 35 h to obtain a scratch-resistant polyurethane paint protective film.
[0060] Comparative Example 3: A polyurethane paint protective film, the specific preparation steps are as follows:
[0061] (1) 110 g of isophorone diisocyanate, 45 g of polytetrahydrofuran diol, 13 g of dimethylol propionic acid, and 0.3 g of dibutyltin dilaurate were mixed, the temperature was raised to 75° C., and the mixture was stirred for reaction for 2.5 h. Then 25 g of isotribenzyl alcohol was added, the temperature was raised to 95° C., and the mixture was stirred for reaction for 1.5 h. Finally, 7.5 g of hydroxyacetohydrazide was added, the temperature was lowered to 65° C., and the mixture was stirred for reaction for 35 min to obtain a hydrazide-terminated hyperbranched polyurethane prepolymer.
[0062] (2) Dissolve 110 g of hydrazide-terminated hyperbranched polyurethane prepolymer in 300 g of acetone, add 9 g of N-methyldiethanolamine, raise the temperature to 45°C, stir and react for 35 min, add deionized water for emulsification, and obtain an aqueous polyurethane prepolymer dispersion with a solid content of 35%;
[0063] (3) 130 g of aqueous polyurethane prepolymer dispersion, 4 g of adipic acid dihydrazide, 3 g of BYK028, 3 g of BYK333, 3 g of BYK-302 and 25 g of deionized water were mixed according to the raw material ratio to obtain a self-healing polyurethane slurry;
[0064] (4) The self-healing polyurethane slurry was coated on the surface of the flat plate, first dried at room temperature for 4 h, and then dried at 63 °C for 35 h to obtain a scratch-resistant polyurethane paint protective film.
[0065] Performance Testing
[0066] Mechanical properties:
[0067] Hardness: According to ASTM D3363 standard, the pencil hardness of the paint protection films obtained in the examples and comparative examples was measured using a pencil hardness tester purchased from Biaugeda Corporation. The test results are shown in Table 1.
[0068] Adhesion: According to ASTM D3359 standard, the adhesion of the paint protection film obtained in the embodiment and comparative example to the Q235 steel substrate was tested by the cross-hatch method. First, the paint protection film was slowly scratched in the horizontal and vertical directions with a scratch spacing of 3mm, and then the scratches were firmly adhered with tape and then slowly peeled off. The degree of peeling of the paint protection film was observed. When the paint protection film was not peeled off at all, the best adhesion grade was 5B. When the paint protection film was peeled off over a large area (>65%), the worst adhesion grade was 1B. The test results are shown in Table 1.
[0069] Wear resistance:
[0070] According to GB / T 1768 standard, the paint protection films obtained in the examples and comparative examples were subjected to friction and wear tests using a BGD523 paint film abrasion tester purchased from Biaogeda. The speed of the friction rubber wheel was set to 60r / min, the number of grinding turns was set to 500 turns, and the load weight was set to 1000g. Before the test began, 50 turns were pre-grinded to remove impurities on the surface of the protective film. The weight of the sample at this time was weighed and recorded as W0. After the test, the friction debris on the protective film was gently brushed off with a brush, and then it was weighed again, and the weight was recorded as W1. The mass wear calculation formula of the sample is as follows:
[0071] Mass wear (mg) = W0-W1
[0072] The test results are shown in Table 1.
[0073] Self-repairing performance: According to GB / T528-1998 standard, the self-repairing polyurethane slurry obtained in the embodiment and the comparative example was prepared into dumbbell-shaped specimen 4, with a specimen length of 10.0±0.5mm and a thickness of 1.0±0.1mm. After tensile testing, the tensile strength was obtained, and then the broken specimen sections were quickly and tightly butted and heated and cured at 100°C for 2 hours. After being fully cooled to room temperature, they were stretched again to measure the tensile strength. The results are shown in Table 2.
[0074] Table 1 Performance test results
[0075] Pencil hardness Adhesion Mass wear (mg) Example 1 6H 4B 3.1 Example 2 6H 4B 2.6 Example 3 6H 4B 2.7 Example 4 6H 4B 2.9 Comparative Example 1 4H 4B 3.9 Comparative Example 2 6H 4B 3.4 Comparative Example 3 3H 3B 4.5
[0076] Table 2 Self-repair performance test results
[0077]
[0078] Data analysis shows that the scratch-resistant polyurethane paint protective film of the present invention has excellent mechanical properties and wear resistance, with a pencil hardness of 6H, an adhesion of 4B, and a minimum mass wear of only 2.6 mg. Most importantly, it has excellent self-repairing properties. When applied to the paint surface of a car body, it can provide good protection and can self-repair small scratches when scratched, and has broad application prospects.
[0079] It can be seen from Example 2 and Comparative Example 1 in Table 1 and Table 2 that the aqueous polyurethane prepolymer dispersion in the anti-scratch polyurethane paint protective film of the present invention introduces a branched and linear cross-linked network. Compared with directly mixing the hydrazide-terminated hyperbranched polyurethane prepolymer with the linear polyurethane prepolymer, the hydrazide-terminated hyperbranched polyurethane prepolymer is added during the synthesis of the linear polyurethane prepolymer, that is, the hydrazide-terminated hyperbranched polyurethane prepolymer can directly participate in the linear polyurethane prepolymer and the polyurethane synthesis process, and the linear polyurethane prepolymer can serve as a cross-linking bridge to cross-link the hyperbranched polyurethane prepolymers to further improve their mechanical properties. At the same time, the linear chain can penetrate the hyperbranched network to make the dynamic covalent bonds and ionic interactions more evenly distributed, thereby further improving the self-healing performance. step improvement; it can be seen from Example 2 and Comparative Examples 2-3 that the branched polyurethane prepolymer is terminated with a hydrazide group, and the hydrazide group can form a dynamic covalent bond with the ketone group in the straight chain, and this dynamic covalent bond can improve the self-repairing ability and mechanical properties of the scratch-resistant polyurethane paint protective film; after the introduction of the straight chain, the straight chain can not only be interspersed in the branched polyurethane prepolymer, but also the 1.3-dihydroxymethylacetone in the straight chain can form a dynamic covalent bond with the hydrazide group of the branched polyurethane prepolymer, and the introduced N-methyldiethanolamine can neutralize the dihydroxymethylpropionic acid in the hydrazide-terminated branched polyurethane prepolymer while serving as a chain extender, thereby improving the water solubility and allowing the linear polyurethane prepolymer and the polyurethane prepolymer to have ionic interactions, further enhancing the self-repairing ability and mechanical properties.
[0080] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention (including the claims) is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.
[0081] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A scratch-resistant polyurethane paint protective film, characterized in that: The self-repairing polyurethane slurry is coated on a flat plate; the self-repairing polyurethane slurry comprises the following raw materials in parts by weight: 100-150 parts of aqueous polyurethane prepolymer dispersion, 3-5 parts of adipic acid dihydrazide, 1-5 parts of defoamer, 1-5 parts of wetting agent, 1-5 parts of leveling agent and 20-30 parts of deionized water; The solid content of the aqueous polyurethane prepolymer dispersion is 30-40%; The aqueous polyurethane prepolymer dispersion is prepared by reacting a hydrazide-terminated branched polyurethane prepolymer with isophorone diisocyanate, polycarbonate diol and 1.3-dihydroxymethylacetone after neutralization with N-methyldiethanolamine, and then adding deionized water for emulsification after the reaction is completed. The hydrazide-terminated branched polyurethane prepolymer is obtained by reacting isophorone diisocyanate, polytetrahydrofuran diol, and dimethylol propionic acid, and then reacting with mesityl alcohol to form a branched polyurethane prepolymer, and then using hydroxyacetohydrazide to terminate the prepolymer. The weight ratio of isophorone diisocyanate, polytetrahydrofuran diol, dimethylol propionic acid, mesitylene glycol and hydroxyacetohydrazide is 100-120:40-50:10-15:20-30:5-10; The weight ratio of the hydrazide-terminated hyperbranched polyurethane prepolymer, N-methyldiethanolamine, isophorone diisocyanate, polycarbonate diol and 1.3-dihydroxymethylacetone is 100-120:8-10:50-60:18-24:15-20.
2. The anti-scratch polyurethane paint protection film according to claim 1, characterized in that: The preparation method of the hydrazide-terminated branched polyurethane prepolymer is as follows: isophorone diisocyanate, polytetrahydrofuran diol, dihydroxymethyl propionic acid and dibutyltin dilaurate are mixed, the temperature is raised to 70-80°C, and the mixture is stirred for reaction for 2-3h, and then isotribenzyl alcohol is added, the temperature is raised to 90-100°C, and the mixture is stirred for reaction for 1-2h, and finally hydroxyacetohydrazide is added, the temperature is lowered to 60-70°C, and the mixture is stirred for reaction for 30-40min to obtain the hydrazide-terminated hyperbranched polyurethane prepolymer.
3. The scratch-resistant polyurethane paint protection film according to claim 1, characterized in that: The preparation method of the waterborne polyurethane prepolymer dispersion is as follows: dissolving a hydrazide-terminated hyperbranched polyurethane prepolymer in acetone, adding N-methyldiethanolamine, heating to 40-50° C., stirring and reacting for 30-40 minutes, then adding isophorone diisocyanate, polycarbonate diol, 1.3-dihydroxymethylacetone, and dibutyltin dilaurate, heating to 70-80° C., stirring and reacting for 1-2 hours, removing acetone by rotary evaporation, and adding deionized water for emulsification to obtain a waterborne polyurethane prepolymer dispersion with a solid content of 30-40%.
4. The anti-scratch polyurethane paint protection film according to claim 1, characterized in that: The molecular weight of the polycarbonate diol is 500-1000; the molecular weight of the polytetrahydrofuran diol is 500-1000.
5. The scratch-resistant polyurethane paint protection film according to claim 1, characterized in that: The defoamer is one of BYK028 and BYK-W961.
6. The anti-scratch polyurethane paint protection film according to claim 1, characterized in that: The wetting agent is one of BYK333 and BYK-3480.
7. The scratch-resistant polyurethane paint protection film according to claim 1, characterized in that: The leveling agent is a silicone or acrylate leveling agent.
8. A method for preparing the scratch-resistant polyurethane paint protective film according to any one of claims 1 to 7, characterized in that: The steps include: S1: mixing an aqueous polyurethane prepolymer dispersion, adipic acid dihydrazide, a defoamer, a wetting agent, a leveling agent and deionized water to obtain a self-healing polyurethane slurry; S2: The self-repairing polyurethane slurry is coated on the surface of the flat plate, first dried at room temperature for 3-5 hours, and then dried at 60-65°C for 34-36 hours to obtain a scratch-resistant polyurethane paint protective film.
Citation Information
Cited By
Lasting hydrophobic automobile paint surface protective film and preparation method thereof
CN121699372A